A cuprous oxide nanoparticle functionalized cellulose hydrogel and its preparation method and application

By in-situ synthesizing cuprous oxide nanoparticles and encapsulating them with tannic acid, the mechanical properties of cellulose hydrogel are enhanced, which solves the problems of poor antifouling performance of cellulose hydrogel and easy flocculation and high toxicity of cuprous oxide nanoparticles. , achieving efficient antifouling effects in the marine environment.

CN114805849BActive Publication Date: 2024-10-01SOUTH CHINA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210382590.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-13
Publication Date
2024-10-01
Estimated Expiration
2042-04-13

AI Technical Summary

Technical Problem

Existing cellulose hydrogels have poor antifouling properties in the marine environment, and the problems of easy flocculation, high toxicity and difficulty in reuse of cuprous oxide nanoparticles have not been effectively solved, affecting their application.

Method used

Cuprous oxide nanoparticles are introduced into cellulose hydrogel through in-situ synthesis and encapsulated with tannic acid to enhance the mechanical properties and antifouling ability of cellulose hydrogel. Combined with the biocidal and antifouling properties of cuprous oxide, Achieve "1+1>2" anti-fouling effect.

Benefits of technology

It improves the mechanical strength and antifouling properties of cellulose hydrogel, solves the problems of easy flocculation and high toxicity of nano-copper oxide, and enhances its durability and broad spectrum of application in the marine environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114805849B_ABST
    Figure CN114805849B_ABST
Patent Text Reader

Abstract

The present invention provides a cuprous oxide nanoparticle functionalized cellulose hydrogel and a preparation method and application thereof. A cellulose hydrogel skeleton with a three-dimensional porous structure is used as an in-situ synthesized microreactor, and the active groups on the cellulose matrix are utilized to anchor cuprous oxide on its surface and inner wall through electrostatic and chelation. Tannic acid is used to encapsulate cuprous oxide, build a bridge between the host and the guest, increase the crosslinking density of the cellulose-based cuprous oxide nanocomposite hydrogel, and thus doubly strengthen the mechanical strength of the cellulose hydrogel. The obtained cuprous oxide nanoparticle functionalized cellulose hydrogel not only solves the problems of easy flocculation, high toxicity, and difficulty in recycling of nano-copper oxide, but also solves the defects existing in the actual application process of marine antifouling, such as the poor broad-spectrum antifouling and environmental durability of cellulose hydrogel. The cuprous oxide nanoparticle functionalized cellulose hydrogel can be used for marine biological antifouling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fiber material preparation, and particularly relates to a cuprous oxide nanoparticle functionalized cellulose hydrogel and a preparation method and application thereof. Background Art

[0002] The attachment, colonization and growth of fouling organisms on the surface of marine structures can lead to a series of destructive effects such as slowing down of ship speed, increased fuel consumption and severe biocorrosion. Introducing Cu2O (cuprous oxide) into cellulose hydrogel can not only solve the defects of cuprous oxide in practical applications such as easy flocculation, high toxicity and difficulty in recycling, but also combine the biocidal and antifouling strategy of cuprous oxide with the fouling inhibition strategy of cellulose hydrogel to achieve an antifouling effect of "1+1>2". In addition, the poor mechanical properties of cellulose hydrogel are the main factor limiting its application. Cuprous oxide nanoparticles with high strength and high toughness can be used as a reinforcing phase to enhance the mechanical strength of cellulose hydrogel to cope with the continuous impact of complex water environments on cellulose hydrogels, thereby improving the environmental durability of cellulose hydrogels.

[0003] The conventional physical blending method for preparing nanocomposite hydrogels requires blending prefabricated nanoparticles with a polymer matrix solution, and then forming a nanocomposite hydrogel through chemical crosslinking. Since the interaction between nanoparticles and polymers is weak, and the presence of nanoparticles weakens the crosslinking density between polymer chains, it has an adverse effect on the mechanical properties of nanocomposite hydrogels. Therefore, finding a suitable loading method to enhance cellulose hydrogels by utilizing the high strength and high toughness mechanical properties of cuprous oxide nanoparticles without destroying the crosslinking network of cellulose hydrogels is an important factor in ensuring the application of cellulose-based nanocomposite hydrogel materials in the field of marine antifouling. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings and deficiencies of the prior art and provide a method for preparing cuprous oxide nanoparticle functionalized cellulose hydrogel.

[0005] Another object of the present invention is to provide cuprous oxide nanoparticle functionalized cellulose hydrogel prepared by the above preparation method.

[0006] Another object of the present invention is to provide an application of the cuprous oxide nanoparticle functionalized cellulose hydrogel.

[0007] The purpose of the present invention is achieved through the following technical solutions:

[0008] A method for preparing cuprous oxide nanoparticle functionalized cellulose hydrogel comprises the following steps:

[0009] (1) Preparation of cellulose solution

[0010] Dissolving sodium hydroxide and urea in water to form a sodium hydroxide / urea aqueous solution, precooling, adding cotton linter pulp to the sodium hydroxide / urea aqueous solution, and stirring to obtain a cellulose solution;

[0011] (2) Preparation of cellulose hydrogel

[0012] Weighing the cellulose solution prepared in step (1), adding epichlorohydrin, stirring, heating to obtain a cellulose hydrogel, and washing; freezing the washed cellulose hydrogel, and freeze-drying to obtain a dried cellulose hydrogel;

[0013] (3) In situ synthesis of cuprous oxide nanoparticles functionalized cellulose hydrogel

[0014] The dried cellulose hydrogel prepared in step (2) is weighed and immersed in a copper sulfate dihydrate solution, and then a sodium hydroxide solution is added dropwise for reaction, and then ascorbic acid is added for stirring and washing to obtain the cuprous oxide nanoparticle functionalized cellulose hydrogel.

[0015] The method for preparing the cuprous oxide nanoparticle functionalized cellulose hydrogel further comprises the following steps:

[0016] In step (3), after the sodium hydroxide solution is added dropwise for reaction, tannic acid is added and stirred.

[0017] The amount of sodium hydroxide added in step (1) is 5% to 10% of the total mass of the sodium hydroxide / urea aqueous solution.

[0018] The amount of urea added in step (1) is 10% to 15% of the total mass of the sodium hydroxide / urea aqueous solution.

[0019] The precooling described in step (1) is precooling to -10 to -15°C for 10 minutes.

[0020] The cotton linter pulp described in step (1) is obtained by crushing a cotton linter pulp board.

[0021] The degree of polymerization of the cotton linter pulp described in step (1) is 600-700.

[0022] The amount of cotton linter pulp added in step (1) is 1-6% of the mass of the sodium hydroxide / urea aqueous solution, preferably 2%.

[0023] The stirring condition described in step (1) is stirring at a speed of 2000-8000 r / min for 10-40 min.

[0024] The mass ratio of the volume of epichlorohydrin described in step (2) to the cotton linter pulp in the cellulose solution is 1-6 mL:0.8 g.

[0025] The stirring condition in step (2) is stirring at 10-30°C for 10-30 min, preferably stirring at 30°C for 30 min.

[0026] The heating conditions in step (2) are heating in a water bath at 50 to 80° C. for 30 to 120 min, preferably heating in a water bath at 60° C. for 60 min.

[0027] The washing conditions described in step (2) are soaking in deionized water for 3 to 7 days, during which the water is changed every 4 to 12 hours.

[0028] The freezing conditions described in step (2) are -18 to -24°C freezing for 1 to 2 days.

[0029] The freeze-drying conditions described in step (2) are to use a freeze dryer to dry for 2 to 4 days.

[0030] The volume ratio of the mass of the cellulose hydrogel described in step (3) to the copper sulfate dihydrate solution is 0.2 g: 50-100 mL.

[0031] The concentration of the copper sulfate dihydrate solution described in step (3) is 0.05-0.50 mol / L.

[0032] The soaking condition described in step (3) is soaking for 4 to 12 hours.

[0033] The volume ratio of the sodium hydroxide solution described in step (3) to the copper sulfate dihydrate solution is 10-50 mL:80 mL.

[0034] The concentration of the sodium hydroxide solution described in step (3) is 1-4 mol / L.

[0035] The reaction time of adding sodium hydroxide solution dropwise in step (3) is 1 to 4 hours.

[0036] The mass ratio of tannic acid to cellulose hydrogel in step (3) is 0.1-0.5:0.2.

[0037] The stirring condition for adding tannic acid in step (3) is 1 to 4 hours.

[0038] The mass ratio of ascorbic acid to cellulose hydrogel in step (3) is 0.5-1.0:0.2.

[0039] The stirring condition for adding ascorbic acid in step (3) is stirring for 2 to 4 hours.

[0040] The washing conditions described in step (3) are soaking in deionized water, with a water change cycle of 8 hours and a soaking cycle of 2 days.

[0041] A cuprous oxide nanoparticle functionalized cellulose hydrogel is prepared by the preparation method.

[0042] Application of the cuprous oxide nanoparticle functionalized cellulose hydrogel in the preparation of antifouling coatings.

[0043] Compared with the prior art, the present invention has the following advantages and effects:

[0044] The invention provides a cuprous oxide nanoparticle functionalized cellulose hydrogel, which uses a cellulose hydrogel skeleton with a three-dimensional porous structure as an in-situ synthesized microreactor, and uses active groups on a cellulose matrix to anchor cuprous oxide nanoparticles on its surface and inner wall through electrostatic and chelation. The in-situ synthesis method not only does not weaken the mechanical strength of the cellulose matrix, but the cuprous oxide nanoparticles well dispersed in the cellulose hydrogel matrix can also play a reinforcing role on the cellulose hydrogel as a reinforcing relative. The cuprous oxide nanoparticles are filled in the defects of the hydrogel, hindering the expansion of microcracks, limiting the movement of cellulose molecular chains, and thus inhibiting the deformation of the cellulose hydrogel under stress. In addition, cuprous oxide nanoparticles encapsulated by tannic acid are used to build a bridge between the host and the guest, increasing the crosslinking density of the cellulose-based cuprous oxide nanoparticle functionalized cellulose hydrogel, thereby doubly strengthening the mechanical strength of the cellulose hydrogel. The obtained cuprous oxide nanoparticle functionalized cellulose hydrogel not only solves the problems of easy flocculation, high toxicity, and difficulty in recycling of nano copper oxide, but also solves the defects existing in the actual application process of marine antifouling, such as poor broad-spectrum antifouling and environmental durability of cellulose hydrogel. In addition, the biocidal and antifouling properties of cuprous oxide nanoparticles and the fouling inhibition properties of cellulose hydrogel are combined to achieve an antifouling effect of "1+1>2". The cuprous oxide nanoparticle-functionalized cellulose hydrogel can be used for marine biofouling prevention. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is a SEM photograph of the cuprous oxide nanoparticle functionalized cellulose hydrogel prepared in Example 6.

[0046] Figure 2 Schematic diagram of the synthesis mechanism of cuprous oxide nanoparticle-functionalized cellulose hydrogel. DETAILED DESCRIPTION

[0047] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.

[0048] The cellulose solution used in the following examples was prepared by the following steps: sodium hydroxide, urea and water were added to a 500 mL beaker in a mass ratio of 7%, 12% and 81%, and stirred to form a 300 g sodium hydroxide / urea aqueous solution; the sodium hydroxide / urea aqueous solution was placed in a low temperature cooling circulation pump and precooled to -12°C for 10 min. Cotton linter pulp (Hubei Chemical Fiber Group Co., Ltd., under 25°C, the degree of polymerization of cellulose in copper ethylenediamine was 623 and the viscosity average molecular weight was 1.01×10 5 g / mol) into 2 cm×2 cm pieces, which were crushed into cotton-like pieces using a high-speed wall breaker to obtain cotton linter pulp; the cotton linter pulp was added into a sodium hydroxide / urea aqueous solution, the cotton linter pulp addition amount being 2% (the percentage of the absolute dry mass of the cotton linter pulp relative to the mass of the sodium hydroxide / urea aqueous solution), and a high-speed dispersing homogenizer was used to stir at a speed of 7000 r / min for 20 min until the solution was clear and transparent and had a certain viscosity, thereby obtaining a cellulose solution.

[0049] Example 1

[0050] This embodiment provides a cuprous oxide nanoparticle functionalized cellulose hydrogel prepared by doping cuprous oxide (Cu2O) using a physical blending method, and the preparation method comprises the following steps:

[0051] (1) Prepare 80 mL of 0.05 mol / L copper sulfate dihydrate (CuSO4·2H2O) solution, add 20 mL of 2 mol / L sodium hydroxide solution dropwise, react for 2 h until blue precipitate is completely precipitated, add 0.88 g of ascorbic acid and stir for 2 h until the precipitate turns orange-yellow, centrifuge the precipitate (3500 r / min, 15 min) and wash it with deionized water 5 times until it is neutral to remove impurities remaining on the surface and inside of the precipitate, finally centrifuge the precipitate (3500 r / min, 15 min) and freeze-dry it for 2 days to obtain cuprous oxide (Cu2O) nanoparticles.

[0052] (2) Weigh 40 g of cellulose solution, add 4 mL of epichlorohydrin, and then add 0.5 g of the cuprous oxide nanoparticles prepared in step (1), stir at 30° C. for 30 min, and then place it in a 60° C. water bath and heat it for 1 h to obtain a cellulose-based cuprous oxide nanocomposite hydrogel. The nanocomposite hydrogel is soaked in deionized water and washed for 4 days, during which the water is changed every 8 h to remove impurities remaining on the surface and inside of the nanocomposite cellulose hydrogel.

[0053] Example 2

[0054] This embodiment provides a cuprous oxide nanoparticle functionalized cellulose hydrogel prepared by doping cuprous oxide nanoparticles encapsulated by tannic acid in a physical blending manner, and the preparation method comprises the following steps:

[0055] (1) 80 mL of 0.05 mol / L copper sulfate dihydrate solution was prepared, and 20 mL of 2 mol / L sodium hydroxide solution was added dropwise. After reacting for 2 h, a blue precipitate was completely precipitated, 0.2 g of tannic acid was added and stirred for 1 h. After the precipitate completely turned into dark green, 0.88 g of ascorbic acid was added and stirred for 2 h until the precipitate turned into orange-yellow. The precipitate was centrifuged (3500 r / min, 15 min) and washed with deionized water for several times until it was neutral to remove impurities remaining on the surface and inside of the precipitate. Finally, the precipitate was centrifuged (3500 r / min, 15 min) and freeze-dried for 2 days to obtain tannic acid-encapsulated cuprous oxide nanoparticles.

[0056] (2) Weigh 40 g of cellulose solution, add 4 mL of epichlorohydrin, and then add the tannic acid-encapsulated cuprous oxide nanoparticles prepared in step (1), stir at 30° C. for 30 min, and then place it in a 60° C. water bath and heat it for 1 h to obtain cuprous oxide nanoparticle-functionalized cellulose hydrogel. The cuprous oxide nanoparticle-functionalized cellulose hydrogel is soaked in deionized water and washed for 4 days, during which the water is changed every 8 h to remove impurities remaining on the surface and inside of the cuprous oxide nanoparticle-functionalized cellulose hydrogel.

[0057] Example 3

[0058] This embodiment provides a pure cellulose hydrogel, and the preparation method comprises the following steps:

[0059] Weigh 40g of cellulose solution, add 4mL of epichlorohydrin, stir at 30℃ for 30 minutes, and then heat it in a 60℃ water bath for 1h to obtain cellulose hydrogel. The hydrogel is washed in deionized water for 4 days, during which the water is changed every 8h to remove impurities remaining on the surface and inside of the cellulose hydrogel.

[0060] Example 4

[0061] This embodiment provides a cellulose / NaOH / TA / AA hydrogel without adding cuprous oxide nanoparticles, and the preparation method comprises the following steps:

[0062] (1) Weigh 40g of cellulose solution, add 4mL of epichlorohydrin, stir at 30℃ for 30min, and then place it in a 60℃ water bath and heat for 1h to obtain cellulose hydrogel. Soak the hydrogel in deionized water and wash for 4 days, changing the water every 8 hours to remove impurities remaining on the surface and inside of the cellulose hydrogel to obtain pure cellulose hydrogel. Place the washed cellulose hydrogel in a -20℃ refrigerator and freeze it for 2 days, then use a freeze dryer to dry the frozen cellulose hydrogel for 2 days to obtain a freeze-dried cellulose hydrogel.

[0063] (2) 0.2 g of freeze-dried cellulose hydrogel was immersed in 20 mL of 2 mol / L sodium hydroxide solution. After reacting for 2 h, 0.2 g of tannic acid was added and stirred for 1 h. Then, 0.88 g of ascorbic acid was added and stirred for 2 h to obtain cellulose / NaOH / TA / AA hydrogel. The cellulose / NaOH / TA / AA hydrogel was immersed in deionized water with a water change cycle of 8 h and a soaking cycle of 2 days to remove impurities remaining on the surface and inside of the cellulose / NaOH / TA / AA hydrogel.

[0064] Example 5

[0065] This embodiment provides a cuprous oxide nanoparticle functionalized cellulose hydrogel prepared by in situ synthesis, and the preparation method comprises the following steps:

[0066] (1) Weigh 40g of cellulose solution, add 4mL of epichlorohydrin, stir at 30℃ for 30 minutes, and then place it in a 60℃ water bath and heat for 1h to obtain a cellulose hydrogel. The hydrogel is soaked in deionized water and washed for 4 days, during which the water is changed every 8h to remove impurities remaining on the surface and inside of the cellulose hydrogel to obtain a pure cellulose hydrogel. The completely washed cellulose hydrogel is placed in a -20℃ refrigerator and frozen for 2 days, and then the frozen cellulose hydrogel is dried in a freezer for 2 days to obtain a freeze-dried cellulose hydrogel.

[0067] (2) 0.2 g of freeze-dried cellulose hydrogel was immersed in 80 mL of 0.05 mol / L copper sulfate dihydrate solution for 4 h. After adsorption equilibrium was reached, 20 mL of 2 mol / L sodium hydroxide solution was added dropwise. After 2 h of reaction, the color of the gel completely turned blue. 0.88 g of ascorbic acid was added and stirred for 2 h until the gel turned orange-yellow. The gel was taken out and immersed in deionized water for washing. The water was changed for 8 h and the immersion period was 2 days to remove impurities remaining on the surface and inside of the nanocomposite hydrogel, thereby obtaining the cuprous oxide nanoparticle functionalized cellulose hydrogel.

[0068] Example 6

[0069] This embodiment provides a method for preparing tannic acid-encapsulated cuprous oxide nanoparticle functionalized cellulose hydrogel by in-situ synthesis, and the preparation method comprises the following steps:

[0070] (1) Weigh 40g of cellulose solution, add 4mL of epichlorohydrin, stir at 30℃ for 30min, and then place it in a 60℃ water bath and heat for 1h to obtain cellulose hydrogel. Soak the hydrogel in deionized water and wash for 4 days, changing the water every 8h to remove impurities remaining on the surface and inside of the cellulose hydrogel to obtain pure cellulose hydrogel. Place the washed cellulose hydrogel in a -20℃ refrigerator and freeze for 2 days, then use a freeze dryer to dry the frozen cellulose hydrogel for 2 days to obtain a freeze-dried cellulose hydrogel.

[0071] (2) 0.2 g of freeze-dried cellulose hydrogel was immersed in 80 mL of 0.05 mol / L copper sulfate dihydrate solution for 4 h. After adsorption equilibrium was reached, 20 mL of 2 mol / L sodium hydroxide solution was added dropwise. After 2 h of reaction, the color of the gel completely turned blue. 0.2 g of tannic acid was added and stirred for 1 h. After the color of the gel turned into dark green, 0.88 g of ascorbic acid was added and stirred for 2 h until the gel turned orange-yellow. The gel was taken out and immersed in deionized water for washing. The water was changed for 8 hours and the immersion period was 2 days to remove impurities remaining on the surface and inside of the nanocomposite hydrogel, thereby obtaining a cellulose hydrogel functionalized with cuprous oxide nanoparticles.

[0072] SEM imaging of cuprous oxide nanoparticle-functionalized cellulose hydrogels. Figure 1 As shown, the photographs show that cuprous oxide nanoparticles with uniform size and morphology are evenly distributed in the cellulose hydrogel matrix.

[0073] Example 7

[0074] Hydrogel performance test

[0075] Mechanical strength test

[0076] The compression test was performed using a universal testing machine. Test conditions: The hydrogel was soaked in deionized water for 24 hours to allow it to absorb water and swell, and a sample with a length, width and height of 10 mm × 10 mm × 10 mm was prepared. The compression speed was 5 mm / min and the temperature was (25 ± 2) °C.

[0077] Underwater contact angle test

[0078] Using the retained drop method, a 4 μL drop of 1,2-dichloroethane oil was dropped onto the hydrogel surface with a microsyringe to form a stable oil contact angle. The underwater contact angles of the drops placed at different positions were measured using an optical contact angle analyzer.

[0079] Antibacterial performance analysis

[0080] The antibacterial activity of the hydrogel was quantitatively determined by the plate colony counting method. Escherichia coli (E. coli, ATCC 25922, provided by the Third Affiliated Hospital of Southern Medical University) was revived with beef extract peptone medium and cultured in a shaking incubator at 37°C for 24 h. The bacterial solution was transferred to a nutrient agar plate and streaked for 24 h. The activated slant E. coli strain was taken with an inoculation loop and placed in a conical flask filled with sterile water. The plate was placed on a shaker and shaken for 1 h to fully mix the bacterial suspension (the bacterial suspension concentration was 1.5×10 8 CFU / mL). Take a sterilized 250mL conical flask, add 70mL PBS buffer, 10mL Escherichia coli suspension, and 0.75g hydrogel, respectively, place it in a 37℃ constant temperature shaker for 4h, and then dilute it to 10 -7 The diluted E. coli suspension was evenly spread on the agar plate and cultured in a 37°C constant temperature incubator for 24 hours. The antibacterial efficiency was estimated by counting the number of colonies. Antibacterial efficiency = (number of blank control colonies - number of sample colonies) / number of blank control colonies * 100%.

[0081] Cytotoxicity assay

[0082] The nanocomposite hydrogel was sterilized (sterilized under UV light for 3 h, immersed in 75% ethanol for 3 h, and washed 3 times with PBS buffer). The sample was placed in a low-glucose complete DMEM medium (containing 10% fetal bovine serum and 1% penicillin / streptomycin, and a glucose content of 1000 mg / L) and placed in a cell culture incubator for 24 h. The material extract was prepared according to the national standard (ISO 10993-12:2012, IDT), where the material surface area / extraction medium = 3 cm 2 / mL.

[0083] The cytotoxicity of the nanocomposite hydrogel was detected by CCK-8 method. Mouse embryonic osteoblasts (MC3T3-E1, provided by the Third Affiliated Hospital of Southern Medical University) were used as test cells and cultured in vitro in low-glucose complete DMEM medium. The medium was renewed every two days and the culture process was carried out in a cell culture incubator (5% CO2, 37°C).

[0084] MC3T3-E1 cells in the logarithmic growth phase were digested with trypsin and plated at 1×10 5The cells were inoculated into a 96-well plate at a density of 10 cells / well and cultured in a cell culture incubator for 2 hours. After most of the cells adhered to the well plate, 500 μL of extract was added to each well, and 500 μL of low-sugar complete DMEM medium was added to the blank control. After 1 day of culture, 50 μL of CCK-8 dye (Beijing Lanjieke Technology Co., Ltd.) was added to each well under light-proof conditions and incubated for 1 hour. The optical density (OD) at 450 nm was detected with a multifunctional microplate reader, and the cell viability was calculated. (For specific experimental steps, please refer to Qiu Yuyu. Structural construction of multilayer composite wound dressing and its research on wound healing mechanism [D]. Jiangnan University, 2019.)

[0085] Table 1 Mechanical properties and antifouling performance test results of hydrogel

[0086]

[0087]

[0088] From the data in Table 1, it can be seen that the cuprous oxide nanoparticle functionalized cellulose hydrogel prepared by the present invention has strong mechanical ability, excellent antifouling property, antibacterial activity and cytotoxicity. The improvement of mechanical properties and antifouling properties mainly comes from the in-situ synthesis of cuprous oxide, the encapsulation effect of tannic acid on cuprous oxide and the bridge effect between host and guest.

[0089] The maximum compressive strength of the cellulose hydrogel prepared in Example 3 is 49.29 kPa. Example 1 shows that the loading of cuprous oxide functionalized nanoparticles by physical blending method has a significant weakening effect on the mechanical properties of cellulose hydrogel. Example 2 shows that the use of tannic acid to encapsulate cuprous oxide nanoparticles helps to improve the mechanical strength of the hydrogel, but it still cannot make up for the weakening of the mechanical properties of cellulose hydrogel by physical blending method. Example 5 shows that the in situ synthesis method has a significant enhancing effect on the mechanical properties and antibacterial properties of cellulose hydrogel functionalized with cuprous oxide nanoparticles. Example 6 shows that the use of tannic acid to encapsulate cuprous oxide nanoparticles helps to further improve the mechanical strength and antibacterial properties of cellulose hydrogel functionalized with cuprous oxide nanoparticles synthesized in situ. The synthesis principle is as follows Figure 2 As shown, cuprous oxide nanoparticles were introduced into the cellulose hydrogel network by in situ synthesis, using the hydrogel skeleton as a microreactor, the cellulose matrix as a stabilizer, and tannic acid as an auxiliary agent.

[0090] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A cuprous oxide nanoparticle functionalized cellulose hydrogel, characterized in that Prepared by the following steps: (1) Preparation of cellulose solution Dissolving sodium hydroxide and urea in water to form a sodium hydroxide / urea aqueous solution, precooling, adding cotton linter pulp to the sodium hydroxide / urea aqueous solution, and stirring to obtain a cellulose solution; (2) Preparation of cellulose hydrogel Weigh the cellulose solution prepared in step (1), add epichlorohydrin, stir, heat to obtain cellulose hydrogel, and wash; Freezing the washed cellulose hydrogel, and freeze-drying the cellulose hydrogel to obtain a dried cellulose hydrogel; (3) In situ synthesis of cuprous oxide nanoparticles functionalized cellulose hydrogel Weigh the dried cellulose hydrogel prepared in step (2), immerse it in a copper sulfate dihydrate solution, then drop a sodium hydroxide solution to react, add tannic acid and stir, then add ascorbic acid and stir, wash, and obtain the cuprous oxide nanoparticle functionalized cellulose hydrogel; The amount of sodium hydroxide added in step (1) is 5% to 10% of the total mass of the sodium hydroxide / urea aqueous solution; The amount of urea added in step (1) is 10% to 15% of the total mass of the sodium hydroxide / urea aqueous solution; The precooling in step (1) is precooling to -10 to -15°C for 10 minutes; The amount of cotton linter pulp added in step (1) is 1 to 6% of the mass of the sodium hydroxide / urea aqueous solution; The cotton linter pulp described in step (1) is obtained by crushing a cotton linter pulp board; The degree of polymerization of the cotton linter pulp described in step (1) is 600 to 700; The stirring condition in step (1) is stirring at a speed of 2000 to 8000 r / min for 10 to 40 min; The mass ratio of the epichlorohydrin volume in step (2) to the cotton linter pulp in the cellulose solution is 1-6 mL: 0.8 g; The stirring condition in step (2) is stirring at 10 to 30° C. for 10 to 30 minutes; The heating condition in step (2) is heating in a water bath at 50 to 80° C. for 30 to 120 min; The washing conditions in step (2) are as follows: soaking in deionized water for 3 to 7 days, during which the water is changed every 4 to 12 hours; The freezing condition in step (2) is freezing at -18 to -24°C for 1 to 2 days; The freeze-drying conditions in step (2) are to use a freeze dryer to dry for 2 to 4 days; The volume ratio of the mass of the cellulose hydrogel described in step (3) to the copper sulfate dihydrate solution is 0.2 g: 80 mL; The volume ratio of the sodium hydroxide solution described in step (3) to the copper sulfate dihydrate solution is 10-50 mL:80 mL; The concentration of the copper sulfate dihydrate solution described in step (3) is 0.05 mol / L; The soaking condition in step (3) is 4 to 12 hours; The concentration of the sodium hydroxide solution in step (3) is 1 to 4 mol / L; The reaction time of adding sodium hydroxide solution in step (3) is 1 to 4 hours; The mass ratio of ascorbic acid to cellulose hydrogel in step (3) is 0.88:0.2; The stirring condition of adding ascorbic acid in step (3) is stirring for 2 to 4 hours; The washing conditions in step (3) are as follows: immersion in deionized water, with a water change period of 8 hours and an immersion period of 2 days; The mass ratio of tannic acid to cellulose hydrogel in step (3) is 1:1; The stirring condition for adding tannic acid in step (3) is 1 to 4 hours.

2. Use of the cuprous oxide nanoparticle functionalized cellulose hydrogel according to claim 1 in the preparation of antifouling coatings.