Semiconductive layer composition for high voltage cables

By using a semiconductive resin composition of polyolefin resin, phenolic compounds, thioether compounds, metal stearates, and specific carbon black, the problem of increased volume resistance of semiconductive materials at high temperatures is solved and excellent mechanical strength is achieved and low volume resistance, extending cable life and reducing costs.

CN114901739BActive Publication Date: 2024-10-11HANWHA SOLUTIONS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080089308.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-23
Filing Date
2020-12-15
Publication Date
2024-10-11
Estimated Expiration
2040-12-15

AI Technical Summary

Technical Problem

The volume resistance of existing semi-conductive materials increases at high temperatures, resulting in shortened cable life, increased costs and reduced mechanical strength of conductive materials.

Method used

A semiconductive resin composition using a polyolefin-based resin, a phenolic compound, a thioether compound, a metal stearate, and a specific packing density of carbon black and a cross-linking agent to provide excellent processability and mechanical strength while Maintain low volume resistance at high temperatures.

Benefits of technology

It achieves maintaining low volume resistance at high temperatures, suppressing partial discharge and electrical stress, improving tensile strength and elongation, extending cable life, and reducing costs at the same time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003707723510000091
    Figure BDA0003707723510000091
Patent Text Reader

Abstract

The present invention relates to a semiconductive resin for high voltage cables. Specifically, the present invention relates to a semiconductive resin comprising carbon black, additives, a crosslinking agent, an oxidant and a lubricant on a polyolefin base resin, thereby exhibiting excellent processability and mechanical strength, and particularly exhibiting excellent volume resistance even at high temperatures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The following disclosure relates to a semiconductive resin composition for a high-voltage power cable, and in particular, to a semiconductive resin composition having excellent processability and mechanical strength by containing carbon black, additives, a crosslinking agent, an oxidizing agent, and a lubricant in addition to a polyolefin-based base resin, and in particular, having excellent volume resistance value even at high temperatures. Background Art

[0002] The semiconductive material for the cable is mainly used as a material for an intermediate layer which maintains the life of the cable for a long time by providing the semiconductive material between an insulator layer and a conductor of the cable to prevent the occurrence of space charge and the like.

[0003] As the temperature of a semiconducting material increases, its volume resistance increases. The volume resistance value increases because the conductive network of the semiconducting material is destroyed by the temperature, thereby blocking the path of electrons.

[0004] In order to solve the above problems, the semiconductive material may further contain a conductive material such as graphene, carbon nanotubes and carbon black. However, if a conductive material is further contained, the cost is greatly increased and the mechanical strength of the semiconductive material is also reduced. In particular, due to the protrusion phenomenon caused by the aggregation of the conductive material, it is not easy to have uniform conductivity, so it is necessary to solve this problem. Summary of the invention

[0005] Technical issues

[0006] One embodiment of the present invention is directed to providing a semiconductive composition having excellent volume resistance even at high temperatures, having no defects such as local carbonization, and having excellent tensile strength and elongation by using carbon black.

[0007] Technical Solution

[0008] In one general aspect, a semiconductive resin composition for a cable is provided, comprising: a base resin, a phenol-based compound, a thioether-based compound, a metal stearate, a bulk density of 220 kg / m 3 Up to 380kg / m 3 of carbon black, and a cross-linking agent.

[0009] The base resin may include one or two or more selected from ethylene vinyl acetate, ethylene butyl acrylate, and ethylene ethyl acetate.

[0010] The base resin may have a weight average molecular weight of 1,000 to 1,000,000 g / mol.

[0011] The phenol-based compound may include one or more selected from the following: 2,2'-thiodiethylene-bis-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 4,4'-thio-bis-(2-tert-butyl-5-methylphenol), 1,2-dihydro-2,2,4-trimethylquinoline, diethyl ((3,5-bis-(1,1-dimethylethyl)-4-hydroxyphenyl)methyl) phosphonate, 1,3,4-tris (4-tert-butyl-3 -hydroxy-2,6-dimethylphenyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, tetrakis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris(2,4-di-tert-butylphenyl)phosphate, and N,N'-bis-(3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionyl)hydrazine.

[0012] The thioether-based compound may include one or more selected from the following: dilauryl thiodipropionate, ditridecyl thiodipropionate, dimyristyl thiodipropionate, distearyl disulfide, bis[2-methyl-4-(3-n-dodecylthiopropionyloxy)-5-tert-butylphenyl] sulfide, pentaerythritol-tetrakis-(3-laurylthiopropionate), 1,4-cyclohexanedimethanol, 3,3'-dimethyl thiodipropionate polymer, and distearyl thiodipropionate.

[0013] The crosslinking agent may include one or more selected from the following: di(tert-butylperoxyisopropyl)benzene, 1,1-(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(butylperoxy)valerate, diisopropylbenzene peroxide (DCP), perbutyl peroxide, 1,1-bis(tert-butylperoxy)-diisopropylbenzene, benzoyl peroxide, 2,5-dimethyl-2,5-di-tert-butylperoxyhexane, tert-butyl peroxybenzoate, di-tert-butyl peroxide, and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.

[0014] The metal stearates may include zinc stearate, calcium stearate, aluminum stearate, and magnesium stearate.

[0015] The semiconductive resin composition may have a volume resistance of 600 Ω·cm or less at 135° C.

[0016] The semiconductive resin composition may further comprise a processing aid.

[0017] In another general aspect, there is provided a cable having a semiconductive layer prepared from the above-described semiconductive resin composition.

[0018] Beneficial Effects

[0019] The present invention can provide a semiconductive resin composition having excellent processability, excellent mechanical properties such as tensile strength and elongation, and particularly excellent volume resistance even at high temperatures by using a polyolefin-based resin such as ethylene vinyl acetate and ethylene butyl acetate as a base resin, combining an oxidizing agent having a specific structure, and combining carbon black having specific characteristics. DETAILED DESCRIPTION

[0020] Hereinafter, the present invention will be described in more detail through specific examples or embodiments. The following specific examples and embodiments are only references for describing the present invention in detail, and the present invention is not limited thereto and can be implemented in various forms.

[0021] In addition, unless otherwise defined, all technical and scientific terms have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein are only used to effectively describe certain embodiments and are not intended to limit the present invention.

[0022] Furthermore, the singular forms used in the detailed description and claims are intended to include the plural forms unless the context indicates otherwise.

[0023] Unless explicitly described to the contrary, “including / comprising” any components will be understood to imply the inclusion of other components rather than the exclusion of other components.

[0024] Furthermore, unless specifically limited, the composition of the present invention refers to a weight ratio.

[0025] The present invention provides a semiconductive resin composition suitable for forming an inner semiconductive layer of a medium voltage power cable and will be described in detail below.

[0026] The present invention provides a semiconductive resin composition for a cable, comprising: a polyolefin-based resin such as ethylene vinyl acetate and ethylene butyl acetate as a base resin, a mixed antioxidant of a phenol-based antioxidant and a thioether-based antioxidant, a bulk density of 220 kg / m 3 Up to 380kg / m 3 of carbon black, and a cross-linking agent.

[0027] In addition, the present invention provides a semiconductive resin composition for a cable, comprising: a polyolefin-based resin such as ethylene vinyl acetate and ethylene butyl acetate as a base resin, a mixed antioxidant of a phenol-based antioxidant and a thioether-based antioxidant, a bulk density of 220 kg / m 3 Up to 380kg / m 3 The invention discloses a method for preparing a carbon black composition comprising: forming a carbon black composition, and a cross-linking agent, and further comprising any one or more components selected from a metal ester-based compound and a lubricant.

[0028] A specific example of the present invention includes a semiconductive resin composition for a cable, the semiconductive resin composition comprising, based on 100 parts by weight of a base resin, 0.1 parts by weight to 3 parts by weight of a phenol-based compound, 0.1 parts by weight to 3 parts by weight of a thioether-based compound, 30 parts by weight to 100 parts by weight of a bulk density value of 220 kg / m 3 Up to 380kg / m 3 of carbon black, and 0.1 parts by weight to 5 parts by weight of a cross-linking agent, but the present invention is not particularly limited thereto.

[0029] Specific examples of the present invention include, but are not limited to, a semiconductive resin composition for a cable, wherein the semiconductive resin composition comprises, based on 100 parts by weight of a base resin, 0.1 to 3 parts by weight of a phenol-based compound, 0.1 to 3 parts by weight of a thioether-based compound, 0.1 to 5 parts by weight of a metal stearate, 30 to 100 parts by weight of a bulk density of 220 kg / m 3 Up to 380kg / m 3 of carbon black, and 0.1 to 5 parts by weight of a cross-linking agent.

[0030] The semiconductive resin composition is used for a semiconductive layer between a conductive layer and an insulating layer in a power cable and may have 10 -9 S / cm to 10 3 The resistance is S / cm.

[0031] However, there is a problem in that the volume resistance value increases as the temperature of the semiconductive resin composition increases.

[0032] Since the composition according to the present invention has a low volume resistivity even at high temperatures by containing carbon black having a specific structure, when used for a high-voltage power cable, it has the effects of suppressing partial discharge even at high temperatures, alleviating electrical stress, and also improving tensile strength and elongation.

[0033] Hereinafter, the components of the composition according to the present invention will be described.

[0034] The base resin is a base resin obtained by mixing one or two or more selected from ethylene vinyl acetate, ethylene butyl acrylate and ethylene ethyl acetate. The weight average molecular weight of the example of the base resin may preferably be 1000 g / mol to 1000000 g / mol, more preferably 5000 g / mol to 800000 g / mol, and still more preferably 10000 g / mol to 600000 g / mol, but is not limited thereto.

[0035] Furthermore, the content ratio of butyl acetate in ethylene butyl acetate may be 10% to 30%, preferably 15% to 25%, and more preferably 16% to 20%.

[0036] The above components are used alone or mixed with each other to prepare a base resin, and the obtained base resin is combined with a mixed antioxidant and carbon black to prepare a semiconductive resin composition having excellent processability, flexibility and durability. In addition, the base resin is suitable for materials such as a semiconductive resin for power cables that require excellent adhesion to conductors and insulators.

[0037] Hereinafter, the carbon black of the present invention will be described. The bulk density of the carbon black of the present invention may be 220 kg / m 3 Up to 380kg / m 3 , preferably 300kg / m 3 Up to 375kg / m 3 , more preferably 300kg / m 3 Up to 330kg / m 3 . When the bulk density of carbon black is within the above range, the effect of the present invention can be significantly improved. In the present invention, the particles of carbon black may also be nanoscale, and preferably 10 nm to 100 nm. When the bulk density of carbon black in the same composition has the above value, the composition significantly suppresses the increase in volume resistance, and particularly has very excellent volume resistance at 90°C or higher. For example, when the bulk density of the present invention is within the above range, the volume resistance values ​​at 90°C or higher in the embodiments and comparative examples have a difference of 2 to 20 times. This difference may result in an increase in local resistance in the power cable due to the high resistance value, and accumulate electrical stress. The volume resistance may be 10Ω·cm to 600Ω·cm, preferably 10Ω·cm to 100Ω·cm, and more preferably 10Ω·cm to 60Ω·cm, but is not limited thereto.

[0038] In addition, the use of carbon black can improve the conductivity of the semiconductive composition and improve the surface smoothness of the semiconductive layer, because the uniform dispersion on the surface of the semiconductive layer can reduce the difference in shrinkage and expansion rate between adjacent areas on the surface of the semiconductive layer. In the present invention, when the bulk density of carbon black is higher than the above range, the effect of the present invention cannot be achieved, from which the unexpected effect of the above range can be seen.

[0039] Therefore, when the composition according to the present invention is used, the volume resistance to each temperature can be reduced without increasing the content of carbon black in the semiconductive resin composition, and the tensile strength and elongation can also be improved.

[0040] Tensile strength can be 150kg / m 2 Up to 400kg / m 2, preferably 200kg / m 2 Up to 300kg / m 2 , more preferably 220kg / m 2 Up to 240kg / m 2 , but not limited to this.

[0041] In addition, the elongation may be 150% to 400%, preferably 230% to 300%, and more preferably 245% to 280%, but is not limited thereto.

[0042] Since high mechanical values ​​are required due to the properties of high-voltage power cables, the use of a composition according to the invention has the great advantage of having high mechanical properties and a low volume resistance for each temperature.

[0043] Furthermore, the composition according to the present invention can be prepared by adding a conductive material containing the carbon black according to the present invention or other carbon black.

[0044] Hereinafter, the mixed antioxidant of the present invention will be described.

[0045] Use of the mixed antioxidant of the present invention is preferred because, even if not specifically shown as an example, the mixed antioxidant of the present invention can prevent significant local carbonization compared with the use of either or other antioxidants alone.

[0046] In one aspect of the present invention, the phenol-based compound may include one or more selected from the following: 2,2'-thiodiethylene-bis-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 4,4'-thio-bis-(2-tert-butyl-5-methylphenol), 1,2-dihydro-2,2,4-trimethylquinoline, diethyl ((3,5-bis-(1,1-dimethylethyl)-4-hydroxyphenyl)methyl)phosphonate, 1,3,4-tris (4- tert-butyl-3-hydroxy-2,6-dimethylphenyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, tetrakis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris(2,4-di-tert-butylphenyl)phosphate, and N,N'-bis-(3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionyl)hydrazine.

[0047] The thioether-based compound of the present invention may include one or more selected from the group consisting of dilauryl thiodipropionate, ditridecyl thiodipropionate, dimyristyl thiodipropionate, dioctadecyl disulfide, bis[2-methyl-4-(3-n-dodecylthiopropionyloxy)-5-tert-butylphenyl] sulfide, pentaerythritol-tetrakis-(3-laurylthiopropionate), 1,4-cyclohexanedimethanol, 3,3'-dimethyl thiodipropionate polymer, and distearyl thiodipropionate.

[0048] The composition ratio of the mixed antioxidant may be, for example, 1:1, but is not limited thereto. In addition, the mixed antioxidant may be used within 0.1 parts by weight to 6 parts by weight based on the total composition of the present invention, but is not necessarily limited thereto.

[0049] The use of the mixed antioxidant can improve the processability of the polymer by processing the semiconductive resin composition, as well as prevent oxidation of the polymer.

[0050] The composition according to the present invention may include a metal stearate, specifically, zinc stearate, calcium stearate, aluminum stearate, and magnesium stearate, preferably calcium stearate and zinc stearate, more preferably zinc stearate, but the metal stearate is not limited thereto.

[0051] The metal stearate may be included in an amount of 0.1 to 5 parts by weight, for example 1 to 3 parts by weight, based on 100 parts by weight of ethylene vinyl acetate.

[0052] The slugging phenomenon of the polymer can be minimized by further including a metal stearate. The semiconductive layer of the present invention manufactured by the metal stearate in the above content does not produce protrusions on the surface and can impart excellent surface properties. In addition, since the metal stearate improves the fluidity of the conductive resin composition, when the conductive resin composition is molded, the change in conductivity caused by stretching can be minimized.

[0053] In one aspect of the present invention, the crosslinking agent may include one or more selected from the following: di(tert-butylperoxyisopropyl)benzene, 1,1-(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(butylperoxy)valerate, diisopropylbenzene peroxide, perbutyl peroxide, 1,1-bis(tert-butylperoxy)-diisopropylbenzene, benzoyl peroxide, 2,5-dimethyl-2,5-di-tert-butylperoxyhexane, tert-butyl peroxybenzoate, di-tert-butyl peroxide, and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.

[0054] The crosslinkable polymer is crosslinked using a crosslinking agent. One suitable method is to impregnate the polymer powder or polymer pellets with the crosslinking agent. The mixture is then heated to a temperature above the decomposition temperature of the crosslinking agent. Suitable cross-linking agents that can be used may include, but are not limited to, for example, di(tert-butylperoxyisopropyl)benzene, 1,1-(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(butylperoxy)valerate, dicumyl peroxide (DCP), perbutyl peroxide, 1,1-bis(tert-butylperoxy)-diisopropylbenzene, benzoyl peroxide, 2,5-dimethyl-2,5-di-tert-butylperoxyhexane, tert-butyl peroxybenzoate, di-tert-butyl peroxide, and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, preferably di(tert-butylperoxyisopropyl)benzene, perbutyl peroxide, 1,1-(tert-butylperoxy)-3,3,5-trimethylcyclohexane, benzoyl peroxide, and dicumyl peroxide, more preferably dicumyl peroxide and perbutyl peroxide.

[0055] The crosslinking agent may be included in an amount of 0.1 to 5 parts by weight in 100 parts by weight of ethylene vinyl acetate. If the crosslinking agent is included in an amount of less than 0.1 parts by weight, crosslinking may not be sufficiently performed and final physical properties may be deteriorated. If the crosslinking agent is included in an amount of 5 parts by weight or more, moldability may be deteriorated.

[0056] When the crosslinking agent is included within the above range, crosslinking properties of the base resin are improved and dispersibility of the additive is improved, so that lifespan may be increased when applying electric power lines to the semiconductive layer.

[0057] The semiconductive resin composition may further include a processing aid. The processing aid may include, but is not limited to, montan wax, fatty acid esters, triglycerides or partial esters thereof, glycerides, polyethylene wax, paraffin wax, metal soap-based lubricants, amide-based lubricants, etc., preferably fatty acid esters, triglycerides or partial esters thereof, and polyethylene wax.

[0058] Since the processing aid is further included, the composition can improve strippability from a conductor and reduce extrusion load.

[0059] The semiconductive resin composition can be easily used as a semiconductive layer of a cable, and in particular, can have a low volume resistance value even at high temperatures. Therefore, the semiconductive resin composition is suitable for a semiconductive layer of a high voltage cable.

[0060] When high voltage power flows from the power cable to the conductor, partial discharge flows into the semiconductive layer, which may cause a temperature increase due to volume resistance generated in the semiconductive layer.

[0061] As the temperature of the semiconductive layer increases, the volume resistance value further increases. Therefore, the above effect leads to a shortened life of the power cable. Since the semiconductive resin composition for a cable according to the present invention has a low volume resistance even at a high temperature, the increase in volume resistance due to an increase in temperature is suppressed, so that the semiconductive resin composition is effectively used for a power cable.

[0062] Embodiments of the invention

[0063] Hereinafter, the present invention will be described in more detail based on Examples and Comparative Examples. However, the following Examples and Comparative Examples are examples for describing the present invention in more detail, and the present invention is not limited to the following Examples and Comparative Examples.

[0064] [Example 1]

[0065] The semiconductive resin composition was prepared by kneading in a Banbury mixer at 150° C. for 30 minutes. Based on 100 parts by weight of an ethylene ethyl acrylate copolymer having a butyl acrylate content of 17 mol% and a melt index (ASTM1238, 190° C., 2.16 kgf) of 7.0 g / 10 minutes, 0.1 parts by weight of 1,2-dihydro-2,2,4-trimethylquinoline (NaugardSuperQ, Miwon Commercial Co., Ltd.), 0.15 parts by weight of dimyristyl thiodipropionate (Mianto-S, Miwon Commercial Co., Ltd.), 53.83 parts by weight of a bulk density of 325 Kg / m 3 Carbon black (420B, HIBLACK), and 1.35 parts by weight of zinc stearate were kneaded at 100° C. for 30 minutes. After the kneaded mixture was passed through a roll mill and a crusher to produce a sheet type, a crosslinking agent (di(tert-butylperoxyisopropyl)benzene, AkzoNobel) was further added in a Brabender mixer, and the mixture was immersed at 75° C. for 10 minutes at 40 rpm and aged in an oven at 70° C. for 8 hours to prepare a semiconductive compound. The tensile strength and elongation (ATSM D 638, 250 mm / min) of the prepared compound composition were measured, and the results are shown in Table 1, and the volume resistivity (ASTM D991) of the prepared compound composition was measured, and the results are shown in Table 2.

[0066] [Example 2]

[0067] Example 2 was carried out in the same manner as in Example 1, except that a bulk density of 375 Kg / m 3 Carbon black (XC200, VULCAN) was used as carbon black.

[0068] [Example 3]

[0069] Example 3 was carried out in the same manner as in Example 1, except that a bulk density of 306 Kg / m 3 Carbon black (XC500, VULCAN) was used as carbon black.

[0070] [Comparative Example 1]

[0071] Comparative Example 1 was carried out in the same manner as in Example 1, except that a bulk density of 395 kg / m 3 Carbon black (150B, HIBLACK) was used as carbon black.

[0072] [Table 1]

[0073] Elongation(%) <![CDATA[Tensile strength (kg / m 2 )]]> Example 1 247 234.3 Example 2 274 220.8 Example 3 260 223.1 Comparative Example 1 259 216.3

[0074] [Table 2]

[0075]

[0076] It can be determined that the elongation and tensile strength values ​​vary depending on the type of carbon black described in Table 1 above.

[0077] It was confirmed that all the Examples had higher tensile strength than the Comparative Examples, and from the above results, the semiconductive resin composition had excellent mechanical strength.

[0078] Furthermore, when the volume resistance at each temperature in Table 2 was determined, the example had a lower volume resistance in the entire temperature range than the comparative example.

[0079] From this, it was determined that the difference in bulk density of carbon black produced a remarkable effect with excellent resistance value not only on mechanical properties such as elongation and tensile strength but also on volume resistance at each temperature.

[0080] In the above, although the present invention has been described by specific matters and limited embodiments, they are only provided to help understand the present invention more generally. Therefore, the present invention is not limited to the exemplary embodiments. Those skilled in the art to which the present invention belongs can make various modifications and changes according to this description.

[0081] Therefore, the spirit of the present invention should not be limited to the above-described embodiments, but the claims and all modifications equal or equivalent to the claims are intended to fall within the scope and spirit of the present invention.

Claims

1. A semiconductive resin composition for a cable, comprising: a base resin, a first antioxidant, a second antioxidant, a metal stearate, a bulk density of 300 kg / m 3 Up to 330kg / m 3 of carbon black, and crosslinking agent, wherein the base resin is one or both selected from ethylene butyl acrylate and ethylene ethyl ester, wherein the first antioxidant is one or more selected from the following: 4,4'-thio-bis-(2-tert-butyl-5-methylphenol), 1,2-dihydro-2,2,4-trimethylquinoline, diethyl ((3,5-bis-(1,1-dimethylethyl)-4-hydroxyphenyl)methyl)phosphonate, 1,3,4-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzene)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, tetrakis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane, tris(2,4-di-tert-butylphenyl)phosphate, and N,N'-bis-(3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionyl)hydrazine, and wherein the second antioxidant is one or more selected from the following: ditridecyl thiodipropionate, dimyristyl thiodipropionate, distearyl disulfide, bis[2-methyl-4-(3-n-dodecylthiopropionyloxy)-5-tert-butylphenyl] sulfide, pentaerythritol-tetrakis-(3-laurylthiopropionate), 1,4-cyclohexanedimethanol, 3,3'-dimethyl thiodipropionate polymer, and distearyl thiodipropionate, and Wherein, based on 100 parts by weight of the base resin, the composition comprises 0.1 to 3 parts by weight of the first antioxidant, 0.1 to 3 parts by weight of the second antioxidant, 0.1 to 5 parts by weight of the metal stearate, 30 to 100 parts by weight of the carbon black, and 0.1 to 5 parts by weight of the crosslinking agent. 2 . The semiconductive resin composition according to claim 1 , wherein the base resin has a weight average molecular weight of 1,000 to 1,000,000 g / mol.

3. The semiconductive resin composition according to claim 1, wherein the crosslinking agent comprises one or more selected from the group consisting of di(tert-butylperoxyisopropyl)benzene, 1,1-(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(butylperoxy)valerate, dicumyl peroxide (DCP), perbutyl peroxide, 1,1-bis(tert-butylperoxy)-diisopropylbenzene, benzoyl peroxide, 2,5-dimethyl-2,5-di-tert-butylperoxyhexane, tert-butyl peroxybenzoate, di-tert-butyl peroxide, and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane. 4 . The semiconductive resin composition according to claim 1 , wherein the metal stearate comprises zinc stearate, calcium stearate, aluminum stearate, and magnesium stearate. 5 . The semiconductive resin composition according to claim 1 , wherein the semiconductive resin composition has a volume resistance of 600 Ω·cm or less at 135° C. The semiconductive resin composition according to claim 1 , further comprising a processing aid.

7. A cable having a semiconductive layer prepared from the semiconductive resin composition for a cable according to any one of claims 1 to 6.