A method for preparing submicron titanium dioxide with controllable particle size
By using polyacrylic acid or polyacrylamide as a control agent in the production of titanium dioxide, hydrolysis and three-step high-temperature heat treatment, the problem of difficult control of titanium dioxide particle size and purity in the prior art is solved, and the submicron level of high purity and controllability are achieved Suitable for industrial production.
Patent Information
- Application Number
- CN202210441770.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-25
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-04-25
AI Technical Summary
In the existing titanium dioxide production process, especially the sulfuric acid method, there are problems of environmental pollution and by-products. Although the chlorination method has excellent performance, its technical level limits its development in my country, and it is difficult to achieve high purity on the submicron-scale particle size. and controllability.
Polyacrylic acid or polyacrylamide is used as process control agent, titanium tetrachloride is added dropwise to deionized water for hydrolysis, and the particle size is controlled and adjustable on the submicron scale through three-step high-temperature heat treatment, so as to obtain uniform dispersion, Rutile-type titanium dioxide powder with high purity.
It realizes controllability and high purity of particle size at the submicron level, simple process, high efficiency and good repeatability, suitable for industrial production, and is suitable for titanium dioxide powder size requirements in different fields.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of inorganic non-metallic materials and new chemical materials, and specifically relates to a method for preparing submicron titanium dioxide with controllable particle size. Background Art
[0002] Titanium dioxide, also known as "titanium dioxide", is an important metal oxide, mainly in three crystal forms: rutile, anatase and brookite; brookite is an unstable crystal form, which is easy to transform into rutile at high temperature and is rarely used in industrial applications. Titanium dioxide has very stable chemical properties, and has the advantages of excellent optical properties, good weather resistance, high tinting power, good whiteness, strong hiding power, etc. It is widely used in coatings, plastics, papermaking, inks, chemical fibers, ceramics, daily chemicals, capacitors, photocatalysis and other fields.
[0003] There are two main methods for industrial production of titanium dioxide: sulfuric acid method and chlorination method. The sulfuric acid method has a long history of application and mature technology, but it causes greater environmental pollution and produces more by-products (titanium dioxide gypsum, ferrous sulfate, etc.). The existing process needs to be upgraded and transformed. The titanium dioxide produced by the chlorination method has better optical and chemical properties, and has the advantages of short production process, continuous operation, high degree of automation, large scale of single series equipment, and less "three wastes". From the perspective of process and production safety, it is the general trend of the development of production methods in the titanium dioxide industry in the future. However, due to the constraints of technical level, the production of titanium dioxide by the chlorination method in my country has progressed very slowly.
[0004] The particle size of titanium dioxide powder has a great influence on its performance. Taking the submicron titanium dioxide required by the coating industry as an example, the tinting power of rutile titanium dioxide decreases significantly with the increase of the primary particle size in the submicron range; when the primary particle size of titanium dioxide pigment is 0.15-0.5μm, its hiding power increases with the increase of particle size. Therefore, when hiding power is the basic requirement, for example, general architectural coatings usually use large-particle titanium dioxide of about 0.4-0.5μm, while in high-decoration occasions, in order to take into account factors such as hiding power, tinting power and glossiness, titanium dioxide of 0.15-0.25μm is generally used.
[0005] Therefore, it is imperative to invent a method for preparing titanium dioxide with high purity, suitable for industrial production, and controllable and adjustable particle size at the submicron scale using the chlorination method. Summary of the invention
[0006] The present invention aims to provide a method for preparing submicron titanium dioxide with controllable particle size, which has simple process, high efficiency and yield, and good repeatability. The prepared titanium dioxide powder has high purity, is evenly dispersed and does not agglomerate, and its particle size is controllable and adjustable on a submicron scale, which is suitable for the industrialized and stable preparation of submicron high-purity titanium dioxide.
[0007] A method for preparing submicron titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0008] (1) Preparation of a metatitanic acid precursor: titanium tetrachloride is added dropwise into deionized water, stirred, heated and hydrolyzed, and then a process control agent is added, stirred, filtered and vacuum dried to obtain a metatitanic acid precursor; wherein the control agent is polyacrylic acid or polyacrylamide, and the hydrolysis temperature is 95 to 105°C;
[0009] (2) Preparation of submicron titanium dioxide powder: The metatitanate precursor obtained in step (1) is subjected to three-step heat treatment in an air atmosphere, and then naturally cooled to room temperature to obtain submicron titanium dioxide powder; wherein the three-step heat treatment process is as follows: the first step heat treatment temperature is 410-430°C, and the time is 1-2 hours; the second step heat treatment temperature is 500-540°C, and the reaction time is 1-2 hours; the third step heat treatment temperature is 630-680°C, and the reaction time is 1-2 hours.
[0010] In the above scheme, in step (1), titanium tetrachloride is added to deionized water to obtain a titanium tetrachloride aqueous solution with a concentration of 1.5 to 2.5 mol / L.
[0011] In the above scheme, in step (1), the concentration of the process control agent in the aqueous solution is 0.5 to 2.5 g / L.
[0012] In the above scheme, in step (1), the hydrolysis time is 0.5 to 2 hours.
[0013] In the above scheme, in step (1), the drying temperature is 105-115° C. and the drying time is 12-24 hours.
[0014] The invention provides a preparation method of submicron titanium dioxide with controllable particle size. Polyacrylic acid or polyacrylamide is used as a process control agent, titanium tetrachloride is controlled to be added dropwise into deionized water, and a hydrolysis reaction is carried out at low temperature boiling (95-105°C), so that the hydrolysis sedimentation kinetic process is effectively promoted, the generated metatitanic acid precursor is rapidly flocculated and sedimented, the conversion efficiency and the reaction efficiency are improved, and the submicron metatitanic acid precursor is obtained. The process control agent is easy to be removed in the subsequent heat treatment, and has no obvious influence on the quality and purity of the product. At the same time, by controlling the temperature and heat treatment time of the three-step high-temperature heat treatment of the obtained metatitanic acid precursor, a uniformly dispersed, high-purity, and fully rutile submicron titanium dioxide powder can be obtained; wherein: in the first step of heat treatment, metatitanic acid reacts to generate anatase-type titanium dioxide, and can remove polyacrylic acid or polyacrylamide process control agents and by-products generated when preparing the metatitanic acid precursor; in the second step of heat treatment, the anatase-type titanium dioxide can be completely converted into rutile-type titanium dioxide; the purpose of the third step of heat treatment is to make the particle size of rutile-type titanium dioxide controllable and adjustable at the submicron scale by adjusting the temperature and time.
[0015] The beneficial effects of the present invention are:
[0016] 1. The present invention provides a method for preparing submicron titanium dioxide with controllable particle size. Polyacrylic acid or polyacrylamide is used as a process control agent, titanium tetrachloride is controlled to be added dropwise into deionized water and hydrolyzed at low temperature boiling (95-105°C), the obtained metatitanic acid precursor is combined with three-step high-temperature heat treatment, and the temperature and heat treatment time of the three-step high-temperature heat treatment are controlled, so that a submicron titanium dioxide powder with uniform dispersion, no agglomeration, high purity and full rutile crystal form can be obtained, and its particle size is controllable and adjustable at the submicron scale.
[0017] 2. The preparation process of the present invention is simple, efficient, high in yield, and has good repeatability, and is suitable for the industrial and stable preparation of submicron high-purity titanium dioxide; at the same time, the particle size of titanium dioxide is controllable and adjustable at the submicron scale, and can be regulated on demand according to the different requirements for the size of titanium dioxide powder in different fields, and has broad application prospects. DETAILED DESCRIPTION
[0018] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0019] Example 1
[0020] A method for preparing submicron titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0021] (1) Preparation of titanate precursor: 1.5 mol titanium tetrachloride was added dropwise into 1 L of deionized water, stirred, heated to 95°C for hydrolysis reaction for 0.5 h, and then 0.5 g polyacrylic acid was added, stirred, filtered, and vacuum dried at 105°C for 12 h to obtain a titanate precursor.
[0022] (2) Preparation of submicron titanium dioxide powder: The metatitanate precursor obtained in step (1) is placed in a muffle furnace with an air atmosphere, heat treated at 410°C for 1 hour, then heated to 500°C for 1 hour, then heated to 630°C for 1 hour, and then naturally cooled to room temperature. The precursor is completely converted into pure white submicron titanium dioxide.
[0023] The average particle size of the titanium dioxide product obtained was measured by scanning electron microscopy, transmission electron microscopy and laser particle size analyzer to be 0.11 μm, and it was evenly dispersed without obvious agglomeration; the crystal form of the titanium dioxide product was measured by X-ray diffractometer to be rutile; the purity of the titanium dioxide product was measured by inductively coupled plasma atomic emission spectrometer to be greater than 99.9%.
[0024] Example 2
[0025] A method for preparing submicron titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0026] (1) Preparation of titanate precursor: 2.5 mol titanium tetrachloride was added dropwise into 1 L of deionized water, stirred, heated to 105 °C for hydrolysis reaction for 2 h, and then 2.5 g polyacrylamide was added, stirred, filtered, and vacuum dried at 115 °C for 24 h to obtain a titanate precursor.
[0027] (2) Preparation of submicron titanium dioxide powder: The metatitanate precursor obtained in step (1) is placed in a muffle furnace with an air atmosphere, heat treated at 430°C for 2 h, then heated to 540°C for 2 h, then heated to 680°C for 2 h, and then naturally cooled to room temperature. The precursor is completely converted into pure white submicron titanium dioxide.
[0028] The average particle size of the titanium dioxide product obtained was measured by scanning electron microscope, transmission electron microscope and laser particle size analyzer, and was 0.83 μm. It was evenly dispersed without obvious agglomeration. The crystal form of the titanium dioxide product was measured by X-ray diffractometer and was rutile. The purity of the titanium dioxide product was measured by inductively coupled plasma atomic emission spectrometer and was greater than 99.9%.
[0029] Example 3
[0030] A method for preparing submicron titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0031] (1) Preparation of titanate precursor: 2.5 mol titanium tetrachloride was added dropwise into 1 L of deionized water, stirred, heated to 105° C. for hydrolysis reaction for 0.5 h, and then 2.5 g polyacrylic acid was added, stirred, filtered, and vacuum dried at 115° C. for 12 h to obtain a titanate precursor.
[0032] (2) Preparation of submicron titanium dioxide powder: The metatitanate precursor obtained in step (1) is placed in a muffle furnace with an air atmosphere, heat treated at 430°C for 1 hour, then heated to 540°C for 1 hour, then heated to 680°C for 1 hour, and then naturally cooled to room temperature. The precursor is completely converted into pure white submicron titanium dioxide.
[0033] The average particle size of the titanium dioxide product obtained was measured by scanning electron microscope, transmission electron microscope and laser particle size analyzer, and was 0.76 μm. It was evenly dispersed without obvious agglomeration. The crystal form of the titanium dioxide product was measured by X-ray diffractometer and was rutile. The purity of the titanium dioxide product was measured by inductively coupled plasma atomic emission spectrometer and was greater than 99.9%.
[0034] Example 4
[0035] A method for preparing submicron titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0036] (1) Preparation of titanate precursor: 1.5 mol titanium tetrachloride was added dropwise into 1 L of deionized water, stirred, heated to 95° C. for hydrolysis reaction for 2 h, and then 0.5 g polyacrylamide was added, stirred, filtered, and vacuum dried at 105° C. for 24 h to obtain a titanate precursor.
[0037] (2) Preparation of submicron titanium dioxide powder: The titanate precursor obtained in step (1) is placed in a muffle furnace with an air atmosphere, heat treated at 410°C for 2 h, then heated to 500°C for 2 h, then heated to 630°C for 2 h, and then naturally cooled to room temperature. The precursor is completely converted into pure white submicron titanium dioxide.
[0038] The average particle size of the titanium dioxide product obtained was measured by scanning electron microscopy, transmission electron microscopy and laser particle size analyzer to be 0.23 μm, and it was evenly dispersed without obvious agglomeration; the crystal form of the titanium dioxide product was measured by X-ray diffractometer to be rutile; the purity of the titanium dioxide product was measured by inductively coupled plasma atomic emission spectrometer to be greater than 99.9%.
[0039] Example 5
[0040] A method for preparing submicron titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0041] (1) Preparation of titanate precursor: 1.5 mol titanium tetrachloride was added dropwise into 1 L of deionized water, stirred, heated to 98°C for hydrolysis reaction for 0.5 h, and then 1.0 g of polyacrylic acid was added, stirred, filtered, and vacuum dried at 105°C for 16 h to obtain a titanate precursor.
[0042] (2) Preparation of submicron titanium dioxide powder: The metatitanate precursor obtained in step (1) is placed in a muffle furnace with air atmosphere, heat treated at 420°C for 1 hour, then heated to 510°C for 1 hour, then heated to 640°C for 1 hour, and then naturally cooled to room temperature. The precursor is completely converted into pure white submicron titanium dioxide.
[0043] The average particle size of the titanium dioxide product obtained was measured by scanning electron microscope, transmission electron microscope and laser particle size analyzer, and was 0.38 μm. It was evenly dispersed without obvious agglomeration. The crystal form of the titanium dioxide product was measured by X-ray diffractometer and was rutile. The purity of the titanium dioxide product was measured by inductively coupled plasma atomic emission spectrometer and was greater than 99.9%.
[0044] Example 6
[0045] A method for preparing submicron titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0046] (1) Preparation of titanate precursor: 2 mol of titanium tetrachloride was added dropwise into 1 L of deionized water, stirred, and heated to 100° C. for hydrolysis reaction for 1 h. Then 1 g of polyacrylamide was added, stirred, filtered, and vacuum dried at 110° C. for 16 h to obtain a titanate precursor.
[0047] (2) Preparation of submicron titanium dioxide powder: The metatitanate precursor obtained in step (1) is placed in a muffle furnace with an air atmosphere, heat treated at 420°C for 1.5 h, then heated to 520°C for 1.5 h, then heated to 650°C for 1.5 h, and then naturally cooled to room temperature. The precursor is completely converted into pure white submicron titanium dioxide.
[0048] The average particle size of the titanium dioxide product obtained was measured by scanning electron microscope, transmission electron microscope and laser particle size analyzer, and was 0.45 μm. It was evenly dispersed without obvious agglomeration. The crystal form of the titanium dioxide product was measured by X-ray diffractometer and was rutile. The purity of the titanium dioxide product was measured by inductively coupled plasma atomic emission spectrometer and was greater than 99.9%.
[0049] Example 7
[0050] A method for preparing submicron titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0051] (1) Preparation of titanate precursor: 2 mol of titanium tetrachloride was added dropwise into 1 L of deionized water, stirred, heated to 100° C. for hydrolysis reaction for 1.5 h, and then 1.5 g of polyacrylic acid was added, stirred, filtered, and vacuum dried at 110° C. for 20 h to obtain a titanate precursor.
[0052] (2) Preparation of submicron titanium dioxide powder: The metatitanate precursor obtained in step (1) is placed in a muffle furnace with an air atmosphere, heat treated at 410°C for 1.5 h, then heated to 530°C for 2 h, and then heated to 660°C for 1.5 h, and then naturally cooled to room temperature. The precursor is completely converted into pure white submicron titanium dioxide.
[0053] The average particle size of the titanium dioxide product obtained was measured by scanning electron microscope, transmission electron microscope and laser particle size analyzer, and was 0.59 μm. It was evenly dispersed without obvious agglomeration. The crystal form of the titanium dioxide product was measured by X-ray diffractometer and was rutile. The purity of the titanium dioxide product was measured by inductively coupled plasma atomic emission spectrometer and was greater than 99.9%.
[0054] Example 8
[0055] A method for preparing submicron titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0056] (1) Preparation of titanate precursor: 2.5 mol titanium tetrachloride was added dropwise into 1 L of deionized water, stirred, heated to 102° C. for hydrolysis reaction for 1.5 h, and then 2 g of polyacrylamide was added, stirred, filtered, and vacuum dried at 115° C. for 20 h to obtain a titanate precursor.
[0057] (2) Preparation of submicron titanium dioxide powder: The metatitanate precursor obtained in step (1) is placed in a muffle furnace with an air atmosphere, heat treated at 430°C for 1.5 h, then heated to 530°C for 1.5 h, then heated to 670°C for 2 h, and then naturally cooled to room temperature. The precursor is completely converted into pure white submicron titanium dioxide.
[0058] The average particle size of the titanium dioxide product obtained was measured by scanning electron microscope, transmission electron microscope and laser particle size analyzer, and was 0.66 μm. It was evenly dispersed without obvious agglomeration. The crystal form of the titanium dioxide product was measured by X-ray diffractometer and was rutile. The purity of the titanium dioxide product was measured by inductively coupled plasma atomic emission spectrometer and was greater than 99.9%.
[0059] Obviously, the above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from this are still within the protection scope of the invention.
Claims
1. A method for preparing submicron titanium dioxide with controllable particle size, characterized in that: The specific steps are as follows: (1) Preparation of a metatitanic acid precursor: titanium tetrachloride is added dropwise into deionized water, stirred, heated and hydrolyzed, and then a process control agent is added, stirred, filtered and vacuum dried to obtain a metatitanic acid precursor; wherein the control agent is polyacrylic acid or polyacrylamide, and the hydrolysis temperature is 95 to 105°C; (2) Preparation of submicron titanium dioxide powder: The metatitanate precursor obtained in step (1) is subjected to three-step heat treatment in an air atmosphere, and then naturally cooled to room temperature to obtain submicron titanium dioxide powder; wherein the three-step heat treatment process is as follows: the first step heat treatment temperature is 410-430°C, and the time is 1-2 hours; the second step heat treatment temperature is 500-540°C, and the reaction time is 1-2 hours; the third step heat treatment temperature is 630-680°C, and the reaction time is 1-2 hours.
2. The preparation method according to claim 1, characterized in that: In the step (1), titanium tetrachloride is added to deionized water to obtain a titanium tetrachloride aqueous solution with a concentration of 1.5 to 2.5 mol / L.
3. The preparation method according to claim 1, characterized in that: In the step (1), the concentration of the process control agent in the aqueous solution is 0.5 to 2.5 g / L.
4. The preparation method according to claim 1, characterized in that: In the step (1), the hydrolysis time is 0.5 to 2 hours.
5. The preparation method according to claim 1, characterized in that: In the step (1), the drying temperature is 105 to 115° C. and the drying time is 12 to 24 hours.