A sand mold riser seat and its application

By designing the upper wide and lower narrow conical holes of the sand-shaped riser seat and the specific raw material ratio, the problems of large contact area and shrinkage holes in traditional sand-shaped casting are solved, and more efficient production and product quality improvement are achieved.

CN114769511BActive Publication Date: 2024-11-05SHANDONG YANSHAN PRECISION MASCH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210386193.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-13
Publication Date
2024-11-05
Estimated Expiration
2042-04-13

AI Technical Summary

Technical Problem

The riser design in traditional sand casting results in a large contact area at the hot joints of the casting, which increases cutting and grinding time, and is prone to shrinkage hole cracks, affecting product quality.

Method used

Design a sand-shaped riser seat, where the middle hole is a conical hole with a wide upper and narrow lower bottom, and is prepared in combination with a specific ratio of raw materials, including bead sand, scrap steel balls and resin, to reduce the contact area between castings and material heads and shrinkage holes , improve the breathability of the molded sand.

Benefits of technology

The cutting and grinding time is shortened, the production rate is increased by 20%, the shrinkage hole crack phenomenon is reduced, and the strength and product quality of the castings are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114769511B_ABST
    Figure CN114769511B_ABST
Patent Text Reader

Abstract

The invention discloses a sand mold riser seat, wherein the raw materials of the sand mold riser seat are composed of the following components in weight percentage: 70-80% of precious sand, 10-15% of scrap steel shot, 7-10% of resin, and 3-5% of curing agent; the sand mold riser seat is prepared by mixing the above raw materials and adding them into a mold for curing and molding. The middle hole of the sand mold riser seat of the invention is a tapered hole that is wide at the top and narrow at the bottom, and the bottom of the tapered hole contacts the casting, the contact area is reduced, the cutting and grinding time is shortened, and the yield rate is increased by 20%; the sand mold riser seat prepared by raw materials of a specific ratio contacts the casting at the shrinkage compensation part, reduces the shrinkage and shrinkage crack phenomenon at the contact part between the casting and the material head, and ensures the product quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sand casting, in particular to a sand mold riser seat and application thereof. Background Art

[0002] Sand casting is the most traditional casting method. Due to its own characteristics (not limited by part shape, size, complexity and alloy type, short production cycle and low cost), sand casting is still the most widely used casting method in casting production. The basic process of traditional sand casting technology has the following steps: sand preparation, mold making, core making, molding, pouring, sand dropping, grinding, inspection and other steps.

[0003] In sand casting, according to the requirements of the casting, risers need to be placed at the hot spots, wall thickness, and high end of the casting for the purpose of exhaust, shrinkage compensation, slag collection, etc. Figure 1 As shown in the figure, during shrinkage compensation, the contact area between the material head in the riser and the casting is large, which increases the time for subsequent cutting and grinding and reduces the yield rate. At the same time, shrinkage, shrinkage holes and cracks are prone to occur at the contact point between the casting and the material head, affecting product quality. Summary of the invention

[0004] In view of the deficiencies of the above-mentioned prior art, the purpose of the present invention is to provide a sand mold riser seat and its application. The middle hole of the sand mold riser seat of the present invention is a tapered hole that is wide at the top and narrow at the bottom. The bottom of the tapered hole contacts the casting, the contact area is reduced, the cutting and grinding time is shortened, and the yield rate is increased by 20%; the sand mold riser seat prepared with raw materials in a specific ratio contacts the casting at the shrinkage compensation position, reducing the shrinkage, shrinkage and cracking phenomena at the contact position between the casting and the material head, and ensuring the product quality; the combination of the molding sand prepared with specific raw materials and raw material ratios and the sand mold riser seat reduces the shrinkage and shrinkage inside the casting, and increases the strength.

[0005] To achieve the above object, the present invention adopts the following technical solution:

[0006] A first aspect of the present invention provides a sand mold riser seat, wherein the raw materials of the sand mold riser seat are composed of the following components in weight percentage: 70-80% of precious sand, 10-15% of scrap steel shot, 7-10% of resin, and 3-5% of curing agent; the sand mold riser seat is prepared by mixing the above raw materials and adding them into a mold for curing and molding.

[0007] Preferably, the sand mold riser seat includes a placement seat body, the upper surface of the placement seat body is a plane, the lower surface of the placement seat body is a three-step structure, a middle hole is provided on the placement seat body, the middle hole is a conical hole that is wide at the top and narrow at the bottom, the three-step structure includes a first step, a second step and a third step that rise step by step, and the middle hole is located on the second step.

[0008] Preferably, the height of the first step is 10 mm, the height of the second step is 20 mm, and the height of the third step is 30 mm.

[0009] Preferably, the placement seat body is an arc-shaped structure, and the curvature of the placement seat body is adapted to the curvature of the prefabricated circular valve plate; the outer periphery of the circular valve plate is a three-level boss structure, and the three-level boss structure includes a first boss, a second boss and a third boss that rise step by step; the three-level step structure fits the three-level boss structure.

[0010] Preferably, the diameter of the upper end of the middle hole is 70 mm, and the diameter of the lower end of the middle hole is 50 mm.

[0011] Preferably, the arc angle of the placement seat body is 97°.

[0012] Preferably, the curing time of the sand mold riser seat in the mold is 5-10 minutes.

[0013] Preferably, the particle size of the precious sand is 40-70 mesh, and the diameter of the scrap steel shot is ≤0.1 mm.

[0014] Preferably, the resin is an alkaline phenolic resin, and the curing agent is an organic ester curing agent, specifically a fatty amine.

[0015] A second aspect of the present invention provides a casting method, comprising the following steps:

[0016] (1) Molding sand;

[0017] (2) Lower box shape;

[0018] (3) preparing the above-mentioned sand mold riser seat;

[0019] (4) Upper box molding, placing the sand mold riser seat on the pattern and fitting it with the pattern, the sand mold riser seat is specifically placed at the position where shrinkage needs to be compensated by the riser, the sand mold riser seat and the pattern are placed in the upper box and filled with molding sand burying box, when the buried molding sand height is flush with the top of the sand mold riser seat, a heating and insulation riser is placed on the sand mold riser seat, the bottom of the heating and insulation riser is connected to the sand mold riser seat so that the heating and insulation riser is connected to the middle hole of the sand mold riser seat; continue to bury the molding sand until the molding sand is flush with the upper end of the heating and insulation riser, and complete the upper box molding;

[0020] (5) Assembling and pouring;

[0021] (6) Sanding and grinding.

[0022] Preferably, in step (1), the raw materials of the molding sand are composed of the following components in weight percentage: 70-80% of precious sand, 10-15% of scrap steel shot, 7-10% of resin, and 3-5% of curing agent.

[0023] Preferably, the resin is an alkaline phenolic resin, and the curing agent is an organic ester curing agent, specifically a fatty amine.

[0024] Preferably, the particle size of the precious sand is 40-70 mesh, and the diameter of the scrap steel shot is ≤0.1 mm.

[0025] Preferably, the casting is a circular valve plate.

[0026] Preferably, in step (5), the pouring temperature is 1600-1610°C.

[0027] Preferably, in step (2), the lower box molding is specifically to place the pattern into the lower box, and to place molding sand into the lower box to complete the lower box molding.

[0028] Preferably, the casting is made of 304 stainless steel or 316 stainless steel.

[0029] Beneficial effects of the present invention:

[0030] 1. The middle hole of the sand mold riser seat of the present invention is a tapered hole that is wide at the top and narrow at the bottom. The bottom of the tapered hole contacts the casting, the contact area is reduced, the cutting and grinding time is shortened, the cutting time is reduced from 5 minutes of the raw material to 1 minute, the output rate is increased by 20%, and the molten steel utilization rate of the product is improved.

[0031] 2. The sand mold riser seat prepared with raw materials of specific proportions contacts the casting at the shrinkage compensation part, reducing the shrinkage, shrinkage and cracking phenomena at the contact part between the casting and the material head, and ensuring the product quality. The present invention adopts scrap steel shot and gem sand to cooperate, on the one hand, to reuse the scrap steel shot, increase the utilization value of the waste, and the utilization amount of scrap steel shot is large, on the other hand, the scrap steel shot in the raw material can increase the cooling speed of the casting, and the cooling effect is good. The cooperation of gem sand and scrap steel shot in a specific proportion can make the air permeability of the molding sand not too high or too low, and make the air permeability of the molding sand just right; the cooperation of the molding sand prepared by specific raw materials and raw material ratios and the sand mold riser seat can reduce the shrinkage and shrinkage inside the casting. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a valve obtained by the existing method; A in the figure is the contact area between the material head and the casting, with a large contact area and many shrinkage cracks;

[0033] Figure 2 The valve is obtained by the method of the present invention; B in the figure is the contact part between the material head and the casting, the contact area is small, and there are few shrinkage cracks;

[0034] Figure 3 It is a cross-sectional view of the sand mold riser seat of the present invention;

[0035] Figure 4It is a cross-sectional view showing the positional relationship of the heat-insulating riser, the sand-molded riser seat and the circular valve plate pattern of the present invention;

[0036] Figure 5 It is a schematic diagram of the top view of the structure of the sand mold riser seat of the present invention;

[0037] As shown in the figure:

[0038] 1. The third step, 2. The second step, 3. The first step, 4. The middle hole, 5. The heat-generating and heat-insulating riser, 6. The first boss, 7. The second boss, 8. The third boss. DETAILED DESCRIPTION

[0039] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0040] In order to enable those skilled in the art to more clearly understand the technical solution of the present application, the technical solution of the present application will be described in detail below in conjunction with specific embodiments.

[0041] Embodiment 1:

[0042] A casting method for a circular valve plate comprises the following steps:

[0043] (1) Molding sand: The raw materials of the molding sand are composed of the following components in weight percentage: 70% of quartz sand, 15% of scrap steel shot, 10% of alkaline phenolic resin, and 5% of fatty amine; the grain size of the quartz sand is 40-70 mesh, and the diameter of the scrap steel shot is ≤ 0.1 mm;

[0044] (2) Lower box molding: The lower box molding specifically involves placing the pattern into the lower box, and placing molding sand into the lower box to complete the lower box molding;

[0045] (3) preparing a sand mold riser seat; the raw materials of the sand mold riser seat are composed of the following components in weight percentage: 70% of quartz sand, 15% of scrap steel shot, 10% of alkaline phenolic resin, and 5% of fatty amine; the grain size of the quartz sand is 40-70 mesh, and the diameter of the scrap steel shot is ≤0.1 mm; the sand mold riser seat is formed by mixing the above raw materials and adding them into a mold for curing for 5-10 minutes;

[0046] (4) Upper box molding, placing the sand mold riser seat on the pattern and fitting it with the pattern, the sand mold riser seat is specifically placed at the position where shrinkage needs to be compensated by the riser, the sand mold riser seat and the pattern are placed in the upper box and filled with molding sand burying box, when the buried molding sand height is flush with the top of the sand mold riser seat, a heating and insulation riser is placed on the sand mold riser seat, the bottom of the heating and insulation riser is connected to the sand mold riser seat so that the heating and insulation riser is connected to the middle hole of the sand mold riser seat; continue to bury the molding sand until the molding sand is flush with the upper end of the heating and insulation riser, and complete the upper box molding;

[0047] (5) Assemble the box and pour; the pouring temperature is 1600-1610℃;

[0048] (6) After sand removal and grinding, the casting is made of 304 stainless steel.

[0049] Embodiment 2:

[0050] A casting method for a circular valve plate comprises the following steps:

[0051] (1) Molding sand: The raw materials of the molding sand are composed of the following components in weight percentage: 80% of quartz sand, 10% of scrap steel shot, 7% of alkaline phenolic resin, and 3% of fatty amine; the particle size of the quartz sand is 40-70 mesh, and the diameter of the scrap steel shot is ≤0.1 mm;

[0052] (2) Lower box molding: The lower box molding specifically involves placing the pattern into the lower box, and placing molding sand into the lower box to complete the lower box molding;

[0053] (3) preparing a sand mold riser seat; the raw materials of the sand mold riser seat are composed of the following components in weight percentage: 80% of precious sand, 10% of scrap steel shot, 7% of alkaline phenolic resin, and 3% of fatty amine; the sand mold riser seat is formed by mixing the above raw materials and adding them into a mold for curing for 5-10 minutes; the particle size of the precious sand is 40-70 mesh, and the diameter of the scrap steel shot is ≤0.1 mm;

[0054] (4) Upper box molding, placing the sand mold riser seat on the pattern and fitting it with the pattern, the sand mold riser seat is specifically placed at the position where shrinkage needs to be compensated by the riser, the sand mold riser seat and the pattern are placed in the upper box and filled with molding sand burying box, when the buried molding sand height is flush with the top of the sand mold riser seat, a heating and insulation riser is placed on the sand mold riser seat, the bottom of the heating and insulation riser is connected to the sand mold riser seat so that the heating and insulation riser is connected to the middle hole of the sand mold riser seat; continue to bury the molding sand until the molding sand is flush with the upper end of the heating and insulation riser, and complete the upper box molding;

[0055] (5) Assemble the box and pour; the pouring temperature is 1600-1610℃;

[0056] (6) After sand removal and grinding, the casting is made of 304 stainless steel.

[0057] Embodiment 3:

[0058] A casting method for a circular valve plate comprises the following steps:

[0059] (1) Molding sand: The raw materials of the molding sand are composed of the following components in weight percentage: 75% of quartz sand, 13% of scrap steel shot, 8% of alkaline phenolic resin, and 4% of fatty amine; the grain size of the quartz sand is 40-70 mesh, and the diameter of the scrap steel shot is ≤0.1 mm;

[0060] (2) Lower box molding: The lower box molding specifically involves placing the pattern into the lower box, and placing molding sand into the lower box to complete the lower box molding;

[0061] (3) preparing a sand mold riser seat; the raw materials of the sand mold riser seat are composed of the following components in weight percentage: 75% of precious sand, 13% of scrap steel shot, 8% of alkaline phenolic resin, and 4% of fatty amine; the sand mold riser seat is formed by mixing the above raw materials and adding them into a mold for curing for 5-10 minutes; the particle size of the precious sand is 40-70 mesh, and the diameter of the scrap steel shot is ≤0.1 mm;

[0062] (4) Upper box molding, placing the sand mold riser seat on the pattern and fitting it with the pattern, the sand mold riser seat is specifically placed at the position where shrinkage needs to be compensated by the riser, the sand mold riser seat and the pattern are placed in the upper box and filled with molding sand burying box, when the buried molding sand height is flush with the top of the sand mold riser seat, a heating and insulation riser is placed on the sand mold riser seat, the bottom of the heating and insulation riser is connected to the sand mold riser seat so that the heating and insulation riser is connected to the middle hole of the sand mold riser seat; continue to bury the molding sand until the molding sand is flush with the upper end of the heating and insulation riser, and complete the upper box molding;

[0063] (5) Assemble the box and pour; the pouring temperature is 1600-1610℃;

[0064] (6) After sand removal and grinding, the casting is made of stainless steel 316.

[0065] Among them, Figure 3-5 As shown, the sand mold riser seat includes a placement seat body, the upper surface of the placement seat body is a plane, the lower surface of the placement seat body is a three-step structure, a middle hole 4 is provided on the placement seat body, the middle hole 4 is a conical hole that is wide at the top and narrow at the bottom, the three-step structure includes a first step 3, a second step 2 and a third step 1 that rise step by step, and the middle hole 4 is located on the second step 2.

[0066] The height of the first step 3 is 10mm, the height of the second step 2 is 20mm, and the height of the third step 1 is 30mm. The placement seat body is an arc-shaped structure, and the curvature of the placement seat body is adapted to the curvature of the prefabricated circular valve plate; the outer periphery of the circular valve plate is a three-level boss structure, and the three-level boss structure includes a first boss 6, a second boss 7 and a third boss 8 that rise step by step; the three-level step structure fits the three-level boss structure. The upper end diameter of the middle hole 4 is 70mm, and the lower end diameter of the middle hole 4 is 50mm. The arc angle of the placement seat body is 97°.

[0067] The circular valve plate castings prepared in Examples 1-3 have significantly reduced internal shrinkage cavities and shrinkage pores, significantly improved pass rates, and significantly increased strength.

[0068] The qualified rate of castings was detected by hydraulic pressure testing, and no leakage was detected at a pressure of 4Mpa. The qualified rate of the products prepared by Example 1 was 98.03%, the qualified rate of the products prepared by Example 2 was 98.11%, and the qualified rate of the products prepared by Example 3 was 98.06%.

[0069] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A sand mold riser seat, characterized in that: The raw materials of the sand mold riser seat are composed of the following components in weight percentage: 70-80% of precious sand, 10-15% of scrap steel shot, 7-10% of resin, and 3-5% of curing agent; the sand mold riser seat is formed by mixing the above raw materials and adding them into a mold for curing; the sand mold riser seat includes a placement seat body, the upper surface of the placement seat body is a plane, the lower surface of the placement seat body is a three-step ladder structure, and a middle hole is provided on the placement seat body. The middle hole is a tapered hole that is wide at the top and narrow at the bottom. The three-step ladder structure includes a first step, a second step and a third step that are gradually increased, and the middle hole is located on the second step; the placement seat body is an arc structure, and the arc of the placement seat body is adapted to the arc of the prefabricated circular valve plate; the outer periphery of the circular valve plate is a three-step boss structure, and the three-step boss structure includes a first boss, a second boss and a third boss that are gradually increased; the three-step ladder structure fits the three-step boss structure; the particle size of the precious sand is 40-70 meshes, and the diameter of the scrap steel shot is ≦0.1mm.

2. The sand mold riser seat according to claim 1, characterized in that: The height of the first step is 10 mm, the height of the second step is 20 mm, and the height of the third step is 30 mm.

3. The sand mold riser seat according to claim 1, characterized in that: The sand mold riser seat solidifies in the mold for 5-10 minutes.

4. A casting method, characterized in that: The steps include: (1) Molding sand; (2) Lower box shape; (3) preparing the sand mold riser seat according to any one of claims 1 to 3; (4) Upper box molding: Place the sand mold riser seat on the pattern and fit it with the pattern. The sand mold riser seat is specifically placed at the position where shrinkage compensation needs to be made through the riser. Put the sand mold riser seat and the pattern into the upper box and fill it with molding sand. When the height of the buried molding sand is flush with the top of the sand mold riser seat, place the heating and insulation riser on the sand mold riser seat. The bottom of the heating and insulation riser is connected to the sand mold riser seat so that the heating and insulation riser is connected to the middle hole of the sand mold riser seat. Continue to bury the molding sand until the molding sand is flush with the upper end of the heating and insulation riser to complete the upper box molding. (5) Assembling and pouring; (6) Sanding and grinding.

5. The method according to claim 4, characterized in that In step (1), the raw materials of the molding sand are composed of the following components in weight percentage: 70-80% of precious sand, 10-15% of scrap steel shot, 7-10% of resin, and 3-5% of curing agent.

6. The method according to claim 4, characterized in that The casting is a circular valve plate.

7. The method according to claim 4, characterized in that In step (5), the pouring temperature is 1600-1610°C.