A high temperature resistant organic impregnation sealing material and preparation method thereof
By using multifunctional group monomers and multifunctional group crosslinking agents with emulsification function for high crosslinking, the problem of easy decomposition of existing organic impregnation sealing materials at high temperatures is solved, and the pass rate and use of metal die castings are improved. Lifetime, achieving high temperature stability and safe and environmentally friendly sealing effect.
Patent Information
- Application Number
- CN202210409333.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-19
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-04-19
AI Technical Summary
The existing organic impregnation sealing materials are prone to decomposition and lose weight under high temperature conditions, and their mechanical properties are degraded, making it difficult to meet the long-term use needs of above 250℃.
Multifunctional group monomers, initiators, polymerization inhibitors and multifunctional group crosslinking agents with emulsification functions are used to improve the high temperature resistance of the material and avoid decomposition and performance degradation.
It significantly improves the pass rate and high-temperature service life of metal die castings, enhances the material's high temperature resistance, glue rod media and solvent resistance, reduces toxicity, and is suitable for a variety of high-temperature applications.
Smart Images

Figure CN114874395B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an organic impregnation sealing material and a preparation method thereof, and in particular to a high temperature resistant organic impregnation sealing material and a preparation method thereof. Background Art
[0002] When the casting solidifies from the liquid molten metal, the internal gas cannot escape completely and the metal crystal shrinks unevenly, resulting in a volume shrinkage of 5% to 7%, resulting in pores, shrinkage cavities, pinholes, cracks and looseness, etc., which are invisible to the naked eye. These defects will not damage the structural strength of the casting, but due to micropore leakage, the sealing performance is lost and it becomes waste, causing economic losses. The traditional practice is to rework or scrap the defective parts, causing great waste. The simple, effective and practical vacuum infiltration method is thus produced, which infiltrates and fills various micropores and gaps with liquid impregnation agents by pressurization or vacuum to seal and reinforce, so that the quality and yield rate of the above-mentioned defective mechanical products can be improved. The basic composition of thermosetting organic impregnation sealing materials mainly includes acrylate monomers, initiators and inhibitors. Important components often also include multifunctional cross-linking agents with emulsification functions, chelating agents, fluorescent agents, dyes, etc. The invention patent with application number 201410653840.8 discloses an acrylate type vacuum organic impregnation sealing material, which contains monofunctional monomers, difunctional monomers, emulsifiers, initiators, and inhibitors uniformly mixed at room temperature. The organic impregnation sealing material has low viscosity and low toxicity. The gel time and hardness of the glue stick after curing can meet the needs of industrial production. At the same time, it has a low volume shrinkage rate and is capable of efficiently blocking larger micropores. The efficiency of one-time blocking of micropores is high. It is an ideal organic impregnation sealing material for metal sealing reinforcement. The above-mentioned organic impregnation sealing material is mainly used for the impregnation sealing of conventional metal die-castings. Due to the use of a mixture of monofunctional monomers and difunctional monomers, its high temperature resistance temperature is only about 150°C. It is easy to decompose, lose weight or significantly reduce mechanical properties at higher temperatures for a long time. Therefore, for occasions with high operating temperatures, the above-mentioned organic impregnation sealing material is difficult to achieve the ideal effect.
[0003] Therefore, it is necessary to use appropriate raw materials to ensure the stability and performance of the organic impregnation sealing material, and to make the cured organic impregnation sealing material resistant to high temperatures to meet the needs of long-term use of metal die castings above 250°C. Summary of the invention
[0004] The purpose of the present invention is to solve the problem that the existing organic impregnation sealing material has poor high temperature resistance and to prepare a high temperature resistant organic impregnation sealing material. The material is prepared from a multifunctional monomer, an initiator, an inhibitor, a stabilizer and a multifunctional crosslinking agent with an emulsifying function. The multifunctional monomer and the multifunctional crosslinking agent with an emulsifying function are used to achieve high crosslinking, avoid long-term decomposition at high temperature, weight loss or obvious decrease in mechanical properties, thereby achieving the purpose of improving the qualified rate of metal die castings and the service life under high temperature conditions.
[0005] The present invention provides a high temperature resistant organic impregnation sealing material, which is obtained by stirring and mixing the following components at room temperature in parts by mass:
[0006]
[0007] Among them, the multifunctional monomer is at least one of ethylene glycol diacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, hexanediol diacrylate, 2-butyl-2-ethyl-1,3-propanediol diacrylate, 2--1,3-propanediol diacrylate, 1,4-butanediol diacrylate, triallyl isocyanurate, trihydroxypropane triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, di(trimethylolpropane) tetraacrylate, dipentaerythritol hexaacrylate, and divinylbenzene.
[0008] The initiator is at least one of benzoyl peroxide, lauroyl peroxide, tert-butyl perbenzoate and tert-butyl pervalerate; the inhibitor is at least one of benzoquinone, naphthoquinone, anthraquinone, 2,6-dibutyl-p-cresol, picric acid and 4-methoxyphenol; and the stabilizer is a heavy metal ion chelating agent, preferably ethylenediaminetetraacetic acid.
[0009] The preparation method of the multifunctional cross-linking agent with emulsifying function is as follows:
[0010] (1) Preparation of hydroxyl-containing low molecular weight polyacrylate
[0011] 8-12 parts of pentaerythritol, 80-160 parts of dimethylol propionic acid and 0.5-1.5 parts of p-toluenesulfonic acid are weighed and added to a reactor according to the mass fraction, and melt-reacted at 130-160° C. for 1-3 hours under normal pressure, mechanical stirring and nitrogen protection; then the reactor is sealed, the pressure is reduced to 0.3-0.8 kPa, and the reaction is carried out for 1-3 hours to obtain a low-molecular polyol; finally, 50-80 parts of glycidyl methacrylate and 0.5-1.5 parts of boron trifluoride ether are added to the reactor, and the reaction is carried out at 90° C. for 1-3 hours to obtain a hydroxyl-containing low-molecular polyacrylate;
[0012] (2) Preparation of isocyanate-terminated hydrophilic polyurethane
[0013] According to the mass fraction, 100 parts of polyethylene glycol monomethyl ether are added to the reaction kettle, the temperature is raised to 105-115°C, dehydrated for 1-2 hours under 0.3-0.8 kPa, then cooled to 50-70°C, 30-50 parts of polyisocyanate and 0.5-1 part of catalyst are added, and the reaction is carried out for 2-4 hours to obtain terminal isocyanate hydrophilic polyurethane;
[0014] (3) Preparation of multifunctional cross-linking agent with emulsifying function
[0015] In terms of weight, 100 parts of the hydroxyl-containing low molecular weight polyacrylate prepared in step (1) and 30-60 parts of the isocyanate-terminated hydrophilic polyurethane prepared in step (2) are added to a reaction kettle, the temperature is raised to 50-70° C., and the reaction is carried out for 2-4 hours to obtain a multifunctional cross-linking agent with emulsifying function.
[0016] In the above-mentioned multifunctional cross-linking agent with emulsifying function, the polyisocyanate described in step (2) is at least one of hexamethylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, toluene diisocyanate, and diphenylmethane diisocyanate; and the catalyst is at least one of dibutyltin dilaurate, stannous octoate, triethylamine, N-ethylmorpholine, N-methylmorpholine, N,N-dimethylcyclohexylamine, triethanolamine, and triethylenediamine.
[0017] The organic impregnation sealing material prepared by the invention has an appearance of oily liquid, a viscosity of 10-60 mPa·s, and a high temperature resistance of >250°C.
[0018] Testing method of the organic impregnation sealing material prepared by the present invention:
[0019] 1. Test of viscosity of organic impregnation sealing materials
[0020] According to "GB / T 10247-2008 Viscosity Measurement Method", the viscosity of the organic impregnation sealing material is tested using a digital rotor viscometer.
[0021] 2. Test on high temperature resistance of organic impregnation sealing material impregnated powder metallurgy ring
[0022] The powder metallurgy ring was impregnated with an organic impregnation sealing material. After cleaning, curing and sealing, the powder metallurgy ring was tested underwater at an air pressure of 0.35 MPa before and after being stored in a 250°C hot air environment for 14 days.
[0023] 3. Test on medium and solvent resistance of organic impregnation sealing material glue stick
[0024] Take the inner diameter Put 4 ml of the organic impregnation sealing material to be tested into a clean test tube, place the test tube in a 90℃ water bath for 30 minutes, and after cooling, break the test tube to take out the glue stick; take the glue stick and cut it into Polish the surface with sandpaper; immerse the glue stick in ethylene glycol, brake fluid, engine oil, 10% sulfuric acid and 10% sodium hydroxide at a temperature of 87°C respectively, and observe the appearance of the glue stick after 1000 hours.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1. The organic impregnation sealing material of the present invention utilizes a multifunctional group cross-linking agent with an emulsifying function to chemically react with a multifunctional group monomer in the organic impregnation sealing material during the curing process, which can not only ensure the cleaning performance of the impregnation sealing material, but also form dense cross-linked chemical bonds during the curing process, thereby improving the high temperature resistance, medium resistance and solvent resistance of the glue stick to the impregnated sealing material.
[0027] 2. The organic impregnation sealing material of the present invention utilizes a multifunctional cross-linking agent with an emulsifying function to increase viscosity, accelerate curing speed, and avoid re-flow of the impregnation sealing material in the initial stage of temperature rise curing, thereby effectively improving the impregnation qualification rate of metal die castings.
[0028] 3. The organic impregnation sealing material of the present invention has low toxicity, does not contain volatile substances, is safe and environmentally friendly, and is suitable for the impregnation sealing of automobile and tractor gearboxes, fuel pumps, hydraulic valves, carburetors, oil cylinders, compressors and hydraulic components, enclosed aircraft instruments and their electronic instrument shields, pneumatic parts and various pneumatic instruments, lining kits, valve guides, gears, cams, bearings, clutch friction plates, electric heating elements, heat exchangers, cutting tools, tools and dies and some corrosion-resistant, high-temperature anti-oxidation and high-temperature resistant parts, transformers, capacitors and motors and other electronic devices, wood (sleepers, telephone poles, etc.), ceramics and fiber-plastic synthetic materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Example 1 Photograph of the impregnated powder metallurgy ring before high temperature resistance test
[0030] Figure 2 Example 1 Photograph of the impregnated powder metallurgy ring after high temperature resistance test
[0031] Figure 3 Comparative Example 1 Photograph of the impregnated powder metallurgy ring before high temperature resistance test
[0032] Figure 4 Comparative Example 1: Photograph of the impregnated powder metallurgy ring after high temperature resistance test
[0033] Figure 5 Example 1 Glue stick medium and solvent resistance test Photos before and after the test
[0034] Figure 6 Comparative Example 1: Photos of glue stick medium and solvent resistance test before and after the test DETAILED DESCRIPTION
[0035] The present invention is described below with examples, but is not intended to be limiting of the present invention.
[0036] Example 1
[0037] 1. Preparation of multifunctional cross-linking agent with emulsifying function
[0038] (1) Preparation of hydroxyl-containing low molecular weight polyacrylate
[0039] Weigh 8 parts of pentaerythritol, 80 parts of dimethylol propionic acid and 0.5 parts of p-toluenesulfonic acid and add them to the reactor, and melt and react at 130°C for 1 hour under normal pressure, mechanical stirring and nitrogen protection. Then close the reactor, reduce the pressure to 0.3kPa and react for 1 hour to obtain low molecular weight polyol. Finally, add 50 parts of glycidyl methacrylate and 0.5 parts of boron trifluoride ether, and react at 90°C for 1 hour to obtain hydroxyl-containing low molecular weight polyacrylate.
[0040] (2) Preparation of isocyanate-terminated hydrophilic polyurethane
[0041] Add 100 parts of polyethylene glycol monomethyl ether to the reactor, heat to 105°C, dehydrate at 0.3 kPa for 1 hour, then cool to 50°C, add 30 parts of hexamethylene diisocyanate and 0.5 parts of dibutyltin dilaurate, react for 2 hours to obtain terminal isocyanate hydrophilic polyurethane.
[0042] (3) Preparation of multifunctional cross-linking agent with emulsifying function
[0043] 100 parts of hydroxyl-containing low-molecular-weight polyacrylate and 30 parts of isocyanate-terminated hydrophilic polyurethane were added to a reaction kettle, the temperature was raised to 50° C., and the reaction was carried out for 2 hours to obtain a multifunctional cross-linking agent with emulsifying function.
[0044] 2. Preparation of organic impregnation sealing materials
[0045] In a reaction kettle, 60 parts of ethylene glycol diacrylate, 40 parts of trihydroxypropane triacrylate, 0.2 parts of dibenzoyl peroxide, 0.05 parts of quinone, 0.05 parts of ethylenediaminetetraacetic acid, and 3 parts of the above-mentioned multifunctional cross-linking agent with emulsification function were stirred and mixed uniformly at room temperature to obtain an organic impregnation sealing material.
[0046] Example 2
[0047] 1. Preparation of multifunctional cross-linking agent with emulsifying function
[0048] (1) Preparation of hydroxyl-containing low molecular weight polyacrylate
[0049] Weigh 10 parts of pentaerythritol, 130 parts of dimethylol propionic acid and 1 part of p-toluenesulfonic acid and add them to the reactor, and melt and react at 150°C for 2 hours under normal pressure, mechanical stirring and nitrogen protection. Then close the reactor, reduce the pressure to 0.6kPa and react for 2 hours to obtain low molecular weight polyols. Finally, add 60 parts of glycidyl methacrylate and 1 part of boron trifluoride ether, and react at 90°C for 2 hours to obtain hydroxyl-containing low molecular weight polyacrylate.
[0050] (2) Preparation of isocyanate-terminated hydrophilic polyurethane
[0051] Add 100 parts of polyethylene glycol monomethyl ether to the reactor, heat to 110°C, dehydrate for 1.5 hours at 0.5 kPa, then cool to 60°C, add 40 parts of toluene diisocyanate and 0.7 parts of N,N-dimethylcyclohexylamine, react for 3 hours to obtain terminal isocyanate hydrophilic polyurethane.
[0052] (3) Preparation of multifunctional cross-linking agent with emulsifying function
[0053] 100 parts of hydroxyl-containing low-molecular-weight polyacrylate and 40 parts of isocyanate-terminated hydrophilic polyurethane were added to the reaction kettle, the temperature was raised to 60° C., and the reaction was carried out for 3 hours to obtain a multifunctional cross-linking agent with emulsifying function.
[0054] 2. Preparation of organic impregnation sealing materials
[0055] In a reaction kettle, 30 parts of 1,4-butanediol diacrylate, 30 parts of triallyl isocyanurate, 40 parts of pentaerythritol triacrylate, 0.5 parts of lauroyl peroxide, 0.07 parts of 2,6-dibutylparacresol, 0.07 parts of ethylenediaminetetraacetic acid and 7 parts of the above-mentioned multifunctional cross-linking agent with emulsification function were stirred and mixed uniformly at room temperature to obtain an organic impregnation sealing material.
[0056] Example 3
[0057] 1. Preparation of multifunctional cross-linking agent with emulsifying function
[0058] (1) Preparation of hydroxyl-containing low molecular weight polyacrylate
[0059] Weigh 12 parts of pentaerythritol, 160 parts of dimethylol propionic acid and 1.5 parts of p-toluenesulfonic acid and add them to the reactor, and melt and react at 160°C for 3 hours under normal pressure, mechanical stirring and nitrogen protection. Then close the reactor, reduce the pressure to 0.8 kPa and react for 3 hours to obtain low molecular weight polyols. Finally, add 80 parts of glycidyl methacrylate and 1.5 parts of boron trifluoride ether, and react at 90°C for 3 hours to obtain hydroxyl-containing low molecular weight polyacrylate.
[0060] (2) Preparation of isocyanate-terminated hydrophilic polyurethane
[0061] Add 100 parts of polyethylene glycol monomethyl ether to the reactor, heat to 115°C, dehydrate for 2 hours at 0.8 kPa, then cool to 70°C, add 50 parts of isophorone diisocyanate and 1 part of stannous octoate, react for 4 hours to obtain terminal isocyanate hydrophilic polyurethane.
[0062] (3) Preparation of multifunctional cross-linking agent with emulsifying function
[0063] 100 parts of hydroxyl-containing low-molecular-weight polyacrylate and 60 parts of isocyanate-terminated hydrophilic polyurethane were added to a reaction kettle, the temperature was raised to 70° C., and the reaction was carried out for 4 hours to obtain a multifunctional cross-linking agent with emulsifying function.
[0064] 2. Preparation of organic impregnation sealing materials
[0065] In a reaction kettle, 60 parts of pentaerythritol triacrylate, 40 parts of pentaerythritol tetraacrylate, 1 part of tert-butyl perbenzoate, 0.1 part of 4-methoxyphenol, 0.1 part of ethylenediaminetetraacetic acid, and 10 parts of the above-mentioned multifunctional cross-linking agent with emulsification function are stirred and mixed uniformly at room temperature to obtain an organic impregnation sealing material.
[0066] Comparative Example 1
[0067] In a reaction kettle, 50 parts of lauryl acrylate, 30 parts of ethylene glycol diacrylate, 20 parts of trihydroxypropane triacrylate, 0.2 parts of dibenzoyl peroxide, 0.05 parts of quinone, 0.05 parts of ethylenediaminetetraacetic acid, and 3 parts of allyl alkyl polyoxyethylene ether were stirred and mixed uniformly at room temperature to obtain an organic impregnation sealing material.
[0068] The viscosity of the organic impregnation sealing material of Example 1, Example 2, Example 3 and Comparative Example 1, the high temperature resistance of the impregnated powder metallurgy ring, and the medium and solvent resistance of the glue stick were tested, and the results were as follows:
[0069]
[0070] The organic impregnation sealing material is liquid before curing, and forms a solid with a three-dimensional network cross-linked structure after curing. The high temperature resistance, medium resistance and solvent resistance of the impregnated powder metallurgy rings of Examples 1-3 are significantly improved compared with those of Comparative Example 1. This is because the present invention utilizes a multifunctional group cross-linking agent with an emulsifying function to chemically react with the multifunctional group monomer in the organic impregnation sealing material during the curing process, which can not only ensure the cleaning performance of the impregnation sealing material before curing, but also form dense cross-linked chemical bonds during the curing process, thereby improving the high temperature resistance, medium resistance and solvent resistance of the impregnated sealing material.
Claims
1. A method for preparing an organic impregnation sealing material, comprising the following steps: (1) Preparation of hydroxyl-containing low molecular weight polyacrylate 8 parts of pentaerythritol, 80 parts of dimethylol propionic acid and 0.5 parts of p-toluenesulfonic acid were weighed and added into a reactor, and melted and reacted at 130°C for 1 hour under normal pressure, mechanical stirring and nitrogen protection; then the reactor was sealed, the pressure was reduced to 0.3 kPa and reacted for 1 hour to obtain a low molecular weight polyol; finally, 50 parts of glycidyl methacrylate and 0.5 parts of boron trifluoride ether were added, and the reaction was carried out at 90°C for 1 hour to obtain a hydroxyl-containing low molecular weight polyacrylate; (2) Preparation of isocyanate-terminated hydrophilic polyurethane 100 parts of polyethylene glycol monomethyl ether were added to the reaction kettle, the temperature was raised to 105° C., dehydrated for 1 hour at 0.3 kPa, then cooled to 50° C., 30 parts of hexamethylene diisocyanate and 0.5 parts of dibutyltin dilaurate were added, and the reaction was carried out for 2 hours to obtain an isocyanate-terminated hydrophilic polyurethane; (3) Preparation of multifunctional cross-linking agent with emulsifying function Add 100 parts of hydroxyl-containing low molecular weight polyacrylate and 30 parts of isocyanate-terminated hydrophilic polyurethane into a reaction kettle, heat to 50° C., and react for 2 hours to obtain a multifunctional crosslinking agent with emulsification function; (4) Preparation of organic impregnation sealing materials In a reaction kettle, 60 parts of ethylene glycol diacrylate, 40 parts of trihydroxypropane triacrylate, 0.2 parts of dibenzoyl peroxide, 0.05 parts of quinone, 0.05 parts of ethylenediaminetetraacetic acid, and 3 parts of the above-mentioned multifunctional cross-linking agent with emulsification function were stirred and mixed uniformly at room temperature to obtain an organic impregnation sealing material.