Solar cell and processing method thereof

Through the combination of in-situ doping and pore surface structure, the leakage problem caused by secondary diffusion in TOPCon solar cells is solved, and the conversion efficiency and contact performance of the battery are improved.

CN114744056BActive Publication Date: 2024-11-12LONGI SOLAR TECH (XIAN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210340019.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-01
Publication Date
2024-11-12
Estimated Expiration
2042-04-01

AI Technical Summary

Technical Problem

The existing TOPCon solar cells form heavy doping through secondary diffusion in the gate line contact area, which easily leads to penetration of the silicon oxide layer and causes leakage problems.

Method used

The first polysilicon layer is formed in the gate line contact area by in-situ doping, and the second polysilicon layer is formed in the non-gate line contact area, so as to improve contact performance through the hole surface structure to avoid secondary diffusion and penetration. Silicon oxide layer.

Benefits of technology

The contact strength between the gate line and the polysilicon layer is improved, the contact performance of the selective emitter is enhanced, the risk of leakage is reduced, and the conversion efficiency of solar cells is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114744056B_ABST
    Figure CN114744056B_ABST
Patent Text Reader

Abstract

The present application discloses a solar cell and a processing method thereof, wherein the method comprises: providing a silicon substrate, wherein one side of the silicon substrate has a gate line contact region and a non-gate line contact region; forming a hole surface structure in the gate line contact region; sequentially depositing a first silicon oxide layer and a first polysilicon layer on the hole surface structure, wherein the first polysilicon layer is formed by an in-situ doping deposition method, and the first polysilicon layer has a first doping concentration; sequentially depositing a second silicon oxide layer and a second polysilicon layer on the non-gate line contact region; doping the second polysilicon layer to obtain a second polysilicon layer with a second doping concentration, wherein the second doping concentration is less than the first doping concentration; forming a gate line in the gate line contact region, wherein the gate line is in ohmic contact with the first polysilicon layer. This solution solves the problem in the prior art that secondary diffusion easily causes secondary diffusion to penetrate the silicon oxide layer, resulting in leakage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention generally relates to the technical field of solar photovoltaic power generation, and in particular to a solar cell and a processing method thereof. Background Art

[0002] TOPCon is a tunnel oxide passivated contact (Tunnel Oxide Passivated Contact) solar cell technology based on the principle of selective carriers. Generally, a TOPCon solar cell includes an N-type silicon substrate, an ultra-thin silicon oxide layer is deposited on the back of the N-type silicon substrate, and then a thin layer of polycrystalline silicon is deposited on the silicon oxide layer. The polycrystalline silicon layer is then doped, and a heavy doping is formed in the gate line contact area, and a light doping is formed in the non-gate line contact area. At present, the gate line contact area is usually heavily doped by secondary diffusion. In this way, the depth of the secondary diffusion is difficult to control, which easily causes the secondary diffusion to penetrate the silicon oxide layer, resulting in leakage problems. Summary of the invention

[0003] In view of the above defects or deficiencies in the prior art, it is desired to provide a solar cell and a processing method thereof to at least solve the problem in the prior art that heavy doping is formed in the gate line contact area through secondary diffusion, which easily causes the secondary diffusion to penetrate the silicon oxide layer and cause leakage.

[0004] In a first aspect, the present invention provides a method for processing a solar cell, comprising the following steps:

[0005] Providing a silicon substrate, wherein one side of the silicon substrate has a gate line contact region and a non-gate line contact region;

[0006] forming a hole surface structure in the gate line contact region;

[0007] Depositing a first silicon oxide layer and a first polysilicon layer sequentially on the hole surface structure, wherein the first polysilicon layer is formed by an in-situ doping deposition method, and the first polysilicon layer has a first doping concentration;

[0008] sequentially depositing a second silicon oxide layer and a second polysilicon layer on the non-gate line contact region;

[0009] doping the second polysilicon layer to obtain a second polysilicon layer with a second doping concentration, wherein the second doping concentration is less than the first doping concentration;

[0010] A gate line is formed in the gate line contact region, and the gate line is in ohmic contact with the first polysilicon layer.

[0011] As an achievable manner, the hole surface structure is formed in the gate line contact area, specifically:

[0012] Polishing one side of the silicon substrate with an alkaline solution;

[0013] Depositing an acid polishing protective layer on the surface polished by the alkaline solution, and patterning the acid polishing protective layer to form a first opening exposing the gate line contact area;

[0014] Performing acid solution polishing on the first opening to form the hole surface structure located in the gate line contact area;

[0015] or,

[0016] Polishing one side of the silicon substrate with an acid solution to obtain a surface with a hole structure;

[0017] Depositing an alkali-polished protective layer on the surface having the hole structure, and patterning the alkali-polished protective layer to form a second opening exposing the non-gate line contact area;

[0018] The second opening is polished with an alkaline solution to remove the hole structure in the non-gate line contact area and retain the hole structure in the gate line contact area to obtain the hole surface structure located in the gate line contact area.

[0019] As an achievable manner, an acid polishing protective layer is deposited on the surface polished by the alkaline solution, and the acid polishing protective layer is patterned to form a first opening exposing the gate line contact area, specifically:

[0020] Depositing an acid polishing protective layer on the surface polished by the alkaline solution;

[0021] Coating a first photoresist layer on the acid polishing protective layer, exposing and developing the first photoresist layer to form a third opening exposing the acid polishing protective layer;

[0022] The acid polishing protection layer within the range of the third opening is removed, and the first opening exposing the gate line contact area is obtained in the acid polishing protection layer.

[0023] As an achievable manner, the alkali-polished protective layer is deposited on the surface having the hole structure, and the alkali-polished protective layer is patterned to form a second opening exposing the non-gate line contact area, specifically:

[0024] Depositing an alkali polishing protective layer on the surface having the porous structure;

[0025] Coating a second photoresist layer on the alkali polishing protective layer, exposing and developing the second photoresist layer to form a fourth opening exposing the alkali polishing protective layer;

[0026] The alkali-polished protective layer within the range of the fourth opening is removed, and the second opening exposing the non-gate line contact area is obtained in the alkali-polished protective layer.

[0027] As an implementable manner, the acid solution polishing includes a first acid solution polishing and a second acid solution polishing performed sequentially; the first acid solution polishing adopts an AgNO3 / HF acid system, and the second acid solution polishing adopts an HF / HNO3 acid system.

[0028] As an implementation manner, the first silicon oxide layer, the first polysilicon layer, the second silicon oxide layer, and the second polysilicon layer are deposited by an atomic layer deposition process or a low pressure chemical vapor deposition process.

[0029] As an achievable manner, the first doping concentration is [3.0-3.5]e 21 , the second doping concentration is [1.5-2.5]e 21 .

[0030] As an achievable manner, the pore surface structure has a pore depth of [300, 400] nm and a pore diameter of [600, 700] nm.

[0031] As an implementable manner, the area of ​​the gate line contact region occupies [2.5%, 3.5%] of the area of ​​one side of the silicon substrate.

[0032] In a second aspect, the present invention provides a solar cell manufactured according to the above-mentioned solar cell processing method.

[0033] In the above scheme, when forming the first polysilicon layer, it is formed by an in-situ doping deposition method, and there is no need to subsequently perform secondary doping on the first polysilicon layer by diffusion. Therefore, the problem of leakage caused by secondary diffusion penetrating the silicon oxide layer is avoided. In addition, the first polysilicon layer is formed by an in-situ doping deposition method, and its doping concentration is high. As the doping concentration increases, the contact strength between the gate line and the first polysilicon layer can be improved to prevent the gate line from falling off. In addition, the formation of a hole surface structure in the gate line contact area can improve the contact performance between the layered structures, thereby enhancing the contact performance of the selective emitter (SE) structure, thereby improving the conversion efficiency of the solar cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Other features, objects and advantages of the present application will become more apparent by reading the detailed description of non-limiting embodiments made with reference to the following drawings:

[0035] Figure 1 A flow chart of a method for processing a solar cell provided in Example 1 of the present invention;

[0036] Figure 2-Figure 9 A schematic diagram of the processing structure of the solar cell processing method provided in Example 1 of the present invention;

[0037] Fig.10 A flow chart of a method for processing a solar cell provided in Example 2 of the present invention;

[0038] Figure 11-Figure 17 A schematic diagram of the structure of the processing process of the solar cell processing method provided in Example 2 of the present invention. DETAILED DESCRIPTION

[0039] The present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention. It is also necessary to explain that, for ease of description, only the parts related to the invention are shown in the accompanying drawings.

[0040] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0041] In the examples of the following embodiments, the order of certain steps can be adjusted according to actual needs. In addition, one or more steps can be omitted or replaced by other existing process steps in the field as needed.

[0042] The patterning (also called patterning process) mentioned in this article includes deposition of film layers, coating of photoresist, mask exposure, development, etching, stripping of photoresist and other processes, which is an existing mature preparation process.

[0043] The following embodiments may include multiple examples.

[0044] Example 1

[0045] like Figure 1-Figure 9 As shown, the processing method of the solar cell provided by the embodiment of the present invention comprises the following steps:

[0046] S101: Provide a silicon substrate 101, wherein one side of the silicon substrate 101 (for example but not limited to the back side of the silicon substrate 101 - the side facing away from the sun when used as a solar cell) has a gate line contact area A and a non-gate line contact area B; wherein the gate line contact area A is the area for preparing the gate line 109 later, and the rest of the area is the non-gate line contact area B. For example but not limited to, the silicon substrate 101 can be an N-type silicon wafer with a resistivity of 0.4-1.8Ω*cm.

[0047] S102: texturing the silicon substrate 101 .

[0048] At least the front side of the silicon substrate 101 may be textured, or both the front and back sides of the silicon substrate 101 may be textured to form a pyramid light trapping structure, namely, a textured surface structure 1011 , on the corresponding surface.

[0049] A potassium hydroxide solution with a concentration of 0.8% to 1.2% may be used for texturing. For example, a potassium hydroxide solution with a mass fraction of 0.8%, 0.9%, 1% or 1.2% may be used as a texturing additive in a tank cleaning machine to texturize the silicon substrate 101 .

[0050] S103: Boron diffusion is performed on the front surface of the silicon substrate 101 after the texturing.

[0051] BCl3 may be used to diffuse boron on the front surface of the texturized silicon substrate 101 to form a boron diffusion layer.

[0052] S104: polishing the back side of the textured silicon substrate 101 with an alkaline solution.

[0053] The back side of the silicon substrate 101 is polished with an alkaline solution to obtain a silicon substrate 101 having a block structure 1012 on the back side.

[0054] In the embodiment of the present invention, the square structure 1012 refers to a structure in which a plurality of squares are distributed on the surface of the silicon substrate 101, and the surface of each square is flat, wherein the silicon substrate 101 can be polished to obtain a silicon wafer having the square structure 1012 on the surface, wherein an alkaline solution polishing process can be selected, and the type and concentration of the alkaline solution and the size of the squares in the square structure 1012 can also be selected according to specific needs. For example, in this example, a KOH solution is selected to polish the back side of the silicon substrate.

[0055] By polishing the back side of the silicon substrate 101 with an alkaline solution, the specific surface area of ​​the back side is made smaller, and relatively fewer microstructures are generated. A lower interface state density can be obtained when each SiOx layer is deposited and grown in the subsequent process, and the passivation effect is more excellent. A polishing structure with high passivation performance is achieved, and the battery open circuit voltage Uoc of the manufactured battery is also relatively higher.

[0056] S105 : depositing an acid polishing protective layer 102 on the back side of the silicon substrate 101 after being polished by an alkaline solution, and patterning the acid polishing protective layer 102 to form a first opening 1021 exposing the gate line contact region A.

[0057] The acid polishing protective layer 102 may be a SiNx layer, and the SiNx layer may be deposited on the back side of the silicon substrate 101 after being polished by an alkaline solution by a plasma enhanced chemical vapor deposition (PECVD) process.

[0058] A first photoresist layer 103 is coated on the acid polishing protective layer 102, and the first photoresist layer 103 is exposed and developed to form a third opening 1031 exposing the acid polishing protective layer 102. That is to say, in the first photoresist layer 103, the photoresist corresponding to the gate line contact area A is removed, so that the acid polishing protective layer 102 within the gate line contact area A is not blocked by the first photoresist layer 103.

[0059] The coating process of the first photoresist layer 103 can be any existing coating process.

[0060] The acid polishing protection layer 102 within the range of the third opening 1031 is removed, and a first opening 1021 with the gate line contact region A exposed is obtained in the acid polishing protection layer 102 .

[0061] The removal process can be determined according to the material of the acid polishing protective layer 102. As described above, if the acid polishing protective layer 102 is a SiNx layer, HF acid pickling can be used to remove the acid polishing protective layer 102 within the range of the third opening 1031. The concentration of HF acid, pickling time and pickling temperature can be determined according to the thickness of the acid polishing protective layer 102 to ensure that the acid polishing protective layer 102 within the range of the third opening 1031 is completely removed, so as to facilitate the subsequent formation of a hole surface structure 1013 in the gate line contact area A.

[0062] S106 : performing acid solution polishing to form a hole surface structure 1013 at the position of the first opening 1021 , that is, the gate line contact area A on the back side of the silicon substrate 101 .

[0063] The acid solution polishing includes a first acid solution polishing and a second acid solution polishing performed sequentially; the first acid solution polishing adopts an AgNO3 / HF acid system, and the second acid solution polishing adopts an HF / HNO3 acid system. That is, a hole is dug on the back of the silicon substrate 101 in the gate line contact area A by using the AgNO3 / HF acid system, and then the hole is expanded by using the HF / HNO3 acid system to form a porous hole surface structure, thereby increasing the contact area with the first silicon oxide layer 104 formed subsequently, so as to improve the contact performance.

[0064] S107: sequentially depositing a first silicon oxide layer 104 and a first polysilicon layer 105 on the hole surface structure 1013 , wherein the first polysilicon layer 105 is formed by an in-situ doping deposition method, and the first polysilicon layer 105 has a first doping concentration.

[0065] The first silicon oxide layer 104 and the first polysilicon layer 105 are sequentially deposited by a low pressure chemical vapor deposition (LPCVD) process. Of course, in other examples, an atomic layer deposition (ALD) process may also be used to deposit the first silicon oxide layer 104. By depositing the first silicon oxide layer 104, and the subsequent first polysilicon layer 105, the second silicon oxide layer 110, and the second polysilicon layer 111 by LPCVD, a good step coverage film structure can be obtained, that is, a uniform film structure can also be deposited at the hole surface structure 1013, so that the first silicon oxide layer 104 has a good passivation effect.

[0066] The first polysilicon layer 105 is formed by an in-situ doping deposition method, which means that during the process of depositing the first polysilicon layer 105 by LPCVD, a doping gas, such as PH3, is introduced into the LPCVD working chamber to form the first polysilicon layer 105 having a first doping concentration, wherein the in-situ doping can obtain a higher doping concentration.

[0067] A second SiNx layer (not shown in the figure) is deposited on the first polysilicon layer 105, and a third photoresist (not shown in the figure) is coated on the second SiNx layer. The third photoresist layer is exposed and developed to form a fifth opening of the second SiNx layer exposing the non-gate line contact area B. That is, in the third photoresist layer, the photoresist corresponding to the non-gate line contact area is removed so that the second SiNx layer in the non-gate line contact area B is not blocked by the third photoresist layer, and the second SiNx layer in the fifth opening is removed by HF acid pickling to expose the surface of the non-gate line contact area B of the first polysilicon layer 105, and the first polysilicon layer 105 and the first silicon oxide layer 104 in the non-gate line contact area B are removed by alkaline washing to expose the surface of the non-gate line contact area B on the back of the silicon substrate 101. For example, alkaline washing can be performed by an alkaline solution containing KOH. The remaining third photoresist layer and the second SiNx layer are then removed. Herein, each photoresist layer can be removed by, but is not limited to, laser etching, and each SiNx layer is removed by HF acid pickling.

[0068] S108 : depositing a second silicon oxide layer 110 and a second polysilicon layer 111 on the non-gate line contact region B in sequence.

[0069] The back side of the structure formed in the above step S106 is sequentially deposited by an LPCVD deposition process to form a second silicon oxide layer 110 and a second polysilicon layer 111 .

[0070] Phosphorus is diffused into the second polysilicon layer 111 to form the second polysilicon layer 111 having a second doping concentration, wherein the second doping concentration is less than the first doping concentration.

[0071] S109: removing the wrap-around plating, that is, removing the polysilicon deposited on the front and side surfaces in the above steps.

[0072] For example, in a tank cleaning machine, a potassium hydroxide solution with a mass fraction of 0.8%, 0.9%, 1% or 1.2% is used for alkaline washing to remove the wrap-around plating.

[0073] S110: An AlOx layer 107 and a third SiNx layer 106 are sequentially deposited on the front side.

[0074] An AlOx layer 107 and a third SiNx layer 106 are sequentially deposited on the front side of the structure formed in the above step S108.

[0075] S111: depositing a fourth SiNx layer 108 on the back side.

[0076] A fourth SiNx layer 108 is deposited on the back side of the structure formed in the above step S109.

[0077] S112: preparing the gate line 109.

[0078] For example, electrode paste is printed in the gate line contact region A by screen printing, and the electrode paste is sintered to form the gate line 109 in ohmic contact with the first polysilicon layer 105 .

[0079] In the above scheme, when forming the first polysilicon layer 105, it is formed by an in-situ doping deposition method, and there is no need to subsequently perform secondary doping on the first polysilicon layer 105 by diffusion. Therefore, the problem of leakage caused by secondary diffusion penetrating the first silicon oxide layer 104 is avoided. In addition, the first polysilicon layer 105 is formed by an in-situ doping deposition method, and its doping concentration is high. As the doping concentration increases, the contact strength between the gate line 109 and the first polysilicon layer 105 can be improved to prevent the gate line 109 from falling off. In addition, the formation of a hole surface structure in the gate line contact area A can improve the contact performance between the layered structures, thereby enhancing the contact performance of the selective emitter (SE) structure, thereby improving the conversion efficiency of the solar cell.

[0080] Example 2

[0081] like Figure 10-Figure 17 As shown, the processing method of the solar cell provided by the embodiment of the present invention comprises the following steps:

[0082] S201: Provide a silicon substrate 201, wherein one side of the silicon substrate 201 (for example but not limited to the back side of the silicon substrate 201 - the side facing away from the sun when used as a solar cell) has a gate line contact area A and a non-gate line contact area B; wherein the gate line contact area A is the area where the gate line 210 is subsequently prepared, and the remaining area is the non-gate line contact area B. For example but not limited to, the silicon substrate 201 can be an N-type silicon wafer with a resistivity of 0.4-1.8Ω*cm.

[0083] S202: texturing the silicon substrate 201 .

[0084] At least the front side of the silicon substrate 201 may be textured, or both the front and back sides of the silicon substrate may be textured to form a pyramid light trapping structure, namely, a textured surface structure 2011 , on the corresponding surface.

[0085] Among them, a potassium hydroxide solution with a concentration of 0.8% to 1.2% can be used for texturing. For example, a potassium hydroxide solution with a mass fraction of 0.8%, 0.9%, 1% or 1.2% can be used as a texturing additive in a tank cleaning machine to texturize the silicon substrate 201.

[0086] S203: Boron diffusion is performed on the front surface of the textured silicon substrate 201 .

[0087] BCl3 may be used to diffuse boron on the front surface of the texturized silicon substrate 201 to form a boron diffusion layer.

[0088] S204: polishing the back side of the silicon substrate 201 with an acid solution to obtain a surface 2012 having a hole structure.

[0089] The acid solution polishing includes a first acid solution polishing and a second acid solution polishing performed sequentially; the first acid solution polishing adopts an AgNO3 / HF acid system, and the second acid solution polishing adopts an HF / HNO3 acid system. That is, a hole is dug on the back of the silicon substrate 201 by the AgNO3 / HF acid system, and then the hole is expanded by the HF / HNO3 acid system to form a porous hole surface structure, thereby increasing the contact area with the first silicon oxide layer formed subsequently, so as to improve the contact performance.

[0090] S205 : depositing an alkali-polished protective layer 202 on the surface 2012 having the hole structure, and patterning the alkali-polished protective layer 202 to form a second opening 2021 exposing the non-gate line contact region B.

[0091] A sixth SiNx layer is deposited on the surface 2012 of the hole structure as an alkali polishing protection layer 202 to protect the hole structure under the alkali polishing protection layer 202 from being removed during polishing with an alkali solution.

[0092] A second photoresist layer (not shown) is coated on the alkali polishing protection layer 202 , and the second photoresist layer is exposed and developed to form a fourth opening exposing the alkali polishing protection layer 202 , wherein the fourth opening corresponds to the non-gate line contact region B.

[0093] The alkali-polished protective layer 202 within the range of the fourth opening is removed, and the second opening 2021 with the non-gate line contact region B exposed is obtained in the alkali-polished protective layer 202 .

[0094] S206 : performing alkaline solution polishing on the second opening 2021 to remove the hole structure in the non-gate line contact region B and retain the hole structure in the gate line contact region A, thereby obtaining the hole surface structure 214 located in the gate line contact region A.

[0095] The second opening 2021 on the back side of the silicon substrate 201 is polished with an alkaline solution to remove the hole structure in the non-gate line contact area B, so that a surface with a block structure 2013 can be obtained at the position of the second opening 2021 .

[0096] In the embodiment of the present invention, the block structure 2013 refers to a structure in which a plurality of blocks are distributed on the surface of the silicon substrate 201, and the surface of each block is flat, wherein the silicon substrate 201 can be polished to obtain a silicon wafer having the block structure 2013 on the surface, wherein an alkaline solution polishing process can be selected, and the type and concentration of the alkaline solution, and the block size in the block structure 2013 can also be selected according to specific needs. For example, in this example, a KOH solution is selected to polish the back side of the silicon substrate. After the alkaline solution polishing, the remaining second photoresist layer and the alkaline polishing protective layer 202 are removed.

[0097] By polishing the back side of the silicon substrate 201 with an alkaline solution, the specific surface area of ​​the back side is made smaller, and relatively fewer microstructures are generated. A lower interface state density can be obtained when each SiOx layer is deposited and grown in the subsequent process, and the passivation effect is more excellent. A polished structure with high passivation performance is achieved, and the battery open circuit voltage Uoc of the manufactured battery is also relatively higher.

[0098] S207: sequentially depositing a first silicon oxide layer 203 and a first polysilicon layer 204 on the hole surface structure 2014 , wherein the first polysilicon layer 204 is formed by an in-situ doping deposition method, and the first polysilicon layer 204 has a first doping concentration.

[0099] The first silicon oxide layer 203 and the first polysilicon layer 204 are sequentially deposited by a low pressure chemical vapor deposition (LPCVD) process. Of course, in other examples, the first silicon oxide layer 203 may also be deposited by an atomic layer deposition (ALD) process. By depositing the first silicon oxide layer 203, and the subsequent first polysilicon layer 204, the second silicon oxide layer 205, and the second polysilicon layer 206 by LPCVD, a good step coverage film structure can be obtained, that is, a uniform film structure can also be deposited at the hole surface structure, so that the first silicon oxide layer 203 has a good passivation effect.

[0100] The first polysilicon layer 204 is formed by an in-situ doping deposition method, which means that during the process of depositing the first polysilicon layer 204 by LPCVD, a doping gas, such as PH3, is introduced into the LPCVD working chamber to form the first polysilicon layer 204 having a first doping concentration, wherein the in-situ doping can obtain a higher doping concentration.

[0101] A second SiNx layer (not shown in the figure) is deposited on the first polysilicon layer, and a third photoresist (not shown in the figure) is coated on the second SiNx layer, and the third photoresist layer is exposed and developed to form a fifth opening of the second SiNx layer exposing the non-gate line contact area B, that is, in the third photoresist layer, the photoresist corresponding to the non-gate line contact area B is removed, so that the second SiNx layer in the non-gate line contact area B is not blocked by the third photoresist layer, and the second SiNx layer in the range of the fifth opening is removed by HF acid pickling to expose the surface of the first polysilicon layer 204 non-gate line contact area B, and the first polysilicon layer 204 and the first silicon oxide layer 203 in the non-gate line contact area B are removed by alkali washing to expose the surface of the non-gate line contact area B on the back of the silicon substrate, for example, alkali washing can be performed by an alkali solution containing KOH. Then, the remaining third photoresist layer and the second SiNx layer are removed. In this article, each photoresist layer can be but not limited to being removed by laser etching, and each SiNx layer is removed by HF acid pickling.

[0102] S208: depositing a second silicon oxide layer 205 and a second polysilicon layer 206 on the non-gate line contact region B in sequence.

[0103] The back side of the structure formed in the above step S206 is sequentially deposited by an LPCVD deposition process to form a second silicon oxide layer 205 and a second polysilicon layer 206 .

[0104] Phosphorus is diffused into the second polysilicon layer 206 to form the second polysilicon layer 206 having a second doping concentration, wherein the second doping concentration is less than the first doping concentration.

[0105] S209: removing the wrap-around plating, that is, removing the polysilicon deposited on the front and side surfaces in the above steps.

[0106] For example, in a tank cleaning machine, a potassium hydroxide solution with a mass fraction of 0.8%, 0.9%, 1% or 1.2% is used for alkaline washing to remove the wrap-around plating.

[0107] S210: An AlOx layer 208 and a third SiNx layer 207 are sequentially deposited on the front side.

[0108] An AlOx layer 208 and a third SiNx layer 207 are sequentially deposited on the front side of the structure formed in the step S208.

[0109] S211: depositing a fourth SiNx layer 209 on the back side.

[0110] A fourth SiNx layer 209 is deposited on the back side of the structure formed in the above step S209.

[0111] S212: preparing the gate line 210 .

[0112] For example, the electrode paste is printed in the gate line contact region A by screen printing, and the electrode paste is sintered to form the gate line 210 in ohmic contact with the first polysilicon layer 204 .

[0113] Example 3

[0114] The processing method of the solar cell provided in this embodiment is different from the above embodiment mainly in that the first doping concentration is [3.0-3.5]e 21 , the second doping concentration is [1.5-2.5]e 21 .

[0115] The first doping concentration can be 3.0e 21 , 3.1e 21 , 3.2e 21 , 3.2e 21 , 3.5e 21 The second doping concentration can be 1.5e 21 , 1.6e 21 , 1.7e 21 , 1.8e 21 , 2.5e 21 wait.

[0116] Example 4

[0117] The processing method of the solar cell provided in this embodiment is different from the above-mentioned embodiment mainly in that the hole depth of the hole surface structure is [300, 400] nm and the hole diameter is [600, 700] nm.

[0118] For example, the pore depth is 300 nm, 350 nm, 400 nm, etc., and the pore diameter is 600 nm, 650 nm, 700 nm, etc.

[0119] Example 5

[0120] The processing method of the solar cell provided in this embodiment is different from the above-mentioned embodiment mainly in that the area of ​​the gate line contact region occupies [2.5%, 3.5%] of the area of ​​one side (eg, the back side) of the silicon substrate.

[0121] For example, the area of ​​the gate line contact region accounts for 2.5%, 2.8%, 3%, 3.5%, etc. of the area of ​​the back side of the silicon substrate.

[0122] In a second aspect, an embodiment of the present invention further provides a solar cell manufactured according to any of the above-mentioned solar cell processing methods.

[0123] The ToPCon battery provided by the embodiment of the present invention has a back surface structure with selective polishing on the back side, and different back surface structures are obtained in different areas. The back grid line contact portion is polished using an acid system to achieve a polished structure with high contact performance, which can better match the back selective TopCon battery. The back grid line non-contact portion is polished using an alkali system, which has the advantages of a smaller specific surface area and relatively fewer microstructures. A lower interface state density can be obtained when SiOx is deposited and grown in the subsequent process, and the passivation effect is more excellent. A polished structure with high passivation performance is achieved, and the Uoc of the manufactured battery is relatively higher. The selective polishing structure takes into account both the high contact performance and high passivation performance of the back side, and effectively matches the back surface structure requirements of the back selective battery, so that the Uoc and FF of the ToPCon battery are greatly improved, thereby achieving the effect of greatly improving the conversion efficiency. Matching the appropriate slurry can simultaneously meet the requirements of high contact, high passivation, and high grid line adhesion.

[0124] In addition, the selective electrode structure realized by in-situ doping and non-in-situ doping can avoid the side effects of the existing selective electrode structure realization methods, such as secondary non-in-situ doping causing the doping atoms and phosphorus atoms to diffuse through SiOx, which can easily cause battery leakage. The laser heavy doping method also has such problems, and laser heavy doping can easily cause damage to silicon wafers. The present invention can effectively solve the above problems.

[0125] It should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like used above to indicate orientations or positional relationships are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.

[0126] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept. For example, the above features are replaced with the technical features with similar functions disclosed in this application (but not limited to) by each other.

Claims

1. A method for processing a solar cell, characterized in that: The following steps are involved: Providing a silicon substrate, wherein one side of the silicon substrate has a gate line contact region and a non-gate line contact region; forming a hole surface structure in the gate line contact region; Depositing a first silicon oxide layer and a first polysilicon layer in sequence on the hole surface structure, wherein the first polysilicon layer is formed by an in-situ doping deposition method, and the first polysilicon layer has a first doping concentration; sequentially depositing a second silicon oxide layer and a second polysilicon layer on the non-gate line contact region; doping the second polysilicon layer to obtain a second polysilicon layer with a second doping concentration, wherein the second doping concentration is less than the first doping concentration; A gate line is formed in the gate line contact region, and the gate line is in ohmic contact with the first polysilicon layer.

2. The method for processing a solar cell according to claim 1, characterized in that: The hole surface structure is formed in the gate line contact area, specifically: Polishing one side of the silicon substrate with an alkaline solution; Depositing an acid polishing protective layer on the surface polished by the alkaline solution, and patterning the acid polishing protective layer to form a first opening exposing the gate line contact area; Performing acid solution polishing on the first opening to form the hole surface structure located in the gate line contact area; or, Polishing one side of the silicon substrate with an acid solution to obtain a surface with a hole structure; Depositing an alkali-polished protective layer on the surface having the hole structure, and patterning the alkali-polished protective layer to form a second opening exposing the non-gate line contact area; The second opening is polished with an alkaline solution to remove the hole structure in the non-gate line contact area and retain the hole structure in the gate line contact area to obtain the hole surface structure located in the gate line contact area.

3. The method for processing a solar cell according to claim 2, characterized in that: The step of depositing an acid polishing protective layer on the surface polished by the alkaline solution and patterning the acid polishing protective layer to form a first opening exposing the gate line contact area is specifically as follows: Depositing an acid polishing protective layer on the surface polished by the alkaline solution; Coating a first photoresist layer on the acid polishing protective layer, exposing and developing the first photoresist layer to form a third opening exposing the acid polishing protective layer; The acid polishing protection layer within the range of the third opening is removed, and the first opening exposing the gate line contact area is obtained in the acid polishing protection layer.

4. The method for processing a solar cell according to claim 2, characterized in that: The step of depositing an alkali-polished protective layer on the surface having the hole structure and patterning the alkali-polished protective layer to form a second opening exposing the non-gate line contact area is specifically as follows: Depositing an alkali polishing protective layer on the surface having the porous structure; Coating a second photoresist layer on the alkali polishing protective layer, exposing and developing the second photoresist layer to form a fourth opening exposing the alkali polishing protective layer; The alkali-polished protective layer within the range of the fourth opening is removed, and the second opening exposing the non-gate line contact area is obtained in the alkali-polished protective layer.

5. The method for processing a solar cell according to claim 3 or 4, characterized in that: The acid solution polishing includes a first acid solution polishing and a second acid solution polishing performed sequentially; the first acid solution polishing adopts an AgNO3 / HF acid system, and the second acid solution polishing adopts an HF / HNO3 acid system.

6. The method for processing a solar cell according to any one of claims 1 to 4, characterized in that: The first silicon oxide layer, the first polysilicon layer, the second silicon oxide layer, and the second polysilicon layer are deposited by an atomic layer deposition process or a low pressure chemical vapor deposition process.

7. The method for processing a solar cell according to any one of claims 1 to 4, characterized in that: The first doping concentration is [3.0-3.5]e 21 , the second doping concentration is [1.5-2.5]e 21 .

8. The method for processing a solar cell according to any one of claims 1 to 4, characterized in that: The pore surface structure has a pore depth of [300, 400] nm and a pore diameter of [600, 700] nm.

9. The method for processing a solar cell according to any one of claims 1 to 4, characterized in that: The area of ​​the gate line contact region accounts for [2.5%, 3.5%] of the area of ​​one side of the silicon substrate.

10. A solar cell, characterized in that: The solar cell is prepared according to the processing method of any one of claims 1 to 9.