High-strength steel sheet with excellent workability and method for producing the same

By optimizing the composition and heat treatment process of the steel plate, combined with the fine structure of tempered martensite, bainite, retained austenite and ferrite, the contradiction between high strength and excellent processability in the existing technology is solved, and the steel plate is achieved. High strength and excellent processing properties, suitable for automotive parts.

CN114846168BActive Publication Date: 2024-10-01POHANG IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080088482.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-18
Filing Date
2020-11-25
Publication Date
2024-10-01
Estimated Expiration
2040-11-25

AI Technical Summary

Technical Problem

It is difficult for the existing technology to produce steel plates that simultaneously meet the requirements of high strength and excellent ductility, bending workability and hole expandability, especially in automotive parts applications.

Method used

By optimizing the composition and microstructure of the steel plate, it contains a specific proportion of tempered martensite, bainite, retained austenite and ferrite, and controls its grain size and interphase hardness difference, using a specific heat treatment process to ensure The tensile strength, elongation and hole expansion rate of the steel plate reach a balance of 22000MPa% and above.

Benefits of technology

It achieves high strength and excellent ductility, bending workability and hole expandability of the steel plate. It is especially suitable for use in automotive parts and meets the needs for lightweight and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003700712480000231
    Figure BDA0003700712480000231
  • Figure BDA0003700712480000241
    Figure BDA0003700712480000241
  • Figure BDA0003700712480000251
    Figure BDA0003700712480000251
Patent Text Reader

Abstract

The present invention relates to a steel sheet which can be used for automobile parts and the like, and relates to a steel sheet which is excellent in balance between strength and ductility and balance between strength and hole expandability and excellent in bending workability, and a method for producing the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a steel sheet that can be used for automobile parts and the like, and to a steel sheet having high strength characteristics and excellent workability, and a method for manufacturing the steel sheet. Background Art

[0002] In recent years, in order to protect the global environment, the automotive industry is focusing on methods that can achieve lightweight materials while ensuring the stability of passengers. In order to meet the demand for such stability and lightweight, the application of high-strength steel plates is increasing rapidly. Generally, it is known that as the strength of a steel plate increases, the workability of the steel plate decreases. Therefore, in steel plates for automotive parts, it is necessary to have high strength characteristics and excellent workability represented by ductility, bending workability, and hole expansion.

[0003] As a technique for improving the workability of steel sheets, Patent Documents 1 and 2 disclose a method using tempered martensite. Tempered martensite, which is obtained by tempering hard martensite, is softened martensite, so there is a difference in strength between tempered martensite and existing untempered martensite (fresh martensite). Therefore, when fresh martensite is suppressed and tempered martensite is formed, workability can be increased.

[0004] However, in the techniques disclosed in Patent Documents 1 and 2, the balance between tensile strength and elongation (TS×El) cannot satisfy 22000 MPa% or more, which means that it is difficult to ensure a steel sheet excellent in both strength and ductility.

[0005] In order to obtain high strength and excellent workability characteristics of steel sheets for automobile parts, transformation induced plasticity (TRIP) steel using the transformation induced plasticity of retained austenite has been developed. Patent document 3 discloses a TRIP steel having excellent strength and workability.

[0006] Patent document 3 attempts to improve ductility and workability by including polygonal ferrite, retained austenite and martensite, but the main phase is bainite, so high strength cannot be ensured, and it is known that the balance between tensile strength and elongation (TS×El) cannot meet 22000 MPa% or more.

[0007] That is, the demand for a steel sheet having high strength and excellent workability such as ductility, bending workability, and hole expandability cannot be met at present.

[0008] (Prior art literature)

[0009] (Patent Document 1) Korean Patent Publication No. 10-2006-0118602

[0010] (Patent Document 2) Japanese Patent Publication No. 2009-019258

[0011] (Patent Document 3) Korean Patent Publication No. 10-2014-0012167 Summary of the invention

[0012] Technical Problems to be Solved by the Invention

[0013] According to one aspect of the present invention, a high-strength steel sheet having excellent ductility, bending workability, and hole expandability by optimizing the composition and microstructure of the steel sheet and a method for manufacturing the same can be provided.

[0014] The technical problems of the present invention are not limited to the above contents. Additional technical problems of the present invention are described in the entire specification, and those skilled in the art can easily understand the additional technical problems of the present invention from the contents described in the specification of the present invention.

[0015] Technical means to solve technical problems

[0016] According to one aspect of the present invention, a high-strength steel sheet with excellent workability may contain, in terms of weight%, C: 0.25-0.75%, Si: 4.0% or less, Mn: 0.9-5.0%, Al: 5.0% or less, P: 0.15% or less, S: 0.03% or less, N: 0.03% or less, the remainder of Fe and inevitable impurities, and the fine structure may contain 30-70 volume % of tempered martensite, 10-45 volume % of bainite, 10-40 volume % of retained austenite, 3-20 volume % of ferrite and inevitable structures, and may satisfy the following [Relationship 1] and [Relationship 2].

[0017] [Equation 1]

[0018] 1.1≤[Si+Al] F / [Si+Al] γ ≤3.0

[0019] In the above relational formula 1, [Si+Al] F is the average total content of Si and Al contained in ferrite (weight %), [Si+Al] γ is the average total content (weight %) of Si and Al contained in retained austenite.

[0020] [Equation 2]

[0021] V(1.2μm,γ) / V(γ)≥0.1

[0022] In the above relational expression 2, V(1.2 μm, γ) is the fraction (volume %) of retained austenite having an average grain size of 1.2 μm or more, and V(γ) is the fraction (volume %) of retained austenite in the steel sheet.

[0023] The steel plate may further include any one or more of the following (1) to (9).

[0024] (1) one or more of Ti: 0-0.5%, Nb: 0-0.5% and V: 0-0.5%,

[0025] (2) one or more of Cr: 0-3.0% and Mo: 0-3.0%,

[0026] (3) Cu: 0-4.5% and Ni: 0-4.5% or more,

[0027] (4) B: 0-0.005%,

[0028] (5) one or more of Ca: 0-0.05%, REM excluding Y: 0-0.05% and Mg: 0-0.05%,

[0029] (6) one or more of W: 0-0.5% and Zr: 0-0.5%,

[0030] (7) one or more of Sb: 0-0.5% and Sn: 0-0.5%,

[0031] (8) one or more of Y: 0-0.2% and Hf: 0-0.2%,

[0032] (9) Co: 0-1.5%.

[0033] The total content of the Si and the Al (Si+Al) may be 1.0-6.0 wt %.

[0034] The steel plate may satisfy the following [Relationship 3].

[0035] [Equation 3]

[0036] V(lath,γ) / V(γ)≥0.5

[0037] In the above relational expression 3, V(lath, γ) is the fraction (volume %) of lath-shaped retained austenite, and V(γ) is the fraction (volume %) of retained austenite in the steel sheet.

[0038] The balance between tensile strength and elongation of the steel plate is expressed by the following [Relationship 4] (B T·E ) can be 22000 (MPa%) or more, and the balance between tensile strength and hole expansion ratio (B T·H) can be 7*10 6 (MPa 2 % 1 / 2 ) above, the bending processing rate (B R ) can satisfy the range of 0.5 to 3.0.

[0039] [Equation 4]

[0040] B T·E =[Tensile strength (TS, MPa)]*[Elongation (El, %)]

[0041] [Equation 5]

[0042] B T·H =[Tensile strength (TS, MPa)] 2 *[Hole expansion ratio (HER, %)] 1 / 2

[0043] [Equation 6]

[0044] B R =R / t

[0045] In the above relational expression 6, R represents the minimum bending radius (mm) at which no cracks are generated after a 90° bending test, and t represents the thickness (mm) of the steel plate.

[0046] According to another aspect of the present invention, a method for manufacturing a high-strength steel sheet with excellent workability may include the following steps: providing a cold-rolled steel sheet, wherein the cold-rolled steel sheet contains, in weight %, C: 0.25-0.75%, Si: 4.0% or less, Mn: 0.9-5.0%, Al: 5.0% or less, P: 0.15% or less, S: 0.03% or less, N: 0.03% or less, and the balance of Fe and inevitable impurities; heating the cold-rolled steel sheet to a temperature range of Ac1 or more and less than Ac3 at an average heating rate of 5°C / second or more (primary heating), and maintaining the temperature for more than 50 seconds (primary maintaining); cooling the cold-rolled steel sheet to a temperature range of 600-850°C at an average cooling rate of 1°C / second or more (primary cooling); The temperature range of the present invention is as follows: the temperature range of 0°C (first cooling termination temperature); cooling to a temperature range of 300-500°C at an average cooling rate of more than 2°C / second (second cooling), and maintaining within the temperature range for more than 5 seconds (second holding); cooling to a temperature range of 100-300°C (second cooling termination temperature) at an average cooling rate of more than 2°C / second (third cooling); heating to a temperature range of 350-550°C (second heating), and maintaining within the temperature range for more than 10 seconds (third holding); cooling to a temperature range of 250-450°C (fourth cooling) at an average cooling rate of more than 1°C / second, and maintaining within the temperature range for more than 10 seconds (fourth holding); and cooling to room temperature (fifth cooling).

[0047] The cold-rolled steel sheet may further contain any one or more of the following (1) to (9).

[0048] (1) One or more of Ti: 0 - 0.5%, Nb: 0 - 0.5% and V: 0 - 0.5%,

[0049] (2) One or more of Cr: 0 - 3.0% and Mo: 0 - 3.0%,

[0050] (3) One or more of Cu: 0 - 4.5% and Ni: 0 - 4.5%,

[0051] (4) B: 0 - 0.005%,

[0052] (5) One or more of Ca: 0 - 0.05%, REM except Y: 0 - 0.05% and Mg: 0 - 0.05%,

[0053] (6) One or more of W: 0 - 0.5% and Zr: 0 - 0.5%,

[0054] (7) One or more of Sb: 0 - 0.5% and Sn: 0 - 0.5%,

[0055] (8) One or more of Y: 0 - 0.2% and Hf: 0 - 0.2%,

[0056] (9) Co: 0 - 1.5%.

[0057] The total content (Si + Al) of the Si and the Al contained in the cold-rolled steel sheet may be 1.0 - 6.0% by weight.

[0058] The cold-rolled steel sheet may be provided by the following steps: heating a steel billet to 1000 - 1350 °C; performing hot finish rolling in a temperature range of 800 - 1000 °C; coiling the hot-rolled steel sheet in a temperature range of 300 - 600 °C; performing hot rolling annealing treatment on the coiled steel sheet for 600 - 1700 seconds in a temperature range of 650 - 850 °C; and performing cold rolling on the steel sheet subjected to hot rolling annealing treatment at a reduction rate of 30 - 90%.

[0059] The cooling rate (Vc1) of the primary cooling and the cooling rate (Vc2) of the secondary cooling may satisfy the relationship of Vc1 < Vc2.

[0060] Advantages of the Invention

[0061] According to a preferred aspect of the present invention, a steel sheet can be provided which has excellent strength and excellent workability such as ductility, bending workability, and hole expandability, and is particularly suitable for use as a steel sheet for automobile parts.

[0062] Best Mode for Carrying Out the Invention

[0063] The present invention relates to a high-strength steel plate with excellent workability and a method for manufacturing the same. The preferred specific embodiments of the present invention are described below. The specific embodiments of the present invention can be modified into various forms, and it should not be interpreted that the scope of the present invention is limited to the specific embodiments described below. This specific embodiment is provided to explain the present invention in more detail to those skilled in the art.

[0064] The inventors of the present invention have recognized that in a transformation induced plasticity (TRIP) steel containing bainite, tempered martensite, retained austenite and ferrite, when the retained austenite is stabilized and the ratio of specific components contained in the retained austenite and ferrite is controlled within a certain range, the hardness difference between the retained austenite and the ferrite is reduced, thereby ensuring the workability and strength of the steel sheet at the same time. By finding this out, a method for improving the ductility and workability of high-strength steel has been developed, thereby completing the present invention.

[0065] Hereinafter, a high-strength steel sheet having excellent workability according to one aspect of the present invention will be described in detail.

[0066] According to one aspect of the present invention, a high-strength steel sheet with excellent workability may contain, in weight %, C: 0.25-0.75%, Si: 4.0% or less, Mn: 0.9-5.0%, Al: 5.0% or less, P: 0.15% or less, S: 0.03% or less, N: 0.03% or less, the remainder of Fe and inevitable impurities, and the fine structure may contain 30-70 volume % of tempered martensite, 10-45 volume % of bainite, 10-40 volume % of retained austenite, 3-20 volume % of ferrite and inevitable structures, and may satisfy the following [Relationship 1] and [Relationship 2].

[0067] [Equation 1]

[0068] 1.1≤[Si+Al] F / [Si+Al] γ ≤3.0

[0069] In the above relational formula 1, [Si+Al] F is the average total content of Si and Al contained in ferrite (weight %), [Si+Al] γ is the average total content (weight %) of Si and Al contained in retained austenite.

[0070] [Equation 2]

[0071] V(1.2μm,γ) / V(γ)≥0.1

[0072] In the above relational expression 2, V(1.2 μm, γ) is the fraction (volume %) of retained austenite having an average grain size of 1.2 μm or more, and V(γ) is the fraction (volume %) of retained austenite in the steel sheet.

[0073] The steel composition of the present invention will be described in more detail below. Unless otherwise specified, the percentages indicating the content of each element are based on weight.

[0074] According to one aspect of the present invention, a high-strength steel sheet with excellent workability contains, in weight %, C: 0.25-0.75%, Si: 4.0% or less, Mn: 0.9-5.0%, Al: 5.0% or less, P: 0.15% or less, S: 0.03% or less, N: 0.03% or less, and the balance Fe and inevitable impurities. In addition, the steel plate may further include: Ti: 0.5% or less (including 0%), Nb: 0.5% or less (including 0%), V: 0.5% or less (including 0%), Cr: 3.0% or less (including 0%), Mo: 3.0% or less (including 0%), Cu: 4.5% or less (including 0%), Ni: 4.5% or less (including 0%), B: 0.005% or less (including 0%), Ca: 0.05% or less (including 0%), REM excluding Y: 0.05% or less (including 0%), Mg: 0.05% or less (including 0%), W: 0.5% or less (including 0%), Zr: 0.5% or less (including 0%), Sb: 0.5% or less (including 0%), Sn: 0.5% or less (including 0%), Y: 0.2% or less (including 0%), Hf: 0.2% or less (including 0%), Co: 1.5% or less (including 0%). Furthermore, the total content of Si and Al (Si+Al) may be 1.0-6.0%.

[0075] Carbon (C): 0.25-0.75%

[0076] Carbon (C) is an element indispensable for ensuring the strength of the steel sheet, and is an element that stabilizes the retained austenite that helps to improve the ductility of the steel sheet. Therefore, in order to achieve the effects described above, the present invention may contain more than 0.25% carbon (C). The preferred carbon (C) content may exceed 0.25%, and may be more than 0.27% and more than 0.30%. A more preferred carbon (C) content may be more than 0.31%. On the other hand, when the carbon (C) content exceeds a certain level, it may be difficult to perform cold rolling due to excessive increase in strength. Therefore, the upper limit of the carbon (C) content may be limited to 0.75% in the present invention. The carbon (C) content may be less than 0.70%, and a more preferred carbon (C) content may be less than 0.67%.

[0077] Silicon (Si): 4.0% or less (except 0%)

[0078] Silicon (Si) is an element that helps to improve strength by solid solution strengthening, and is also an element that improves processability by strengthening ferrite and homogenizing the organization. In addition, silicon (Si) is an element that helps the formation of retained austenite by suppressing the precipitation of cementite. Therefore, in order to achieve the effect as described above, silicon (Si) must be added in the present invention. The preferred silicon (Si) content can be more than 0.02%, and the more preferred silicon (Si) content can be more than 0.05%. However, when the silicon (Si) content exceeds a certain level, plating defect problems such as unplated are caused in the plating process, and the weldability of the steel sheet may be reduced, so the upper limit of the silicon (Si) content can be limited to 4.0% in the present invention. The upper limit of the preferred silicon (Si) content can be 3.8%, and the more preferred upper limit of the silicon (Si) content can be 3.5%.

[0079] Aluminum (Al): 5.0% or less (except 0%)

[0080] Aluminum (Al) is an element that acts as a deoxidizer by combining with oxygen in steel. In addition, like silicon (Si), aluminum (Al) is an element that stabilizes residual austenite by inhibiting the precipitation of cementite. Therefore, in order to achieve the above-mentioned effect, aluminum (Al) must be added in the present invention. The preferred aluminum (Al) content can be more than 0.05%, and the more preferred aluminum (Al) content can be more than 0.1%. On the other hand, when too much aluminum (Al) is added, the inclusions of the steel plate increase and the processability of the steel plate may be reduced, so the upper limit of the aluminum (Al) content can be limited to 5.0% in the present invention. The preferred upper limit of the aluminum (Al) content can be 4.75%, and the more preferred upper limit of the aluminum (Al) content can be 4.5%.

[0081] In addition, the total content (Si+Al) of silicon (Si) and aluminum (Al) is preferably 1.0-6.0%. Silicon (Si) and aluminum (Al) are components that affect the formation of microstructures and thus affect ductility, bending workability and hole expansion in the present invention, so the total content of silicon (Si) and aluminum (Al) is preferably 1.0-6.0%. More preferably, the total content (Si+Al) of silicon (Si) and aluminum (Al) can be 1.5% or more and 4.0% or less.

[0082] Manganese (Mn): 0.9-5.0%

[0083] Manganese (Mn) is a useful element for improving both strength and ductility. Therefore, in order to achieve the above-mentioned effect, the lower limit of the manganese (Mn) content can be limited to 0.9% in the present invention. The lower limit of the preferred manganese (Mn) content can be 1.0%, and the lower limit of the more preferred manganese (Mn) content can be 1.1%. On the other hand, when too much manganese (Mn) is added, the enrichment of carbon (C) in austenite is insufficient due to the increase in bainite transformation time, so there is a problem that the desired austenite fraction cannot be ensured. Therefore, the upper limit of the manganese (Mn) content can be limited to 5.0% in the present invention. The upper limit of the preferred manganese (Mn) content can be 4.7%, and the more preferred upper limit of the manganese (Mn) content can be 4.5%.

[0084] Phosphorus (P): 0.15% or less (including 0%)

[0085] Phosphorus (P) is an element contained as an impurity and deteriorates impact toughness. Therefore, the content of phosphorus (P) is preferably controlled to 0.15% or less.

[0086] Sulfur (S): 0.03% or less (including 0%)

[0087] Sulfur (S) is contained as an impurity and is an element that forms MnS in the steel sheet and deteriorates ductility. Therefore, the content of sulfur (S) is preferably 0.03% or less.

[0088] Nitrogen (N): 0.03% or less (including 0%)

[0089] Nitrogen (N) is contained as an impurity and forms nitrides during continuous casting to cause cracks in the slab. Therefore, the nitrogen (N) content is preferably 0.03% or less.

[0090] In addition, the steel sheet of the present invention may further contain alloy compositions in addition to the above-mentioned alloy components, which will be described in detail below.

[0091] Titanium (Ti): 0-0.5%, niobium (Nb): 0-0.5% and vanadium (V): 0-0.5% or more

[0092] Titanium (Ti), niobium (Nb) and vanadium (V) are elements that refine the crystal grains by forming precipitates, and are also elements that contribute to improving the strength and impact toughness of the steel sheet. Therefore, in order to achieve the above-mentioned effects, one or more of titanium (Ti), niobium (Nb) and vanadium (V) may be added in the present invention. However, when the content of each of titanium (Ti), niobium (Nb) and vanadium (V) exceeds a certain level, too many precipitates are formed, thereby reducing the impact toughness and causing an increase in manufacturing costs. Therefore, in the present invention, the content of titanium (Ti), niobium (Nb) and vanadium (V) may be limited to 0.5% or less.

[0093] Chromium (Cr): 0-3.0% and molybdenum (Mo): 0-3.0% or more

[0094] Chromium (Cr) and molybdenum (Mo) inhibit the decomposition of austenite during alloying treatment, and like manganese (Mn), chromium (Cr) and molybdenum (Mo) are elements that stabilize austenite. Therefore, in order to achieve the above-mentioned effects, one or more of chromium (Cr) and molybdenum (Mo) may be added in the present invention. However, when the content of chromium (Cr) and molybdenum (Mo) exceeds a certain level, the enrichment of carbon (C) in austenite is insufficient due to the increase in bainite transformation time, and thus the desired residual austenite fraction cannot be ensured. Therefore, in the present invention, the content of chromium (Cr) and molybdenum (Mo) may be limited to 3.0% or less, respectively.

[0095] Copper (Cu): 0-4.5% and nickel (Ni): 0-4.5% or more

[0096] Copper (Cu) and nickel (Ni) are elements that stabilize austenite and inhibit corrosion. In addition, copper (Cu) and nickel (Ni) are elements that are enriched on the surface of the steel plate and prevent the intrusion of hydrogen that migrates into the steel plate, thereby inhibiting hydrogen-induced delayed fracture. Therefore, in order to achieve the above-mentioned effects, one or more of copper (Cu) and nickel (Ni) can be added in the present invention. However, when the content of copper (Cu) and nickel (Ni) exceeds a certain level, it leads to excessive characteristic effects and becomes a cause of increased manufacturing costs. Therefore, in the present invention, the content of copper (Cu) and nickel (Ni) can be limited to less than 4.5%, respectively.

[0097] Boron (B): 0-0.005%

[0098] Boron (B) is an element that improves strength by improving hardenability, and is also an element that inhibits nucleation of grain boundaries. Therefore, in order to achieve the above-mentioned effects, boron (B) can be added in the present invention. However, when the content of boron (B) exceeds a certain level, it leads to excessive characteristic effects and becomes a cause of increased manufacturing costs, so the content of boron (B) can be limited to less than 0.005% in the present invention.

[0099] Calcium (Ca): 0-0.05%, magnesium (Mg): 0-0.05% and rare earth elements (REM) other than yttrium (Y): 0-0.05% or more

[0100] Here, rare earth elements (REM) refer to scandium (Sc), yttrium (Y) and lanthanoids. Rare earth elements (REM) other than calcium (Ca), magnesium (Mg) and yttrium (Y) are elements that contribute to improving the ductility of the steel sheet by spheroidizing sulfides. Therefore, in order to achieve the above-mentioned effects, one or more rare earth elements (REM) other than calcium (Ca), magnesium (Mg) and yttrium (Y) may be added in the present invention. However, when the content of rare earth elements (REM) other than calcium (Ca), magnesium (Mg) and yttrium (Y) exceeds a certain level, it leads to excessive characteristic effects and becomes a cause of increased manufacturing costs. Therefore, in the present invention, the content of rare earth elements (REM) other than calcium (Ca), magnesium (Mg) and yttrium (Y) may be limited to 0.05% or less, respectively.

[0101] Tungsten (W): 0-0.5% and zirconium (Zr): 0-0.5% or more

[0102] Tungsten (W) and zirconium (Zr) are elements that increase the strength of the steel sheet by improving hardenability, so in order to achieve the above-mentioned effects, one or more of tungsten (W) and zirconium (Zr) may be added in the present invention. However, when the content of tungsten (W) and zirconium (Zr) exceeds a certain level, it leads to excessive characteristic effects and becomes a cause of increased manufacturing costs, so in the present invention, the content of tungsten (W) and zirconium (Zr) may be limited to less than 0.5%, respectively.

[0103] Antimony (Sb): 0-0.5% and tin (Sn): 0-0.5% or more

[0104] Antimony (Sb) and tin (Sn) are elements that improve the plating wettability and plating adhesion of the steel sheet. Therefore, in order to achieve the above-mentioned effects, one or more of antimony (Sb) and tin (Sn) may be added in the present invention. However, when the content of antimony (Sb) and tin (Sn) exceeds a certain level, the brittleness of the steel sheet increases, and cracks may be generated during hot working or cold working. Therefore, in the present invention, the content of antimony (Sb) and tin (Sn) can be limited to less than 0.5%, respectively.

[0105] One or more of yttrium (Y): 0-0.2% and hafnium (Hf): 0-0.2%

[0106] Yttrium (Y) and hafnium (Hf) are elements that improve the corrosion resistance of steel sheets. Therefore, in order to achieve the above-mentioned effects, one or more of yttrium (Y) and hafnium (Hf) may be added in the present invention. However, when the content of yttrium (Y) and hafnium (Hf) exceeds a certain level, the ductility of the steel sheet may deteriorate. Therefore, in the present invention, the content of yttrium (Y) and hafnium (Hf) may be limited to 0.2% or less, respectively.

[0107] Cobalt (Co): 0-1.5%

[0108] Cobalt (Co) is an element that increases the TRIP effect by promoting bainite transformation, and therefore, in the present invention, cobalt (Co) may be added for the above-mentioned effect. However, when the content of cobalt (Co) exceeds a certain level, the weldability and ductility of the steel sheet may deteriorate, and therefore, in the present invention, the content of cobalt (Co) may be limited to 1.5% or less.

[0109] The high-strength steel sheet with excellent workability according to one aspect of the present invention may contain a balance of Fe and other inevitable impurities in addition to the above-mentioned components. However, in the usual manufacturing process, unnecessary impurities are inevitably mixed from the raw materials or the surrounding environment, so these impurities cannot be completely excluded. These impurities are well known to those skilled in the art, so all of them are not particularly mentioned in this specification. In addition, the further addition of effective components other than the above-mentioned components is not completely excluded.

[0110] According to one aspect of the present invention, a high-strength steel sheet with excellent workability may contain tempered martensite, bainite, retained austenite and ferrite as fine structures. As a preferred example, in terms of volume fraction, a high-strength steel sheet with excellent workability according to one aspect of the present invention may contain 30-70% tempered martensite, 10-45% bainite, 10-40% retained austenite, 3-20% ferrite and inevitable structures. The inevitable structures of the present invention may include fresh martensite, pearlite, island martensite (Martensite Austenite Constituent, MA), etc. When too much fresh martensite or pearlite is formed, the workability of the steel sheet may be reduced, or the fraction of retained austenite may be reduced.

[0111] In a high-strength steel sheet with excellent workability according to one aspect of the present invention, as shown in the following [Relationship 1], the average total content of silicon (Si) and aluminum (Al) contained in ferrite ([Si+Al] F , weight %) and the average total content of silicon (Si) and aluminum (Al) contained in the retained austenite ([Si+Al] γ, weight %) satisfies the range of 1.1-3.0. As shown in the following [Relationship 2], the ratio of the fraction of retained austenite with an average grain size of 1.2 μm or more (V(1.2 μm, γ), volume %) to the fraction of retained austenite in the steel plate (V(γ), volume %) can be greater than 0.1.

[0112] [Equation 1]

[0113] 1.1≤[Si+Al] F / [Si+Al] γ ≤3.0

[0114] [Equation 2]

[0115] V(1.2μm,γ) / V(γ)≥0.1

[0116] In addition, in a high-strength steel sheet with excellent workability according to one aspect of the present invention, as shown in the following [Relationship 3], the ratio of the fraction of lath-shaped retained austenite (V (lath, γ), volume %) to the fraction of retained austenite of the steel sheet (V (γ), volume %) can be 0.5 or more.

[0117] [Equation 3]

[0118] V(lath,γ) / V(γ)≥0.5

[0119] In the high-strength steel sheet with excellent workability according to one aspect of the present invention, the balance between tensile strength and elongation (B T·E ) is 22000 (MPa%) or more, and the balance between tensile strength and hole expansion ratio (B T·H ) is 7*10 6 (MPa 2 % 1 / 2 ) above, the bending processing rate (B R ) satisfies the range of 0.5 to 3.0, and thus the steel plate can have an excellent balance between strength and ductility and a balance between strength and hole expansion ratio, and can also have excellent bending workability.

[0120] [Equation 4]

[0121] B T·E =[Tensile strength (TS, MPa)]*[Elongation (El, %)]

[0122] [Equation 5]

[0123] B T·H =[Tensile strength (TS, MPa)] 2 *[Hole expansion ratio (HER, %)] 1 / 2

[0124] [Equation 6]

[0125] B R =R / t

[0126] In the above relational expression 6, R represents the minimum bending radius (mm) at which no cracks are generated after a 90° bending test, and t represents the thickness (mm) of the steel plate.

[0127] The purpose of the present invention is to ensure high strength properties, excellent ductility and bendability at the same time, so it is important to stabilize the retained austenite of the steel plate. In order to stabilize the retained austenite, it is necessary to enrich the carbon (C) and manganese (Mn) in the ferrite, bainite and tempered martensite of the steel plate in the austenite. However, when the carbon (C) is enriched in the austenite by using ferrite, due to the low strength characteristics of ferrite, the strength of the steel plate may be insufficient, and excessive phase hardness difference may be generated, which may reduce the hole expansion ratio (HER). Therefore, the present invention uses bainite and tempered martensite to enrich carbon (C) and manganese (Mn) in austenite.

[0128] When the content of silicon (Si) and aluminum (Al) in the retained austenite is limited within a certain range, a large amount of carbon (C) and manganese (Mn) can be enriched in the retained austenite from bainite and tempered martensite, so the retained austenite can be effectively stabilized. In addition, as the content of silicon (Si) and aluminum (Al) in austenite is limited within a certain range, the content of silicon (Si) and aluminum (Al) in ferrite can be increased. As the content of silicon (Si) and aluminum (Al) in ferrite increases, the hardness of ferrite increases, and the interphase hardness difference between ferrite as a soft structure and tempered martensite, bainite and retained austenite as hard structures can be effectively reduced.

[0129] Therefore, the present invention uses the average total content of silicon (Si) and aluminum (Al) contained in ferrite ([Si+Al] F , weight %) and the average total content of silicon (Si) and aluminum (Al) contained in the retained austenite ([Si+Al] γ , weight %) is limited to 1.1 or more, so the hardness difference between the soft structure and the hard structure can be effectively reduced. On the other hand, when the content of silicon (Si) and aluminum (Al) in ferrite is too high, the ferrite is over-hardened, and the workability is reduced. Therefore, it may not be possible to ensure the desired balance between tensile strength and elongation (TS×El) and the balance between tensile strength and hole expansion rate (TS 2 ×HER 1 / 2 ) and bending processing rate (R / t). Therefore, in the present invention, the average total content of silicon (Si) and aluminum (Al) contained in ferrite ([Si+Al] F, weight %) and the average total content of silicon (Si) and aluminum (Al) contained in the retained austenite ([Si+Al] γ , weight %) ratio is limited to 3.0 or less.

[0130] The retained austenite having an average grain size of 1.2 μm or more is heat-treated at a bainite-forming temperature so that the average grain size thereof increases, thereby suppressing transformation of austenite into martensite, and thus the workability of the steel sheet can be improved.

[0131] In addition, the lath-shaped retained austenite in the retained austenite affects the workability of the steel sheet. The retained austenite is divided into lath-shaped retained austenite formed between bainite phases and block-shaped retained austenite formed in the portion without bainite phase. The block-shaped retained austenite is further transformed into bainite during the heat treatment process, and the lath-shaped retained austenite increases, which can effectively improve the workability of the steel sheet.

[0132] Therefore, in order to improve the ductility and workability of the steel sheet, it is preferable to increase the fraction of retained austenite having an average grain size of 1.2 μm or more and the fraction of lath-shaped retained austenite in the retained austenite.

[0133] In a high-strength steel sheet having excellent workability according to one aspect of the present invention, the ratio of the fraction of retained austenite having an average grain size of 1.2 μm or more (V(1.2 μm, γ), volume %) to the fraction of retained austenite of the steel sheet (V(γ), volume %) can be limited to 0.1 or more, and the ratio of the fraction of lath-shaped retained austenite (V(lath, γ), volume %) to the fraction of retained austenite of the steel sheet (V(γ), volume %) can be limited to 0.5 or more. When the ratio of the fraction of retained austenite having an average grain size of 1.2 μm or more (V (1.2 μm, γ), volume %) to the fraction of retained austenite in the steel sheet (V (γ), volume %) is less than 0.1, or the ratio of the fraction of lath-shaped retained austenite (V (lath, γ), volume %) to the fraction of retained austenite in the steel sheet (V (γ), volume %) is less than 0.5, the bending working ratio (R / t) cannot satisfy 0.5 to 3.0, and therefore there is a problem in that the desired workability cannot be ensured.

[0134] Due to the transformation induced plasticity generated when austenite is transformed into martensite during processing, the steel sheet containing retained austenite has excellent ductility and bending workability. When the fraction of retained austenite is lower than a certain level, the balance of tensile strength and elongation (TS×El) is less than 22000MPa%, or the bending work rate (R / t) may exceed 3.0. In addition, when the fraction of retained austenite exceeds a certain level, the local elongation (Local Elongation) may decrease. Therefore, in the present invention, in order to obtain a steel sheet with excellent balance of tensile strength and elongation (TS×El) and bending work rate (R / t), the fraction of retained austenite can be limited to the range of 10-40 volume %.

[0135] In addition, both untempered martensite (fresh martensite) and tempered martensite are fine structures that improve the strength of the steel plate. However, compared with tempered martensite, fresh martensite has the characteristic of greatly reducing the ductility and hole expandability of the steel plate. This is because the fine structure of tempered martensite is softened by the tempering heat treatment. Therefore, in the present invention, in order to provide a steel plate with a balance between strength and ductility, a balance between strength and hole expandability, and excellent bending workability, it is preferred to use tempered martensite. When the fraction of tempered martensite is lower than a certain level, it is difficult to ensure a balance between tensile strength and elongation (TS×El) of 22000MPa% or more or 7*10 6 (MPa 2 % 1 / 2 ) above the balance of tensile strength and hole expansion rate (TS 2 ×HER 1 / 2 ), when the fraction of tempered martensite exceeds a certain level, ductility and workability decrease, so the balance of tensile strength and elongation (TS×El) is less than 22000MPa%, or the bending working ratio (R / t) exceeds 3.0, which is not preferred. Therefore, in the present invention, in order to obtain the balance of tensile strength and elongation (TS×El), the balance of tensile strength and hole expansion ratio (TS 2 ×HER 1 / 2 ) and a steel sheet with excellent bending working ratio (R / t), the fraction of tempered martensite can be limited to the range of 30-70 volume %.

[0136] In order to improve the balance between tensile strength and elongation (TS×El), the balance between tensile strength and hole expansion rate (TS 2 ×HER 1 / 2 ) and bending working ratio (R / t), the microstructure preferably contains bainite appropriately. Only when the bainite fraction is above a certain level, the balance of tensile strength and elongation (TS×El) of 22000MPa% and 7*10 6 (MPa 2 % 1 / 2) above the balance of tensile strength and hole expansion rate (TS 2 ×HER 1 / 2 ) and a bending working ratio (R / t) of 0.5 to 3.0. On the other hand, when the fraction of bainite is too large, the fraction of tempered martensite is inevitably reduced, so that the balance between tensile strength and elongation (TS×El) and the balance between tensile strength and hole expansion ratio (TS 2 ×HER 1 / 2 ) and bending working ratio (R / t). Therefore, in the present invention, the fraction of bainite can be limited to the range of 10-45 volume %.

[0137] Ferrite is an element that contributes to improving ductility. Therefore, only when the ferrite fraction is above a certain level, the balance between tensile strength and elongation (TS×El) desired in the present invention can be ensured. However, when the ferrite fraction is too large, the hardness difference between the phases increases, and the hole expansion ratio (HER) may decrease, so that the balance between tensile strength and hole expansion ratio (TS×El) desired in the present invention cannot be ensured. 2 ×HER 1 / 2 ). Therefore, in the present invention, the fraction of ferrite can be limited to the range of 3-20 volume %.

[0138] Hereinafter, an example of a method for producing the steel sheet of the present invention will be described in detail.

[0139] According to one aspect of the present invention, a method for manufacturing a high-strength steel sheet with excellent workability may include the following steps: providing a cold-rolled steel sheet having a specified composition; heating the cold-rolled steel sheet to a temperature range of Ac1 or higher and lower than Ac3 at an average heating rate of 5°C / second or higher (primary heating), and maintaining the temperature for more than 50 seconds (primary maintaining); cooling the cold-rolled steel sheet to a temperature range of 600-850°C (primary cooling termination temperature) at an average cooling rate of 1°C / second or higher (primary cooling); cooling the cold-rolled steel sheet to a temperature range of 300-500°C at an average cooling rate of 2°C / second or higher; The invention relates to the following steps: the first step is to cool the steel sheet to a temperature range of 100-300°C (secondary cooling) and keep it in the temperature range for more than 5 seconds (secondary holding); the second step is to cool the steel sheet to a temperature range of 350-550°C (secondary heating) and keep it in the temperature range for more than 10 seconds (third holding); the second step is to cool the steel sheet to a temperature range of 250-450°C (fourth cooling) and keep it in the temperature range for more than 10 seconds (fourth holding); and the third step is to cool the steel sheet to room temperature (fifth cooling).

[0140] In addition, the cold-rolled steel sheet of the present invention can be provided by the following steps: heating the steel billet to 1000-1350°C; performing hot finish rolling in the temperature range of 800-1000°C; coiling the hot-rolled steel sheet in the temperature range of 300-600°C; performing hot rolling annealing heat treatment on the coiled steel sheet for 600-1700 seconds in the temperature range of 650-850°C; and cold rolling the hot-rolled annealing heat treated steel sheet at a reduction rate of 30-90%.

[0141] Billet preparation and heating

[0142] A steel slab having a predetermined composition is prepared. The steel slab of the present invention has an alloy composition corresponding to the alloy composition of the steel plate described above, and therefore the alloy composition of the steel slab will be described in place of the alloy composition of the steel slab.

[0143] The prepared steel billet may be heated to a certain temperature range, and the heating temperature of the steel billet may be in the range of 1000-1350° C. This is because when the heating temperature of the steel billet is lower than 1000° C., hot rolling may be performed in a temperature range below the desired hot finishing rolling temperature range, and when the heating temperature of the steel billet exceeds 1350° C., the steel may reach the melting point and melt.

[0144] Hot rolling and coiling

[0145] The heated steel slab can be hot rolled to provide a hot rolled steel sheet. The hot finishing rolling temperature during hot rolling is preferably in the range of 800-1000°C. This is because when the hot finishing rolling temperature is lower than 800°C, excessive rolling load may become a problem, and when the hot finishing rolling temperature exceeds 1000°C, coarse grains of the hot rolled steel sheet are formed, which may cause a decrease in the physical properties of the final steel sheet.

[0146] The hot-rolled steel sheet that has completed hot rolling can be cooled at an average cooling rate of 10° C. / second or more, and can be coiled at a temperature of 300-600° C. This is because when the coiling temperature is lower than 300° C., it is not easy to coil, and when the coiling temperature exceeds 600° C., surface scale is formed inside the hot-rolled steel sheet, so it may be difficult to perform pickling.

[0147] Hot rolling annealing heat treatment

[0148] In order to facilitate pickling and cold rolling as subsequent processes after coiling, it is preferred to perform a hot rolling annealing heat treatment process. The hot rolling annealing heat treatment can be performed in a temperature range of 650-850°C for 600-1700 seconds. When the hot rolling annealing heat treatment temperature is lower than 650°C or the hot rolling annealing heat treatment time is less than 600 seconds, the strength of the steel plate treated by hot rolling annealing is high, so it may not be easy to perform subsequent cold rolling. On the other hand, when the hot rolling annealing heat treatment temperature exceeds 850°C or the hot rolling annealing heat treatment time exceeds 1700 seconds, pickling may not be easy due to the oxide scale formed deep inside the steel plate.

[0149] Pickling and cold rolling

[0150] After the hot rolling annealing heat treatment, pickling may be performed to remove the oxide scale formed on the surface of the steel sheet, and cold rolling may be performed. In the present invention, there is no particular restriction on the pickling and cold rolling conditions, but cold rolling is preferably performed at a cumulative reduction rate of 30-90%. When the cumulative reduction rate of cold rolling exceeds 90%, it may be difficult to perform cold rolling in a short time due to the high strength of the steel sheet.

[0151] The cold rolled steel sheet can be subjected to an annealing heat treatment process to be made into an uncoated cold rolled steel sheet, or can be subjected to a plating process to be made into a plated steel sheet in order to impart corrosion resistance. The plating can be applied by a plating method such as hot dip galvanizing, electro galvanizing, hot dip aluminum plating, etc., and the method and type are not particularly limited.

[0152] Annealing heat treatment

[0153] In the present invention, in order to simultaneously ensure the strength and workability of the steel sheet, an annealing heat treatment process is performed.

[0154] The cold rolled steel sheet is heated to a temperature range of Ac1 or higher and lower than Ac3 (two-phase region) (primary heating), and maintained in the temperature range for more than 50 seconds (primary holding). When the primary heating or primary holding temperature is Ac3 or higher (single-phase region), the desired ferrite structure cannot be achieved, and therefore the desired level of [Si+Al] cannot be achieved. F / [Si+Al] γ and the balance between tensile strength and hole expansion rate (TS 2 ×HER 1 / 2 ). In addition, when the temperature of the first heating or the first holding is lower than the temperature range of Ac1, sufficient heating cannot be performed, and the desired fine structure of the present invention cannot be achieved even through subsequent heat treatment. The average heating rate of the first heating can be 5°C / second or more.

[0155] When the primary holding time is less than 50 seconds, the structure cannot be sufficiently homogenized, so the physical properties of the steel plate may be reduced. There is no particular upper limit on the primary holding time, but in order to prevent the reduction of toughness due to the coarsening of grains, the primary heating time is preferably limited to 1200 seconds or less.

[0156] After the primary holding, it is preferred to cool (primary cooling) to a temperature range of 600-850°C (primary cooling end temperature) at an average cooling rate of 1°C / sec or more. The upper limit of the average cooling rate of the primary cooling does not need to be particularly specified, but is preferably limited to 100°C / sec or less. When the primary cooling end temperature is lower than 600°C, too much ferrite is formed and insufficient retained austenite, thereby possibly reducing [Si+Al] F / [Si+Al] γ and the balance of tensile strength and elongation (TS×El). In addition, the upper limit of the primary cooling end temperature is preferably 30°C lower than the primary holding temperature, so the upper limit of the primary cooling end temperature can be limited to 850°C.

[0157] After the primary cooling, it is preferred to cool the steel sheet to a temperature range of 300-500°C at an average cooling rate of 2°C / s or more (secondary cooling), and hold the steel sheet in the temperature range for 5 seconds or more (secondary holding). When the average cooling rate of the secondary cooling is less than 2°C / s, excessive ferrite is formed and insufficient retained austenite, thereby possibly reducing [Si+Al] F / [Si+Al] γ and the balance of tensile strength and elongation (TS×El). The upper limit of the average cooling rate of the secondary cooling does not need to be specifically specified, but is preferably limited to 100°C / s or less. In addition, when the secondary holding temperature exceeds 500°C, the residual austenite is insufficient, which may reduce [Si+Al] F / [Si+Al] γ , V(lath, γ) / V(γ), balance of tensile strength and elongation (TS×El), and bending processing rate (R / t). In addition, when the secondary holding temperature is lower than 300°C, V(1.2μm, γ) / V(γ) and bending processing rate (R / t) may be reduced due to the low heat treatment temperature. When the secondary holding time is less than 5 seconds, the heat treatment time is insufficient, so V(1.2μm, γ) / V(γ), V(lath, γ) / V(γ) and bending processing rate (R / t) may be reduced. On the other hand, the upper limit of the secondary holding time does not need to be specifically specified, but is preferably set to 600 seconds or less.

[0158] In addition, the average cooling rate (Vc1) of the primary cooling is preferably smaller than the average cooling rate (Vc2) of the secondary cooling (Vc1 <Vc2)。

[0159] After the secondary holding, it is preferred to cool (tertiary cooling) at an average cooling rate of 2°C / s or more to a temperature range of 100-300°C (secondary cooling termination temperature). When the average cooling rate of the tertiary cooling is less than 2°C / s, V(1.2μm, γ) / V(γ) and the bending working ratio (R / t) may be reduced due to slow cooling. There is no need to specifically specify an upper limit for the average cooling rate of the tertiary cooling, but it is preferably limited to 100°C / s or less. In addition, when the secondary cooling termination temperature exceeds 300°C, too much bainite is formed and insufficient tempered martensite is present, thereby possibly reducing the balance of tensile strength and elongation (TS×El). On the other hand, when the secondary cooling termination temperature is lower than 100°C, too much tempered martensite is formed and insufficient retained austenite is present, thereby possibly reducing [Si+Al] F / [Si+Al] γ , V(1.2μm, γ) / V(γ), balance of tensile strength and elongation (TS×El) and bending ratio (R / t).

[0160] After the third cooling, it is preferably heated (secondary heating) to a temperature range of 350-550°C and held (third holding) in this temperature range for more than 10 seconds. When the third holding temperature exceeds 550°C, the retained austenite is insufficient, so [Si+Al] F / [Si+Al] γ , V(lath, γ) / V(γ), balance of tensile strength and elongation (TS×El) and bending processing rate (R / t). On the other hand, when the three-holding temperature is lower than 350°C, the holding temperature is low, so V(1.2μm, γ) / V(γ) and bending processing rate (R / t) may be reduced. When the three-holding time is less than 10 seconds, the holding time is insufficient, so V(1.2μm, γ) / V(γ), V(lath, γ) / V(γ) and bending processing rate (R / t) may be reduced. There is no particular limitation on the upper limit of the three-holding time, but the preferred three-holding time may be less than 1800 seconds.

[0161] After the three holdings, it is preferred to cool (fourth cooling) to a temperature range of 250-450°C at an average cooling rate of 1°C / second or more, and hold in this temperature range for more than 10 seconds (fourth holding). When the average cooling rate of the four coolings is less than 1°C / second, V(1.2μm, γ) / V(γ) and the bending processing rate (R / t) may be reduced due to slow cooling. The upper limit of the average cooling rate of the four coolings does not need to be particularly specified, but is preferably limited to 100°C / second or less. When the four holding temperature exceeds 450°C, V(1.2μm, γ) / V(γ), V(lath, γ) / V(γ) and the bending processing rate (R / t) may be reduced due to long-term heat treatment. On the other hand, when the four holding temperature is lower than 250°C / second, V(1.2μm, γ) / V(γ), V(lath, γ) / V(γ) and the bending processing rate (R / t) may be reduced due to the low holding temperature. When the four holding times are less than 10 seconds, the holding time is insufficient, and thus V(1.2 μm, γ) / V(γ), V(slat, γ) / V(γ), and the bending processing rate (R / t) may be reduced. The upper limit of the four holding times is not particularly limited, but the preferred four holding times may be 176,000 seconds or less.

[0162] After the four times of holding, it is preferred to cool to room temperature at an average cooling rate of 1° C. / sec or more (fifth cooling).

[0163] In the high-strength steel plate with excellent workability manufactured by the above-mentioned manufacturing method, the fine structure may include tempered martensite, bainite, retained austenite and ferrite. As a preferred example, the fine structure may include 30-70% tempered martensite, 10-45% bainite, 10-40% retained austenite, 3-20% ferrite and inevitable structure by volume fraction.

[0164] In addition, in the high-strength steel sheet with excellent workability manufactured by the above manufacturing method, as shown in the following [Relationship 1], the average total content of silicon (Si) and aluminum (Al) contained in ferrite ([Si+Al] F , weight %) and the average total content of silicon (Si) and aluminum (Al) contained in the retained austenite ([Si+Al] γ , weight %) can satisfy the range of 1.1-3.0. As shown in the following [Relationship 2], the ratio of the fraction of retained austenite with an average grain size of more than 1.2 μm (V(1.2 μm, γ), volume %) to the fraction of retained austenite in the steel plate (V(γ), volume %) can be greater than 0.1.

[0165] [Equation 1]

[0166] 1.1≤[Si+Al] F / [Si+Al] γ ≤3.0

[0167] [Equation 2]

[0168] V(1.2μm,γ) / V(γ)≥0.1

[0169] In addition, in the high-strength steel plate with excellent workability manufactured by the above-mentioned manufacturing method, as shown in the following [Relationship 3], the ratio of the fraction of lath-shaped retained austenite (V (lath, γ), volume %) to the fraction of retained austenite in the steel plate (V (γ), volume %) can be greater than 0.5.

[0170] [Equation 3]

[0171] V(lath,γ) / V(γ)≥0.5

[0172] In the high-strength steel sheet with excellent workability produced by the above-mentioned production method, the balance between tensile strength and elongation (B T·E ) can be 22000 (MPa%) or more, and the balance between tensile strength and hole expansion ratio (B T·H ) can be 7*10 6 (MPa 2 % 1 / 2 ) above, the bending processing rate (B R ) can satisfy the range of 0.5 to 3.0.

[0173] [Equation 4]

[0174] B T·E =[Tensile strength (TS, MPa)]*[Elongation (El, %)]

[0175] [Equation 5]

[0176] B T·H =[Tensile strength (TS, MPa)] 2 *[Hole expansion ratio (HER, %)] 1 / 2

[0177] [Equation 6]

[0178] B R =R / t

[0179] In the above relational expression 6, R represents the minimum bending radius (mm) at which no cracks are generated after a 90° bending test, and t represents the thickness (mm) of the steel plate. DETAILED DESCRIPTION

[0180] Hereinafter, a high-strength steel plate with excellent workability and a method for manufacturing the same in one aspect of the present invention will be described in more detail through specific examples. It should be noted that the following examples are only used to understand the present invention and are not intended to limit the scope of the present invention. The scope of the present invention is determined by the contents described in the claims and the contents reasonably derived therefrom.

[0181] (Example)

[0182] A steel billet having a thickness of 100 mm and having an alloy composition (balance being Fe and inevitable impurities) described in Table 1 below was manufactured, heated at 1200° C., and then hot-finished rolled at 900° C. Thereafter, it was cooled at an average cooling rate of 30° C. / sec, and coiled at the coiling temperature of Tables 2 and 3, thereby manufacturing a hot-rolled steel sheet having a thickness of 3 mm. The hot-rolled steel sheet was subjected to hot rolling annealing heat treatment according to the conditions of Tables 2 and 3. Thereafter, it was pickled to remove surface oxide scale, and then cold rolled to a thickness of 1.5 mm.

[0183] Thereafter, heat treatment was performed according to the annealing heat treatment conditions in Tables 2 to 7 to produce steel sheets.

[0184] The microstructure of the steel plate manufactured as described above was observed, and the results are shown in Tables 8 and 9. The cross section of the polished test piece was etched with nital, and then the ferrite (F), bainite (B), tempered martensite (TM) and pearlite (P) in the microstructure were observed by SEM. Among them, the bainite and tempered martensite that are difficult to distinguish are calculated using the expansion curve after the expansion evaluation. In addition, the new martensite (FM) and the retained austenite (retained γ) are also difficult to distinguish, so the value of the retained austenite calculated by the X-ray diffraction method is subtracted from the martensite and retained austenite fractions observed by the SEM as the new martensite fraction.

[0185] In addition, the [Si+Al] F / [Si+Al] γ , V(1.2μm, γ) / V(γ), V(lath, γ) / V(γ), balance of tensile strength and elongation (TS×El), balance of tensile strength and hole expansion (TS 2 ×HER 1 / 2 ) and the bending processing rate (R / t) were observed, and the results are shown in Tables 10 and 11.

[0186] The average total content of silicon (Si) and aluminum (Al) contained in the retained austenite ([Si+Al] γ, weight %) and the average total content of silicon (Si) and aluminum (Al) contained in ferrite ([Si+Al] F , weight %). In addition, the fraction of retained austenite having an average grain size of 1.2 μm or more (V(1.2 μm, γ)) and the fraction of lath-shaped retained austenite (V(lath, γ)) were determined by measuring the area within the retained austenite using the EPMA phase map (Phase Map).

[0187] The tensile strength (TS) and elongation (El) are evaluated by a tensile test, that is, a test piece is taken in a direction of 90° relative to the rolling direction of the rolled plate and evaluated according to JIS No. 5 standard to measure the tensile strength (TS) and elongation (El). The bending processing rate (R / t) is evaluated by a V-bending test, in which a test piece is taken in a direction of 90° relative to the rolling direction of the rolled plate and the minimum bending radius R without cracks after the 90° bending test is divided by the thickness t of the plate to calculate. The hole expansion ratio (HER) is evaluated by a hole expansion test. After punching a hole (die inner diameter 10.3 mm, gap 12.5%), a conical punch with a top angle of 60° is inserted into the hole in the direction where the burr of the hole becomes the outside, and the peripheral part of the hole is squeezed and expanded at a moving speed of 20 mm / min, and then calculated using the following [Relationship 7].

[0188] [Equation 7]

[0189] Hole expansion ratio (HER, %) = {(D-D0) / D0} × 100

[0190] In the above relational expression 5, D represents the hole diameter (mm) when the crack penetrates the steel plate along the thickness direction, and D0 represents the initial hole diameter (mm).

[0191] [Table 1]

[0192]

[0193] [Table 2]

[0194]

[0195] [Table 3]

[0196]

[0197] [Table 4]

[0198]

[0199] [Table 5]

[0200]

[0201] [Table 6]

[0202]

[0203] [Table 7]

[0204]

[0205] [Table 8]

[0206]

[0207] [Table 9]

[0208]

[0209] [Table 10]

[0210]

[0211] [Table 11]

[0212]

[0213] As shown in Tables 1 to 11, in the case of the test pieces satisfying the conditions proposed in the present invention, [Si+Al] F / [Si+Al] γ The value of satisfies the range of 1.1 to 3.0, V(1.2μm, γ) / V(γ) is 0.1 or more, V(lath, γ) / V(γ) is 0.5 or more, the balance of tensile strength and elongation (TS×El) is 22000MPa% or more, the balance of tensile strength and hole expansion rate (TS 2 ×HER 1 / 2 ) is 7*10 6 (MPa 2 % 1 / 2 ) or above, and the bending working ratio (R / t) satisfies the range of 0.5 to 3.0, so it can be seen that it has excellent strength and processability.

[0214] Test pieces 2 to 5 overlapped with the alloy composition range of the present invention, but the hot rolling annealing temperature and time were outside the range of the present invention, so it was confirmed that pickling was poor or cracks occurred during cold rolling.

[0215] In the test piece 6, the primary heating or holding temperature during the annealing heat treatment after cold rolling exceeded the range limited by the present invention, so the amount of ferrite generated was insufficient. As a result, it can be confirmed that the [Si+Al] F / [Si+Al] γ The value is less than 1.1, the balance between tensile strength and hole expansion rate (TS2 ×HER 1 / 2 ) is less than 7*10 6 (MPa 2 % 1 / 2 ).

[0216] In the test piece 8, the primary cooling end temperature is low, so too much ferrite is formed, and a small amount of retained austenite is formed. As a result, it can be confirmed that the [Si+Al] F / [Si+Al] γ The value of exceeds 3.0, and the balance of tensile strength and elongation (TS×El) is less than 22000 MPa%.

[0217] In the test piece 9, due to the low average cooling rate of the secondary cooling, too much ferrite was formed and a small amount of retained austenite was formed. As a result, it can be confirmed that the [Si+Al] F / [Si+Al] γ The value of exceeds 3.0, and the balance of tensile strength and elongation (TS×El) is less than 22000 MPa%.

[0218] In the test piece 11, the secondary holding temperature is high, so a small amount of retained austenite is formed. As a result, it can be confirmed that the [Si+Al] F / [Si+Al] γ The value exceeds 3.0, V(lath, γ) / V(γ) is less than 0.5, the balance of tensile strength and elongation (TS×El) is less than 22000 MPa%, and the bending ratio (R / t) exceeds 3.0.

[0219] In test piece 12, the secondary holding temperature is low, so it can be confirmed that V(1.2μm, γ) / V(γ) is less than 0.1 and the bending processing rate (R / t) exceeds 3.0. In test piece 13, the secondary holding time is short, so it can be confirmed that V(1.2μm, γ) / V(γ) is less than 0.1, V(lath, γ) / V(γ) is less than 0.5, and the bending processing rate (R / t) exceeds 3.0.

[0220] In the test piece 14, since the average cooling rate of the three coolings was low, it was confirmed that V(1.2 μm, γ) / V(γ) was less than 0.1 and the bending ratio (R / t) exceeded 3.0.

[0221] In the test piece 15, the secondary cooling end temperature was high, so too much bainite was formed and a small amount of tempered martensite was formed. As a result, it was confirmed that the balance of tensile strength and elongation (TS×El) of the test piece 15 was less than 22000 MPa%.

[0222] In the test piece 16, the secondary cooling end temperature is low, so too much tempered martensite is formed, and a small amount of retained austenite is formed. As a result, it can be confirmed that the [Si+Al] F / [Si+Al] γ The value exceeds 3.0, V(1.2μm, γ) / V(γ) is less than 0.1, the balance between tensile strength and elongation (TS×El) is less than 22000MPa%, and the bending ratio (R / t) exceeds 3.0.

[0223] In the test piece 17, the temperature was kept high three times, so a small amount of retained austenite was formed. As a result, it can be confirmed that the [Si+Al] F / [Si+Al] γ The value exceeds 3.0, V(lath, γ) / V(γ) is less than 0.5, the balance of tensile strength and elongation (TS×El) is less than 22000 MPa%, and the bending processing rate (R / t) exceeds 3.0.

[0224] In the test piece 18, since the temperature was kept low three times, it was confirmed that V(1.2 μm, γ) / V(γ) was less than 0.1 and the bending ratio (R / t) exceeded 3.0.

[0225] In Test Piece 19, since the three holding times were short, it was confirmed that V(1.2 μm, γ) / V(γ) was less than 0.1, V(lath, γ) / V(γ) was less than 0.5, and the bending ratio (R / t) exceeded 3.0.

[0226] In test piece 20, the temperature was kept high four times, so it can be confirmed that V(1.2μm, γ) / V(γ) is less than 0.1, V(slat, γ) / V(γ) is less than 0.5, and the bending processing rate (R / t) exceeds 3.0. On the other hand, in test piece 21, the temperature was kept low four times, so it can be confirmed that V(1.2μm, γ) / V(γ) is less than 0.1, V(slat, γ) / V(γ) is less than 0.5, and the bending processing rate (R / t) exceeds 3.0.

[0227] In the test piece 22, since the four holding times were short, it was confirmed that V(1.2 μm, γ) / V(γ) was less than 0.1, V(lath, γ) / V(γ) was less than 0.5, and the bending ratio (R / t) exceeded 3.0.

[0228] Test pieces 45 to 53 are cases where the manufacturing conditions proposed in the present invention are met but the alloy composition is not within the range proposed in the present invention. In this case, it can be confirmed that all of them cannot simultaneously meet the [Si+Al] F / [Si+Al] γ, V(1.2μm, γ) / V(γ), V(lath, γ) / V(γ), balance of tensile strength and elongation (TS×El), balance of tensile strength and hole expansion (TS 2 ×HER 1 / 2 ) is 7*10 6 (MPa 2 % 1 / 2 ) and bending processing rate (R / t). In addition, the total content of aluminum (Al) and silicon (Si) in test piece 47 is less than 1.0%, which can confirm that it cannot meet the [Si+Al] F / [Si+Al] γ , the balance of tensile strength and elongation (TS×El) and the bending processing rate (R / t) conditions.

[0229] The present invention has been described in detail above through the embodiments, but other forms of embodiments may also be included. Therefore, the technical concept and scope of the claims are not limited to the embodiments.

Claims

1. A method for producing a high-strength steel sheet with excellent workability, wherein The following steps are involved: A cold-rolled steel sheet is provided, wherein the cold-rolled steel sheet comprises, in weight percent, 0.25-0.75% C, 4.0% or less Si, 0.9-5.0% Mn, 5.0% or less Al, 0.15% or less P, 0.03% or less S, 0.03% or less N, and the balance Fe and unavoidable impurities; The cold-rolled steel sheet is heated to a temperature range of more than Ac1 and less than Ac3 at an average heating rate of more than 5°C / s, i.e., heated once, and maintained for more than 50 seconds, i.e., maintained once; Cooling to a temperature range of 600-850°C of a primary cooling termination temperature at an average cooling rate of 1°C / s or more, i.e., primary cooling; Cooling to a temperature range of 300-500°C at an average cooling rate of more than 2°C / s, i.e., secondary cooling, and holding in this temperature range for more than 5 seconds, i.e., secondary holding; Cooling to a temperature range of 100-300°C secondary cooling termination temperature at an average cooling rate of 2°C / s or more, i.e., tertiary cooling; Heating to a temperature range of 350-550°C, i.e., secondary heating, and maintaining within this temperature range for more than 10 seconds, i.e., third holding; Cooling to a temperature range of 250-450° C. at an average cooling rate of 1° C. / s or more, i.e., cooling four times, and holding in the temperature range for more than 10 seconds, i.e., holding four times; and Cool to room temperature, i.e. cool five times.

2. The method for producing a high-strength steel sheet having excellent workability according to claim 1, in, The cold-rolled steel sheet further comprises any one or more of the following (1) to (9): (1) one or more of Ti: 0-0.5%, Nb: 0-0.5% and V: 0-0.5%, (2) one or more of Cr: 0-3.0% and Mo: 0-3.0%, (3) Cu: 0-4.5% and Ni: 0-4.5% or more, (4)B:0-0.005%, (5) one or more of Ca: 0-0.05%, REM excluding Y: 0-0.05% and Mg: 0-0.05%, (6) one or more of W: 0-0.5% and Zr: 0-0.5%, (7) one or more of Sb: 0-0.5% and Sn: 0-0.5%, (8) one or more of Y: 0-0.2% and Hf: 0-0.2%, (9) Co: 0-1.5%.

3. The method for producing a high-strength steel sheet having excellent workability according to claim 1, in, The total content Si+Al of the Si and Al contained in the cold-rolled steel sheet is 1.0-6.0 wt %.

4. The method for producing a high-strength steel sheet having excellent workability according to claim 1, in, The cold rolled steel sheet is provided by the following steps: Heat the steel billet to 1000-1350°C; Hot finishing rolling is carried out in a temperature range of 800-1000°C; The hot rolled steel plate is coiled in the temperature range of 300-600°C; In the temperature range of 650 - 850 °C, hot rolling and annealing heat treatment is carried out on the coiled steel plate for 600 - 1700 seconds; and The cold rolling is carried out on the steel plate subjected to hot rolling and annealing heat treatment at a reduction rate of 30 - 90%.

5. The method for manufacturing a high-strength steel plate with excellent manufacturability according to claim 1, wherein, The cooling rate Vc1 of the primary cooling and the cooling rate Vc2 of the secondary cooling satisfy the relationship of Vc1 < Vc2.