A modified biochar / attapulgite composite material, preparation method and application thereof

Through the preparation of modified biochar/attapulgite composite materials, the problem of low efficiency of existing adsorption methods in the treatment of various heavy metal wastewater has been solved, and efficient removal of multi-element heavy metal systems has been achieved, especially the adsorption of cadmium and lead. showed significant improvements.

CN114870800BActive Publication Date: 2024-10-15SOUTHEAST UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210479253.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-05
Publication Date
2024-10-15
Estimated Expiration
2042-05-05

AI Technical Summary

Technical Problem

Existing adsorption methods have synergistic, antagonistic or competitive effects when treating wastewater containing multiple heavy metal ions, resulting in low removal efficiency of certain heavy metals and affecting practical applications.

Method used

Modified biochar/attapulgite composite materials are used. Through the pyrolysis treatment of rice straw and attapulgite in calcium chloride and sodium hydroxide solutions, a composite material with a porous structure and high specific surface area is formed, which enhances the resistance to heavy metal ions. adsorption performance.

Benefits of technology

The composite material shows good adsorption effects in both mono- and multi-element heavy metal systems, significantly improves the removal rate of cadmium and lead, and solves the competition problem of adsorbents for multiple heavy metals in the existing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114870800B_ABST
    Figure CN114870800B_ABST
Patent Text Reader

Abstract

The present invention relates to a modified biochar / attapulgite composite material, a preparation method and an application thereof, wherein the preparation method comprises the following steps: step 1, raw material pretreatment: sieved rice straw and attapulgite are mixed and placed in a calcium chloride solution for immersion treatment, and then dried, dried, ground, and sieved in sequence to obtain a composite raw material; step 2, pyrolysis: the composite raw material is placed in a tubular furnace, pyrolyzed in an inert gas atmosphere, and then washed with deionized water to neutrality, dried, ground, and sieved to obtain a composite material; step 3, sodium hydroxide modification: the composite material is added to a sodium hydroxide solution for immersion treatment, dried, pyrolyzed for 1h, washed with deionized water to neutrality, and dried to obtain a sodium hydroxide modified biochar / attapulgite composite material. The present invention has a good adsorption effect when treating mono-heavy metal system wastewater and multi-heavy metal system wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmental protection, and in particular relates to a modified biochar / attapulgite composite material, a preparation method and application thereof. Background Art

[0002] Heavy metal pollution is one of the most harmful water pollution problems. In freshwater ecosystems, the main sources of heavy metals in wastewater are natural (rock weathering and volcanic activity, etc.) and man-made (industrial and agricultural activities, domestic sewage discharge). Unlike organic pollutants, heavy metals are non-degradable, so they will continue to accumulate in the environment. When they accumulate to a certain limit, they will cause serious harm to the aquatic ecosystem and pose a risk to human health directly or indirectly through the food chain. At present, many technologies have been applied to remove harmful heavy metal ions in aqueous solutions, such as adsorption, chemical precipitation, ion exchange and membrane filtration. Among them, the adsorption method is widely used in heavy metal wastewater treatment due to its advantages of high treatment efficiency, simple operation and low cost.

[0003] However, when using the adsorption method to treat heavy metals in sewage, there are the following problems. For example, when adsorbents such as activated carbon, clay minerals, chitosan, carbon nanotubes, graphene and metal oxides adsorb heavy metal ions in the unit system, they have better adsorption effects. However, for actual wastewater containing multiple heavy metal ions, due to the synergistic, antagonistic or competitive effects between the heavy metals during the adsorption process, these adsorbents improve the removal efficiency of heavy metals with strong competitiveness, while the removal effect on other heavy metal ions is extremely poor or even no removal effect; thus affecting its application in treating actual wastewater. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects in the prior art and provide a modified biochar / attapulgite composite material, a preparation method and its application, which has good adsorption effect when treating mono-heavy metal system wastewater and multi-heavy metal system wastewater.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] Technical solution 1:

[0007] A method for preparing a modified biochar / attapulgite composite material comprises the following steps:

[0008] Step 1, raw material pretreatment: sieve the attapulgite, wash and dry the rice straw, crush and sieve it, then mix the rice straw and attapulgite and immerse them in a calcium chloride solution, and then dry, bake, grind and sieve them in sequence to obtain a rice straw / attapulgite composite raw material;

[0009] Step 2, pyrolysis: placing the rice straw / attapulgite composite raw material obtained in step 1 in a tubular furnace, heating it to 400-600°C under an inert gas atmosphere, and pyrolyzing it at 400-600°C for 1 hour. After the pyrolysis is completed, cooling it to room temperature, washing it with deionized water to neutrality, drying, grinding, and sieving to obtain a calcium chloride modified biochar / attapulgite composite material.

[0010] Furthermore, in step 1, the rice straw and attapulgite are sieved through a 60-mesh standard sieve before and after mixing;

[0011] The sieve used for sieving in step 2 is 100 mesh.

[0012] Furthermore, in step 1, the mass volume ratio of rice straw, attapulgite and calcium chloride solution is: 1-5g:1g:100mL; the concentration of the calcium chloride solution is 2-20g / 100mL.

[0013] Furthermore, in step 1, during the immersion treatment, ultrasonic immersion is first performed for 30 minutes to 2 hours, then stirred immersion is performed for 4 to 6 hours, and then static immersion is performed for 12 to 24 hours;

[0014] The stirring and impregnation is carried out by stirring with a magnetic stirrer.

[0015] Furthermore, it also includes: Step 3, sodium hydroxide modification: adding the biochar / attapulgite composite material prepared in step 2 into a sodium hydroxide solution and impregnating it at 40°C. After the impregnation, drying and grinding it, then placing it in a tubular furnace, heating it to 600°C under an inert gas atmosphere, and pyrolyzing it at 600°C for 1 hour. After the pyrolysis is completed again, cooling it to room temperature, washing it with deionized water to neutrality, and drying it to obtain a sodium hydroxide modified biochar / attapulgite composite material.

[0016] Furthermore, the inert gas is nitrogen;

[0017] The heating rate in step 2 is 10℃·min -1 , the inert gas flow rate is 0.5 L min -1 ;

[0018] The heating rate in step 3 is 10℃·min -1 , the inert gas flow rate is 0.2L·min -1 .

[0019] Further, the concentration of the sodium hydroxide solution in step 3 is 0.5 to 4 mol / L;

[0020] In step 3, during the impregnation treatment, the mixture is first stirred and impregnated for 4 to 6 hours, and then allowed to stand and impregnate for 12 to 24 hours;

[0021] Furthermore, in step 3, the drying temperature is 105° C. and the drying time is 6 to 10 hours.

[0022] Technical solution 2:

[0023] A modified biochar / attapulgite composite material prepared by the above preparation method.

[0024] Technical solution three:

[0025] An application of the modified biochar / attapulgite composite material in sewage treatment.

[0026] Furthermore, the application method is: mixing the modified biochar / attapulgite composite material with wastewater containing cadmium and lead, and obtaining a filtrate after oscillation, centrifugation and filtration.

[0027] Furthermore, the concentration of cadmium and lead ions in the wastewater is 50-800 mg / L.

[0028] Furthermore, the solid-liquid ratio of the modified biochar / attapulgite composite material to wastewater is 1 to 8 g:1 / L.

[0029] Furthermore, the oscillation rate is 200 r / min, the oscillation time is 24 h, the centrifugal rate is 3000 r / min, and the centrifugal time is 5 min.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1. The raw materials used in the present invention are rice straw and attapulgite, which are widely available and pollution-free. Among them, rice straw is used as raw material for pyrolysis to produce biochar, which realizes the resource utilization of agricultural and forestry wastes, can solve the problems of non-point source pollution and increased greenhouse gas emissions caused by returning straw to the fields, and can also adsorb and fix pollutants.

[0032] 2. The present invention prepares biochar / attapulgite composite materials by co-pyrolysis of biomass raw materials, attapulgite and calcium chloride, wherein the biochar is used as a good porous matrix to support and carry clay mineral nanoparticles. At the same time, the higher cation exchange capacity and specific surface area of ​​the clay mineral are conducive to improving the adsorption capacity of the biochar, increasing the specific surface area of ​​the composite material, optimizing its pore structure, and at the same time increasing the number of oxygen-containing functional groups, providing more adsorption sites, and improving its adsorption performance for heavy metal ions.

[0033] 3. The present invention modifies the biochar / attapulgite composite material by sodium hydroxide, thereby increasing the alkaline oxygen-containing functional groups, enriching the pore structure, and significantly improving the adsorption capacity of the composite material for cadmium and lead in a multi-metal system. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 is a SEM image of the sodium hydroxide modified biochar / attapulgite composite material in Example 3 of the present invention;

[0035] Figure 2 This is the XRD spectrum of the sodium hydroxide modified biochar / attapulgite composite material before and after adsorption of lead or cadmium in Effect Example 3 of the present invention. DETAILED DESCRIPTION

[0036] The present invention is further described in detail below with reference to specific embodiments.

[0037] Example 1

[0038] A method for preparing a calcium chloride modified biochar / attapulgite composite material comprises the following steps:

[0039] Step 1, raw material pretreatment: pass the attapulgite through a 60-mesh sieve, wash and dry the rice straw, crush it and pass it through a 60-mesh sieve, then mix 12g of rice straw and 4g of attapulgite and place it in 100mL of 8.0g / 100mL calcium chloride solution for immersion treatment (the mass ratio of rice straw to attapulgite in this embodiment is 3:1), and the immersion treatment is carried out at room temperature, first ultrasonically immerse for 2h, then stir and immerse for 6h, and finally stand and immerse for 24h, and then dry, dry, grind, and pass it through a 60-mesh sieve in sequence to obtain a rice straw / attapulgite composite raw material for standby use;

[0040] Step 2, pyrolysis: The rice straw / attapulgite composite material prepared in step 1 is placed in a tubular furnace and heated to 600°C under a nitrogen atmosphere at a heating rate of 10°C·min -1 , nitrogen flow rate is 0.5 L·min -1 , and pyrolyzed at 600°C for 1h, cooled to room temperature after the pyrolysis, then washed with deionized water until neutral, dried, ground, and passed through a 100-mesh sieve to obtain a calcium chloride-modified biochar / attapulgite composite material for later use;

[0041] Example 2

[0042] A method for preparing a calcium chloride modified biochar / attapulgite composite material comprises the following steps:

[0043] Step 1, raw material pretreatment: pass the attapulgite through a 60-mesh sieve, wash and dry the rice straw, crush it and pass it through a 60-mesh sieve, then mix 14 g of rice straw and 2.8 g of attapulgite and place it in 100 mL of 8.4 g / 100 mL calcium chloride solution for immersion treatment (the mass ratio of rice straw to attapulgite in this embodiment is 5:1), and the immersion treatment is carried out at room temperature, first ultrasonically immerse for 2 hours, then stir and immerse for 6 hours, and finally stand and immerse for 24 hours, and then dry, dry, grind, and pass it through a 60-mesh sieve in sequence to obtain a rice straw / attapulgite composite raw material for standby use;

[0044] Step 2, pyrolysis: The rice straw / attapulgite composite material prepared in step 1 is placed in a tubular furnace and heated to 600°C under a nitrogen atmosphere at a heating rate of 10°C·min -1 , nitrogen flow rate is 0.5 L·min -1 , and pyrolyzed at 600°C for 1h, cooled to room temperature after the pyrolysis, then washed with deionized water until neutral, dried, ground, and passed through a 100-mesh sieve to obtain a calcium chloride-modified biochar / attapulgite composite material for later use;

[0045] Embodiment 3:

[0046] A method for preparing a modified biochar / attapulgite composite material comprises the following steps:

[0047] Step 1, raw material pretreatment: pass the attapulgite through a 60-mesh sieve, wash and dry the rice straw, crush it and pass it through a 60-mesh sieve, then mix 14 g of rice straw and 2.8 g of attapulgite and place it in 100 mL of 8.4 g / 100 mL calcium chloride solution for immersion treatment (the mass ratio of rice straw to attapulgite in this embodiment is 5:1). During the immersion treatment, first ultrasonically immerse for 2 hours, then stir and immerse for 6 hours, and finally stand and immerse for 24 hours, and then dry, dry, grind, and pass through a 60-mesh sieve in sequence to obtain a rice straw / attapulgite composite raw material for standby use;

[0048] Step 2, pyrolysis: The rice straw / attapulgite composite material prepared in step 1 is placed in a tubular furnace and heated to 600°C under a nitrogen atmosphere at a heating rate of 10°C·min -1 , nitrogen flow rate is 0.5 L·min -1 , and pyrolyzed at 600°C for 1h, cooled to room temperature after the pyrolysis, then washed with deionized water until neutral, dried, ground, and passed through a 100-mesh sieve to obtain a calcium chloride-modified biochar / attapulgite composite material for later use;

[0049] Step 3, sodium hydroxide modification: weigh 10 g of the calcium chloride modified biochar / attapulgite composite material obtained in step 2, add it to 100 mL of a sodium hydroxide solution with a mass concentration of 2 mol / L, and immerse it at 40 ° C. During the immersion treatment, first stir and immerse it at 40 ° C for 6 h, and then stand and immerse it at 40 ° C for 12 h; after the immersion is completed, dry and grind it, and then place it in a tubular furnace, heat it to 600 ° C in a nitrogen atmosphere, and the heating rate is 10 ° C min -1 , nitrogen flow rate is 0.2L·min -1 , and pyrolyzed at 600℃ for 1h, cooled to room temperature after the pyrolysis was completed, washed with deionized water until neutral, and dried to obtain a sodium hydroxide modified biochar / attapulgite composite material. The prepared sodium hydroxide modified biochar / attapulgite composite material was scanned by SEM. The results are shown in Figure 1 .

[0050] Embodiment 4:

[0051] A method for preparing a sodium hydroxide modified biochar / attapulgite composite material comprises the following steps:

[0052] Step 1, raw material pretreatment: pass the attapulgite through a 60-mesh sieve, wash and dry the rice straw, crush it and pass it through a 60-mesh sieve, then mix 10 g of rice straw and 2.5 g of attapulgite and place it in 100 mL of a 5 g / 100 mL calcium chloride solution for immersion treatment (the mass ratio of rice straw to attapulgite in this embodiment is 4:1). During the immersion treatment, first ultrasonically immerse for 2 hours, then stir and immerse for 6 hours, and finally stand and immerse for 24 hours, and then dry, dry, grind, and pass it through a 60-mesh sieve in sequence to obtain a rice straw / attapulgite composite raw material for standby use;

[0053] Step 2, pyrolysis: The rice straw / attapulgite composite material prepared in step 1 is placed in a tubular furnace and heated to 600°C under a nitrogen atmosphere at a heating rate of 10°C·min -1 , nitrogen flow rate is 0.5 L·min -1 , and pyrolyzed at 600°C for 1h, cooled to room temperature after the pyrolysis, then washed with deionized water until neutral, dried, ground, and passed through a 100-mesh sieve to obtain a calcium chloride-modified biochar / attapulgite composite material for later use;

[0054] Step 3, sodium hydroxide modification: weigh 10 g of the calcium chloride modified biochar / attapulgite composite material obtained in step 2, add it to 100 mL of a sodium hydroxide solution with a mass concentration of 4 mol / L, and immerse it at 40°C. During the immersion treatment, first stir and immerse it at 40°C for 6 h, and then stand and immerse it at 40°C for 24 h; after the immersion is completed, dry and grind it, then place it in a tubular furnace, and heat it to 600°C under a nitrogen atmosphere at a heating rate of 10°C min -1, nitrogen flow rate is 0.2L·min -1 , and pyrolyzed at 600 ° C for 1 h. After the pyrolysis was completed again, it was cooled to room temperature, washed with deionized water to neutrality, and dried to obtain the sodium hydroxide modified biochar / attapulgite composite material.

[0055] Comparative Example 1

[0056] A method for preparing biochar comprises the following steps:

[0057] Step 1, raw material pretreatment: wash and dry the rice straw, crush it through a 60-mesh sieve, and obtain the rice straw raw material for later use;

[0058] Step 2, pyrolysis: The rice straw raw material obtained in step 1 is placed in a tubular furnace and heated to 600°C under a nitrogen atmosphere at a heating rate of 10°C·min -1 , nitrogen flow rate is 0.5 L·min -1 , and pyrolyze at 600℃ for 1h, cool to room temperature after pyrolysis, grind and pass through a 100-mesh sieve to obtain biochar material for later use;

[0059] Effect Example 1

[0060] The calcium chloride modified biochar / attapulgite composite materials of Examples 1 to 2 and the biochar prepared in Comparative Example 1 were used as heavy metal adsorbents to conduct a heavy metal adsorption experiment under a monovalent heavy metal system. The experimental method is as follows:

[0061] 0.05 g of adsorbent was placed in a 50 mL polyethylene centrifuge tube, and 25 mL of cadmium solution with concentrations of 160, 240 and 320 mg / L or lead solution with concentrations of 200, 400 and 600 mg / L was added. After constant temperature oscillation at 200 r / min at 25 °C for 24 h, centrifugation was performed at 3000 r / min for 5 min, and the supernatant was filtered with a 0.45 μm filter membrane and stored. The concentration of lead or cadmium was determined by inductively coupled plasma optical emission spectroscopy (ICP-OES), and the adsorption removal rate was calculated. The results are shown in Tables 1 and 2.

[0062] Adsorbent for Cd 2+ and Pb 2+ The adsorption amount and removal rate are calculated using formula (1) and formula (2):

[0063]

[0064]

[0065] Where R is the removal rate of lead or cadmium by the composite material (%); C0, C eare the initial concentration and equilibrium concentration of the solution (mg / L), respectively; Q is the equilibrium adsorption capacity (mg / g), V is the volume of the solution (mL), and m is the amount of adsorption material added (g).

[0066] Table 1 Examples 1 to 2 and Comparative Example 1 for Cd 2+ or Pb 2+ The adsorption amount

[0067]

[0068]

[0069] Table 2 Examples 1 to 2 and Comparative Example 1 for Cd 2+ or Pb 2+ Removal rate

[0070]

[0071] It can be seen from Tables 1 and 2 that the calcium chloride modified biochar / attapulgite composite material has a significant effect on the Cd 2+ or Pb 2+ The adsorption and removal rates of Pb were significantly higher than those of biochar materials, and the composite material of Example 1 (the mass ratio of rice straw to attapulgite was 3:1) had a significant effect on the adsorption and removal of Pb 2+ The adsorption capacity of the composite material is higher than that of the composite material in Example 2 (the mass ratio of rice straw to attapulgite is 5:1). 2+ :160mg / L, Pb 2+ : 200 mg / L), Comparative Example 1 (biochar material) for Cd 2+ and Pb 2+ The adsorption capacity of the composite material of Example 2 (rice straw to attapulgite mass ratio of 5:1) was 63.57 mg / g and 99.89 mg / g. 2+ and Pb 2+ The adsorption capacity of Cd is 79.74mg / g and 99.87mg / g. 2+ The removal rate increased from 79.45% in Comparative Example 1 to 99.67% in Example 2. 2+ , there is no significant change. At higher heavy metal concentrations (Cd 2+ :320mg / L, Pb 2+ :600mg / L), Comparative Example 1 (biochar material) for Cd 2+ and Pb 2+ The adsorption capacity of the composite material of Example 2 (rice straw to attapulgite mass ratio of 5:1) was 69.95 mg / g and 171.15 mg / g. 2+ and Pb 2+The adsorption capacity of Cd 2+ The removal rate of Pb increased from 43.72% in Comparative Example 1 to 85.19% in Example 2. 2+ The removal rate increased from 57.05% in Comparative Example 1 to 74.67% in Example 2.

[0072] Effect Example 2:

[0073] The modified biochar / attapulgite composite material before and after sodium hydroxide modification in Example 3 (that is, the calcium chloride modified biochar / attapulgite composite material prepared in step 2 of Example 3 and the sodium hydroxide modified biochar / attapulgite composite material prepared in step 3) was used as a heavy metal adsorbent to conduct heavy metal adsorption experiments under a monovalent heavy metal system and a binary heavy metal system. The experimental method is as follows:

[0074] 0.05g of modified biochar / attapulgite composite material was placed in a 50mL polyethylene centrifuge tube, 25mL of 600mg / L lead and / or 400mg / L cadmium was added, and the mixture was shaken at 200r / min at 25℃ for 24h, centrifuged at 3000r / min for 5min, and the supernatant was filtered with a 0.45μm filter membrane and stored. The concentration of lead or cadmium was determined by inductively coupled plasma emission spectroscopy (ICP-OES). The removal rate was calculated based on the difference in cadmium and lead concentrations before and after adsorption. The results are shown in Table 3.

[0075] Table 3: Effect of sodium hydroxide modification on the adsorption of heavy metals in Example 3

[0076]

[0077] It can be seen from the data in Table 2 that after the composite material is modified with sodium hydroxide, the adsorption of diaphragm and lead in both the mono- and binary systems is significantly improved compared with that before the modification with sodium hydroxide; in the binary system, after the composite material is modified with sodium hydroxide, although the adsorption of diaphragm is lower than that in the mono- system, it still has a high adsorption effect within an acceptable range, and the adsorption of lead is greatly improved compared with that in the mono- system; therefore, the sodium hydroxide-modified biochar / attapulgite composite material prepared by the present invention can maintain a good adsorption effect for cadmium and lead when it is in a multi-metal system of sewage.

[0078] Effect example 3:

[0079] The sodium hydroxide modified biochar / attapulgite composite material of Example 3 was used as a heavy metal adsorbent to conduct an adsorption experiment of heavy metals in a monovalent heavy metal system, and the XRD spectra of the composite material were scanned before and after adsorption. The results are as follows: Figure 2 As shown, the experimental method is as follows:

[0080] 0.05 g of the sodium hydroxide modified biochar / attapulgite composite material was placed in a 50 mL polyethylene centrifuge tube, 25 mL of 600 mg / L lead or 400 mg / L cadmium was added, and the mixture was oscillated at 200 r / min at 25 °C for 24 h, and then centrifuged at 3000 r / min for 5 min. The sodium hydroxide modified biochar / attapulgite composite material after adsorption of lead or cadmium was scanned for XRD patterns.

[0081] From the figure, it can be seen that there are three obvious characteristic peaks in the composite material before adsorption, among which 2θ=29.41° is the characteristic peak of CaCO3, 2θ=20.86° and 2θ=26.64° are both characteristic peaks of SiO2 and are consistent with the crystal structure of attapulgite; 2+ New diffraction peaks appeared after the adsorption, indicating that new mineral phases were generated. The diffraction peaks at 2θ = 19.85°, 24.76°, 34.16° and 40.40° represent Pb3(CO3)2(OH)2. 2+ After that, the diffraction peaks at 2θ = 23.49°, 30.28° and 36.42° also indicate that CdCO3 is generated on the composite material. In addition, the diffraction peaks at 2θ = 29.91° and 30.178° are pyrochloroformite Pb5(PO4)3Cl, which may be Pb 2+ With dissolved anions such as PO4 3~ and Cl ~ These diffraction peaks all have obvious peaks, which indicates that after the introduction of attapulgite, the composite material forms more precipitation during the adsorption process, further enhancing the adsorption of Cd in the solution. 2+ and Pb 2+ removal.

[0082] The above-described embodiments are only preferred embodiments of the present invention, and are not exhaustive of the feasible implementations of the present invention. For those skilled in the art, any obvious changes made thereto without departing from the principles and spirit of the present invention should be considered to be included in the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a modified biochar / attapulgite composite material, characterized in that: The steps include: Step 1, raw material pretreatment: sieve the attapulgite, wash and dry the rice straw, crush and sieve it, then mix the rice straw and attapulgite and immerse them in a calcium chloride solution, and then dry, bake, grind and sieve them in sequence to obtain a rice straw / attapulgite composite raw material; Step 2, pyrolysis: heating the rice straw / attapulgite composite raw material obtained in step 1 to 400-600° C. in an inert gas atmosphere, and pyrolyzing it at 400-600° C. for 1 hour, cooling it to room temperature after the pyrolysis, and then washing it with deionized water to neutrality, drying, grinding, and sieving to obtain a calcium chloride modified biochar / attapulgite composite material; Step 3, sodium hydroxide modification: adding the biochar / attapulgite composite material prepared in step 2 into a sodium hydroxide solution and impregnating it at 40°C. After the impregnation, drying and grinding, then heating to 600°C in an inert gas atmosphere, and pyrolyzing at 600°C for 1 hour, cooling to room temperature after the pyrolysis is completed, washing with deionized water to neutrality, and drying to obtain a sodium hydroxide modified biochar / attapulgite composite material; In step 1, the rice straw and attapulgite are sieved through a 60-mesh standard sieve before and after mixing; The sieve used in step 2 is 100 mesh; In step 1, the mass volume ratio of rice straw, attapulgite and calcium chloride solution is: 1-5 g: 1 g: 100 mL; the concentration of the calcium chloride solution is 2-20 g / 100 mL; In step 1, during the immersion treatment, firstly ultrasonic immersion is performed for 30 minutes to 2 hours, then immersion is performed under stirring for 4 to 6 hours, and then static immersion is performed for 12 to 24 hours; The stirring and dipping is carried out by stirring with a magnetic stirrer; The inert gas is nitrogen; The heating rate in step 2 is 10℃·min -1 , the inert gas flow rate is 0.5 L min -1 ; The heating rate in step 3 is 10℃·min -1 , the inert gas flow rate is 0.2L·min -1 ; In step 3, the concentration of the sodium hydroxide solution is 0.5-4 mol / L, and the amount of the sodium hydroxide solution is 50-100 mL; In step 3, during the immersion treatment, the mixture is first stirred and immersed for 4 to 6 hours, and then allowed to stand and immersed for 12 to 24 hours.

2. The method for preparing a modified biochar / attapulgite composite material according to claim 1, characterized in that: In step 3, the drying temperature is 105° C. and the drying time is 6 to 10 hours.

3. A modified biochar / attapulgite composite material prepared by the preparation method according to any one of claims 1 to 2.

4. Use of the modified biochar / attapulgite composite material as claimed in claim 3 in sewage treatment.