Blade repair method, blade and gas turbine

Through the surfacing technology of two-layer welding materials, combined with high welding properties and high temperature strength materials, the problem of blades being prone to cracking again after brazing repair is solved, and crack suppression and thermal fatigue strength are improved in operation and welding operations. .

CN114929999BActive Publication Date: 2024-12-06MITSUBISHI HEAVY IND LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080088873.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-23
Filing Date
2020-12-17
Publication Date
2024-12-06
Estimated Expiration
2040-12-17

AI Technical Summary

Technical Problem

The prior art After brazing and repair, the strength of the blades is insufficient and cracks are easily generated again, especially during operation and welding operations.

Method used

Using the surfacing technology of two-layer welding materials, first use the first welding material with high welding properties but low high temperature strength to fill the first area, and then use the second welding material with high temperature strength but low welding properties to fill the second area. The thickness of the second area is controlled to be 1.0 mm or more and 3.0 mm or less to suppress the occurrence of cracks.

Benefits of technology

It effectively suppresses the generation of cracks during operation and welding operations, improves the heat fatigue strength of the repaired part, and extends the service life of the repaired parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114929999B_ABST
    Figure CN114929999B_ABST
Patent Text Reader

Abstract

The present invention provides a method for repairing a blade, the method comprising: a first welding step, in which a first area that constitutes a notch and is located on the blade body side is filled with the first welding material by surfacing welding using a first welding material; and a second welding step, in which, after the first welding step, a second area that constitutes a notch and is located on the end face side of a platform is filled with the second welding material by surfacing welding using a second welding material, the high temperature strength of the second welding material is higher than the high temperature strength of the first welding material, the weldability of the first welding material is higher than the weldability of the second welding material, and the second area is an area ranging from the end face of the platform toward the blade body in a range of more than 1.0 mm and less than 3.0 mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a blade repair method, a blade and a gas turbine.

[0002] This application claims priority from patent application No. 2019-231773 filed in Japan on December 23, 2019, and the contents are incorporated herein by reference. Background Art

[0003] Gas turbines have moving blades and stationary blades as high-temperature parts. The moving blades and stationary blades are exposed to a high-temperature combustion gas environment, which causes material degradation. As a result, cracks may sometimes occur in the outer periphery of the platform constituting the moving blade or the platform constituting the stationary blade.

[0004] Patent Document 1 discloses that a repaired portion of a base material having cracks is filled with a brazing repair material and subjected to diffusion heat treatment to thereby integrally bond the brazing repair material to the repaired portion to repair the repaired portion.

[0005] Previous technical literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2009-285664 Summary of the invention

[0008] Technical issues to be solved by the invention

[0009] However, when brazing repair is performed, since the strength of the brazing material is low, the strength is insufficient even if the repair is performed, so there is a possibility that cracks etc. will occur again.

[0010] Therefore, an object of the present invention is to provide a blade repair method, a blade, and a gas turbine capable of suppressing cracks from being generated on the end surface of the platform during operation and suppressing cracks from being generated during welding work.

[0011] Means for solving technical problems

[0012] In order to solve the above-mentioned problems, in the blade repair method involved in the present invention, the blade comprises: a blade body, which is arranged in a combustion gas flow path where the combustion gas flows and is in the shape of a blade; and a platform, which is arranged at one end of the blade body in the blade height direction and extends in the blade width direction including a direction perpendicular to the blade height direction to partition a part of the edge of the combustion gas flow path. The repair method is for repairing a crack formed from the end face of the platform in the blade width direction toward the blade body. The repair method includes: a notch forming step, forming the notch, the notch is formed from the end face of the platform toward the crack by removing the crack-containing area in the platform before repair. The blade body is recessed and includes a first area located on the blade body side and a second area located on the end face side closer to the platform than the first area; a first welding process, by using a first welding material for surfacing, the first area is filled with the first welding material; and a second welding process, after the first welding process, by using a second welding material for surfacing, the second area is filled with the second welding material, the high temperature strength of the second welding material is higher than the high temperature strength of the first welding material, the weldability of the first welding material is higher than the weldability of the second welding material, and the second area is an area in the range of 1.0 mm or more and 3.0 mm or less from the end face of the platform toward the blade body.

[0013] Effects of the Invention

[0014] According to the present invention, it is possible to suppress the reoccurrence of cracks in the repaired portion. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 It is a schematic cross-sectional view of a gas turbine according to a first embodiment of the present invention.

[0016] Figure 2 yes Figure 1 A perspective view of a repaired turbine rotor blade is shown.

[0017] Figure 3 Cut along line A1-A2 Figure 2 A cross-sectional view of a repaired turbine rotor blade is shown.

[0018] Figure 4 Is magnification Figure 2 A top view of the portion of the platform enclosed by area B is shown.

[0019] Figure 5 It means from Figure 4 The notch portion shown is a plan view showing a state where the first weld portion and the second weld portion are removed.

[0020] Figure 6Cut along the C1-C2 line Figure 4 A cross-sectional view of the structure shown.

[0021] Figure 7 This is a flowchart for explaining a process for determining whether to implement the blade (turbine blade) repair method according to the first embodiment of the present invention.

[0022] Figure 8 This is a top view of an enlarged portion of the platform where a crack has occurred.

[0023] Fig. 9 This is a flowchart for explaining the method for repairing a blade (turbine blade) according to the first embodiment of the present invention.

[0024] Fig.10 It is a schematic representation of the removal of the components Figure 8 A top view of the state of the thermal barrier coating of the platform is shown.

[0025] Fig.11 It is schematically represented in Fig.10 This is a plan view showing a state in which a notch is formed on the platform.

[0026] Fig.12 It is a schematic representation of Fig.11 The notch portion shown in the figure has its tip facing downward and is in a state where a first welding material is build-up welded in a first region of the notch portion.

[0027] Fig.13 Cut along the F1-F2 line Fig.12 A cross-sectional view of the structure shown.

[0028] Fig.14 It is schematically represented in Fig.11 FIG. 1 is a diagram showing a state where the second welding material is build-up welded in the second region of the notch portion.

[0029] Fig.15 Cut along the G1-G2 line Fig.14 A cross-sectional view of the structure shown.

[0030] Fig.16 It is a cross-sectional view of the first region of the platform after finishing.

[0031] Fig.17 It is a cross-sectional view of the second region of the platform after finishing. DETAILED DESCRIPTION

[0032] [First embodiment]

[0033] refer to Figure 1 A gas turbine 10 according to the first embodiment will be described. Figure 1In FIG. 1 , for convenience of explanation, a generator 15 which is not a component of the gas turbine 10 is also shown.

[0034] exist Figure 1 In the figure, Ar represents the axis of the rotor 30 (hereinafter referred to as the “axis Ar”), Dc represents the circumferential direction of the rotor 30 (hereinafter referred to as the “circumferential direction Dc”), Dr represents the radial direction of the rotor 30 (hereinafter referred to as the “radial direction Dr”), Dri represents the radial inner side of the radial direction Dr close to the axis Ar (hereinafter referred to as the “radial inner side Dri”), and Dro represents the radial outer side in the opposite direction of the radial inner side Dri and away from the axis Ar (hereinafter referred to as the “radial outer side Dro”).

[0035] The axis Ar is also the axis of the turbine rotor 31. Figure 1 The arrows shown indicate the direction of gas flow.

[0036] In the first embodiment, as an example, the case where the plurality of turbine blades 37 include the repaired turbine blade 37B is described below.

[0037] The crack 69 generated in the platform 47 on the ventral side of the turbine blade 37B is repaired. The main cause of the crack 69 is thermal fatigue caused by repetition of thermal stress generated during the start-up, operation, and shutdown of the gas turbine 10.

[0038] (Overall structure of gas turbine)

[0039] The gas turbine 10 includes a compressor 11 , a combustor 12 , and a turbine 13 .

[0040] The compressor 11 includes a compressor rotor 21 , a plurality of compressor blade stages 23 , a compressor housing 24 , and a plurality of compressor stationary blade stages 25 .

[0041] The compressor rotor 21 is a rotating body formed into a cylindrical shape. The compressor rotor 21 has an outer peripheral surface 21a. The compressor rotor 21 is connected to a turbine rotor 31 constituting the turbine 13. The compressor rotor 21 and the turbine rotor 31 together constitute the rotor 30. The compressor rotor 21 rotates around the axis Ar.

[0042] The plurality of compressor blade layers 23 are arranged at intervals in the direction of the axis Ar on the outer peripheral surface 21a of the compressor rotor 21. The compressor blade layer 23 has a plurality of compressor blades 27 arranged at intervals in the circumferential direction Dc of the outer peripheral surface 21a of the compressor rotor 21. The plurality of compressor blades 27 rotate together with the compressor rotor 21.

[0043] The compressor housing 24 accommodates the compressor rotor 21 and the plurality of compressor blade layers 23 with a gap therebetween at the tip ends of the plurality of compressor blades 27 .

[0044] The compressor housing 24 is a cylindrical member having the axis Ar as a central axis. The compressor housing 24 has an inner peripheral surface 24a.

[0045] The plurality of compressor vane layers 25 are arranged at intervals in the axis Ar direction on the inner peripheral surface 24a of the compressor housing 24. When viewed from the axis Ar direction, the plurality of compressor vane layers 25 are arranged so that the compressor moving blade layers 23 and the compressor vane layers 25 are alternately arranged.

[0046] The compressor vane layer 25 includes a plurality of compressor vanes 28 arranged at intervals in the circumferential direction Dc of the inner peripheral surface 24 a of the compressor housing 24 .

[0047] The compressor 11 configured as described above sucks in combustion air to generate compressed air. The compressed air generated by the compressor 11 flows into the combustor 12 .

[0048] The combustor 12 is provided between the compressor 11 and the turbine 13. The combustor 12 generates combustion gas by injecting fuel into the compressed air generated by the compressor 11. The high-temperature combustion gas generated by the combustor 12 is introduced into the turbine 13 to drive the turbine 13.

[0049] The turbine 13 includes a turbine rotor 31 , a plurality of turbine blade stages 33 , a turbine casing 34 , and a plurality of turbine stationary blade stages 35 .

[0050] The turbine rotor 31 is a rotating body formed into a cylindrical shape. The turbine rotor 31 has an outer peripheral surface 31a. The turbine rotor 31 rotates around the axis Ar.

[0051] The plurality of turbine blade layers 33 are arranged at intervals in the direction of the axis Ar on the outer peripheral surface 31a of the turbine rotor 31. The turbine blade layer 33 includes a plurality of turbine blades 37 arranged at intervals in the circumferential direction Dc of the outer peripheral surface 31a of the turbine rotor 31. The plurality of turbine blades 37 rotate together with the turbine rotor 31.

[0052] The plurality of turbine blades 37 include turbine blades 37A that have not been repaired and turbine blades 37B in which portions of the cracks 69 have been repaired.

[0053] In addition, refer to Figure 2 to Figure 6 The specific structure of the repaired turbine blade 37B will be described later.

[0054] The turbine housing 34 accommodates the turbine rotor 31 and the plurality of turbine blade stages 33 with a gap therebetween at the tip ends of the plurality of turbine blades 37 .

[0055] The turbine housing 34 is a cylindrical member having the axis Ar as a central axis. The turbine housing 34 has an inner peripheral surface 34a.

[0056] An annular space in which the turbine blades 37 and the turbine vanes 38 are arranged in the direction of the axis Ar between the turbine casing 34 and the turbine rotor 31 functions as a combustion gas flow path 41 through which the combustion gas generated by the combustor 12 flows.

[0057] The plurality of turbine blade layers 35 are arranged at intervals in the axis Ar direction on the inner peripheral surface 34a of the turbine housing 34. When viewed from the axis Ar direction, the plurality of turbine blade layers 35 are arranged so that the turbine moving blade layers 33 and the turbine blade layers 35 are alternately arranged.

[0058] The turbine vane layer 35 includes a plurality of turbine vanes 38 arranged at intervals in the circumferential direction Dc of the inner peripheral surface 34 a of the turbine housing 34 .

[0059] (Overall structure of the repaired turbine blade)

[0060] refer to Figure 2 to Figure 6 The structure of the turbine rotor blade 37B (blade) to be repaired will be described. Figure 2 In FIG. 4 , Dwh represents the height direction of the blade body 45 (hereinafter referred to as the “blade height direction Dwh”), and Dwp represents the blade width direction including a component perpendicular to the blade height direction Dwh (hereinafter referred to as the “blade width direction Dwp”). Figure 5 In FIG. 1 , for convenience of explanation, a crack 69 removed from the platform body 62 by forming the notch portion 63 is shown by a dotted line.

[0061] exist Figure 2 In, with Figure 1 The same structural parts of the structures shown are marked with the same symbols. Figure 2 to Figure 6 In the drawings, the same symbols are given to the same structural parts.

[0062] The turbine blade 37B includes a blade body 45 , a repaired platform 47 , a fillet portion 48 , and a shaft mounting portion 49 .

[0063] (Structure of the blade body)

[0064] The blade body 45 is formed in a blade shape and is arranged in the combustion gas flow path 41 (see FIG. Figure 1 )Inside.

[0065] The blade body 45 has a leading edge 45A, a trailing edge 45B, a pressure surface side blade wall 51 , a suction surface side blade wall 52 , a top plate 54 , and a refrigerant flow path (not shown).

[0066] The pressure surface side blade wall 51 and the suction surface side blade wall 52 extend from the gas passage surface 47a of the platform 47 in the radial direction Dr (blade height direction Dwh). The pressure surface side blade wall 51 and the suction surface side blade wall 52 are respectively set to a curved shape. The pressure surface side blade wall 51 and the suction surface side blade wall 52 are connected to each other through the leading edge 45A and the trailing edge 45B.

[0067] The pressure surface side blade wall 51 has a pressure surface 51 a which is the outer surface of the pressure surface side blade wall 51. The suction surface side blade wall 52 has a suction surface 52 a which is the outer peripheral surface of the suction surface side blade wall 52.

[0068] The top plate 54 is a plate-shaped member, and is provided at the tip end portion arranged on the radially outer side Dro among the end portions (specifically, the base end portion and the tip end portion) of the pressure-side blade wall 51 and the suction-side blade wall 52.

[0069] A refrigerant flow path (not shown) is formed inside the blade body 45. A cooling medium for cooling the blade body 45 disposed in a high temperature environment flows through the refrigerant flow path (not shown).

[0070] The blade body 45 having the above-described structure is configured to include a metal base 57 having the shape of the blade body 45 and a thermal barrier coating 58 (Thermal Barrier Coating layer (TBC layer)) formed on the surface of the metal base 57 .

[0071] The metal substrate 57 is made of a metal material having excellent heat resistance. As the metal material used for the metal substrate 57, for example, a Ni-based superalloy can be used.

[0072] The thermal barrier coating 58 has a function of protecting the metal substrate 57 from high-temperature combustion gas.

[0073] (The overall structure of the repaired platform)

[0074] The platform 47 is provided at the base end of the blade body 45 in the blade height direction Dwh. The platform 47 has a gas passage surface 47a on which the base end of the blade body 45 is arranged. Figure 1 A portion of the edge of the combustion gas flow path 41 is shown.

[0075] The platform 47 includes a platform body 62 , a notch portion 63 , a first weld portion 65 , a second weld portion 66 , and a thermal barrier coating 58 .

[0076] (Structure of the platform body)

[0077] The platform body 62 extends in the blade width direction Dwp including a direction perpendicular to the blade height direction Dwh. The platform body 62 has an end face 62a disposed on the pressure surface 51a side in the blade width direction Dwp, a surface 62b disposed on the blade body 45 side, and another surface 62c disposed on the opposite side of the surface 62b (on the shaft mounting portion 49 side).

[0078] The crack 69 generated in the platform 47 is formed in the direction from the end surface 62a toward the blade body 45. Furthermore, the crack 69 is likely to be repeatedly generated at a specific position of the end surface 62a of the platform body 62.

[0079] The platform main body 62 having the above-described structure is composed of a metal base material 57 in the shape of the platform 47 .

[0080] (Structure of the notch)

[0081] The notch portion 63 is formed in the platform body 62 by removing a crack-containing region P where the crack 69 is generated in the platform body 62. The notch portion 63 is formed so as to be recessed from the end surface 62a of the platform body 62 toward the blade body 45.

[0082] The notch portion 63 is recessed from the end surface 62 a of the platform body 62 toward the blade body 45 , and has a first region 71 and a second region 72 .

[0083] The first region 71 is a region of the notch portion 63 that is disposed on the blade body 45 side.

[0084] The first region 71 has a penetration portion 74 and a non-penetration portion 75. The penetration portion 74 is a space formed by penetrating a region where the slit 69 is formed in the platform body 62 constituting the gas passage surface 47a in the thickness direction of the platform body 62 (blade height direction Dwh).

[0085] The non-penetrating portion 75 is a space formed by cutting a portion of the platform body 62 located on the blade body 45 side and leaving a portion located on the shaft mounting portion 49 side. The non-penetrating portion 75 and the penetrating portion 74 are formed integrally.

[0086] The second region 72 is arranged on the side closer to the end surface 62a of the platform body 62 than the first region 71. The second region 72 and the first region 71 are formed integrally.

[0087] The length L2 of the second region 72 in the direction from the end surface 62 a toward the blade body 45 is configured to be considerably shorter than the length L1 of the first region 71 in the direction from the end surface 62 a toward the blade body 45 .

[0088] (Structure of the first welded portion and the second welded portion)

[0089] The first weld portion 65 is disposed so as to fill the first region 71. The first weld portion 65 has one surface 65a and the other surface 65b.

[0090] One surface 65a is arranged on the blade body 45 side and is flush with one surface 62b of the platform body 62. The other surface 65b is arranged on the opposite side (the shaft attachment portion 49 side) of the one surface 65a and is flush with the other surface of the platform body 62.

[0091] The first weld portion 65 is formed of a first welding material 81 used when the first region 71 is built-up welded.

[0092] The second weld portion 66 is arranged so as to fill the second region 72. The second weld portion 66 is composed of the second welding material 82 used when cladding the second region 72. That is, the notch portion 63 is filled by the first weld portion 65 and the second weld portion 66. The second weld portion 66 has one surface 66a, the other surface 66b, one end surface 66c, and the other end surface 66d.

[0093] One surface 66a is arranged on the blade body 45 side and is flush with one surface 62b of the platform body 62. The other surface 66b is arranged on the opposite side (the shaft attachment portion 49 side) of the one surface 66a and is flush with the other surface 62c of the platform body 62.

[0094] The one end surface 66c is arranged on the end surface 62a side of the platform body 62. The one end surface 66c is configured to be flush with the end surface 62a of the platform body 62.

[0095] The other end surface 66 d is arranged on the opposite side (the blade body 45 side) to the one end surface 66 c. The other end surface 66 d is in contact with the first welded portion 65 .

[0096] The one end surface 66c and the other end surface 66d are arranged in the blade width direction Dwp.

[0097] When one end surface 66c of the second weld portion 66 arranged on the end surface 62a side of the platform body 62 is used as a reference, the thickness M1 of the second weld portion 66 in the direction from the one end surface 66c of the second weld portion 66 toward the blade body 45 is equal to the value of the length L2 of the second region 72 described above.

[0098] The thickness M1 of the second weld portion 66 is set to be 1.0 mm or more and 3.0 mm or less. The thickness M1 of the second weld portion 66 is preferably 1.5 mm or more and 2.5 mm or less, and more preferably 1.5 mm or more and 2.0 mm or less.

[0099] The portion of the notch 63 where the first weld portion 65 and the second weld portion 66 are arranged is a repaired portion of the platform 47 (hereinafter, simply referred to as a “repaired portion”).

[0100] (Structure of the first welding material and the second welding material)

[0101] As the material of the first welding material 81 , a material having higher weldability than that of the second welding material 82 is used.

[0102] As the material of the second welding material 82 , a material having higher high temperature strength than the first welding material 81 is used.

[0103] Specifically, as the material of the first welding material 81, for example, Inconel 625 (composition / Ni: 61.0 mass %, Cr: 22.0 mass %, Mo: 9.0 mass %, Fe: 5.0 mass %) which is a Ni-Cr-Fe-based nickel alloy can be used.

[0104] When Inconel 625 is used as the material of the first welding material 81 , as the material of the second welding material 82 , for example, MGA1400 (general casting alloy), No. 14, MGA2400 (general casting alloy) or the like having higher high temperature strength than Inconel 625 can be used.

[0105] Among these three materials, MGA1400 has the highest high temperature strength, and MGA2400 has the lowest high temperature strength. The high temperature strength of No.14 is lower than that of MGA1400, and higher than that of MGA2400.

[0106] The composition of MGA1400 is set to Cr: 12.0~14.3 mass%, Co: 8.5~11.0 mass%, Mo: 1.0~3.5 mass%, W: 3.5~6.2 mass%, Ta: 3.0~5.5 mass%, Al: 3.5~4.5 mass%, Ti: 2.0~3.2 mass%, C: 0.04~0.12 mass%, B: 0.005~0.05 mass%, Zr: 0.001~5ppm, and the remainder: Ni and inevitable impurities.

[0107] The composition of No. 14 is set to C: more than 0.13 mass% and less than 0.30 mass%, Cr: more than 15.7 mass% and less than 16.3 mass%, Co: more than 8.00 mass% and less than 9.00 mass%, Ta: more than 1.50 mass% and less than 2.00 mass%, at least any one of Mo and W: more than 1.5 mass% and less than 5.0 mass%, Ti: more than 1.70 mass% and less than 3.20 mass%, Al: more than 1.70 mass% and less than 3.20 mass%, and the remainder: Ni.

[0108] The composition of MGA2400 is composed of C: 0.05-0.25 mass%, Cr: 10-20 mass%, Co: 15-25 mass%, W and Mo: one or two of 3.5 mass% Mo and 0.5-10 mass% W (the value of W+1 / 2Mo is 0.5-10 mass%), Ti: 1.0-5.0 mass%, Al: 1.0-4.0 mass%, Ta: 0.5-4.5 mass%, Nb: 0.2-3.0 mass%, Zr: 0.005-0.10 mass%, B: 0.001-0.01 mass%, and the remainder: Ni and inevitable impurity elements. For example, the amount of (Al+Ti) can be set to about 5.5 mass% and the amount of (W+1 / 2Mo) can be set to about 6.0 mass%.

[0109] The thermal barrier coating 58 is formed to cover the repaired one surface 62 b , one surface 65 a of the first weld 65 , one surface 66 a of the second weld 66 , and a portion of one end surface 66 c of the second weld 66 located on the blade body 45 side.

[0110] The thermal barrier coating 58 has a function of protecting the platform body 62 and the repaired portion of the platform body 62 from high-temperature combustion gases.

[0111] The fillet portion 48 is a connection portion between the blade body 45 and the platform 47, and has a surface 48a on which the combustion gas flows.

[0112] The surface 48a is configured to partition the combustion gas flow path 41 (see Figure 1 The gas passage surface 47a of the platform 47 which is a part of the edge of the blade body 45 gradually becomes the blade surface (at Figure 3 In the case of , it is a curved surface of the pressure surface 51a).

[0113] The fillet portion 48 has a starting end 48S and a terminal end 48E arranged in the blade width direction Dwp.

[0114] The start end 48S is an end disposed on the platform 47 side. The terminal end 48E is an end disposed on the blade body 45 side.

[0115] The fillet portion 48 has a heat-affected zone 48A (HAZ) formed when build-up welding is performed during the formation of the first weld portion 65. The heat-affected zone 48A is arranged closer to the end surface 62a of the platform body 62 than the terminal end 48E of the fillet portion 48.

[0116] The heat-affected width W1 , which is the width of the heat-affected portion 48A in the blade width direction Dwp, can be set to, for example, 3 mm.

[0117] The shaft mounting portion 49 has a shank 85 and a blade root 86 .

[0118] The handle 85 is provided on the side of the platform 47 opposite to the side on which the blade body 45 is provided. The handle 85 extends away from the platform 47 in the blade height direction Dwh.

[0119] The blade root 86 is provided at the end portion of the shank 85 located at the radial inner side Dri. The blade root 86 extends in the blade height direction Dwh away from the shank 85. The cross-sectional shape of the blade root 86 is set to be a Christmas tree shape. The blade root 86 is formed on the turbine rotor 31 (refer to Figure 1 ) is engaged with the blade root groove (not shown) on the blade.

[0120] (Operation and Effect of Blade (Turbine Blade) of First Embodiment)

[0121] As described above, the first region 71 of the notch 63 located on the side close to the blade body 45 is formed of the first welding material 81 having higher weldability than the second welding material 82, thereby suppressing the generation of cracks 69 caused by welding. In other words, the generation of cracks 69 caused by residual stress after welding can be suppressed.

[0122] The crack 69 formed in the platform 47 is first formed on the end surface 62 a of the platform 47 and then expands into the platform 47 .

[0123] Therefore, by configuring the second weld portion 66 composed of the second welding material 82 having high-temperature strength higher than the high-temperature strength of the first welding material 81 in the second region 72 located closer to the end surface 62a of the platform 47 than the first region 71 in the notch portion 63, it is possible to suppress the occurrence of cracks 69 in the second weld portion 66 when the gas turbine 10 is operating.

[0124] This can suppress the occurrence of cracks 69 in the repaired portion (the portion where the first weld portion 65 and the second weld portion 66 are arranged in the notch portion 63 ) during operation.

[0125] Generally, as characteristics of welding materials, material strength and weldability are contradictory, and this becomes prominent particularly when high temperature strength is required.

[0126] That is, welding materials with high creep or high-temperature LCF strength have poor weldability and are prone to cracking after welding.

[0127] On the other hand, materials with good weldability have relatively low high temperature strength and are less likely to crack after welding.

[0128] Furthermore, a difficult-to-weld material with low weldability such as the second welding material 82 requires an increased amount of heating during welding, so the base material is easily affected by the heat during welding, and cracks are easily generated in the heat affected zone (HAZ).

[0129] Furthermore, if the thickness M1 of the second weld portion 66 in the direction from one end surface 66c of the second weld portion 66 toward the blade body 45 is set to less than 1.0 mm, the thickness M1 of the second weld portion 66 in the direction from one end surface 66c toward the blade body 45 becomes too thin, making it difficult to suppress the generation of cracks 69 in the second weld portion 66 during operation.

[0130] Furthermore, since the second welding material 82 has higher strength against thermal fatigue than the first welding material 81, in terms of structural design, in order to ensure sufficient strength against the repeated thermal stress generated in the end of the platform 47 during operation, it is preferred to increase the thickness M1 of the second welding portion 66 formed by the second welding material 82.

[0131] However, if the thickness M1 of the second weld portion 66 is greater than 3.0 mm, the portion of the repaired portion that is prone to cracks 69 (not shown) caused by the welding operation after welding will increase relatively, and the heat-affected portion 48A of the base material will also become larger, which is not preferred with respect to welding cracks generated after repair.

[0132] Therefore, by setting the thickness M1 of the second welded portion 66 within the range of 1.0 mm to 3.0 mm, cracks 69 are less likely to occur on the end surface 62a during operation, and the repaired portion can be provided with fewer cracks 69 (not shown) caused by welding work.

[0133] Furthermore, by setting the thickness M1 of the second welded portion 66 within a range of 1.5 mm to 2.5 mm, it is possible to further suppress the occurrence of cracks 69 (not shown) in the repaired portion due to the welding work.

[0134] Furthermore, by setting the thickness M1 of the second welded portion 66 within a range of 1.5 mm to 2.0 mm, it is possible to further suppress the occurrence of cracks 69 (not shown) in the repaired portion due to the welding work.

[0135] Furthermore, by providing the first region 71 with the non-penetrating portion 75 that does not penetrate the platform body 62, when the first region 71 is welded using the first welding material 81, the non-penetrating portion 75 can function as a supporting portion that supports the molten first welding material 81. Thus, welded deposition using the first welding material 81 can be easily performed.

[0136] Furthermore, by arranging the heat-affected portion 48A closer to the one end surface 66c of the terrace 47 than the terminal end 48E of the fillet portion 48, it is possible to suppress the heat-affected portion 48A from being formed on the blade 45. Thus, it is possible to suppress the performance degradation of the blade 45 caused by the heat-affected portion 48A.

[0137] In addition, in the first embodiment, as an example, the case where the platform 47 constituting the turbine moving blade 37B which is one of the blades is repaired is described, but for example, when a crack 69 occurs in a shroud (a structure not shown corresponding to the platform 47 of the moving blade) constituting the turbine stationary blade 38, a notch portion 63 can be formed on the shroud, and a first weld portion 65 and a second weld portion 66 can be arranged on the notch portion 63.

[0138] Next, refer to Figure 3 , Figure 7 and Figure 8 The determination of whether to repair the turbine blade 37B having the crack 69 will be described. Figure 8 In, with Figure 2 and Figure 3 The same components of the structures shown are denoted by the same reference numerals.

[0139] like Figure 7 The process shown in FIG. 1 starts. Then, in step S1, as shown in FIG. Figure 8 As shown, a distance N1 is measured from a tip 69A of the slit 69 closest to the blade body 45 to a terminal end 48E of the fillet 48 .

[0140] Next, in step S2 , it is determined whether the distance N1 is larger than the heat affected width W1 of the heat affected portion 48A.

[0141] In step S2 , if it is determined that the distance N1 is larger than the heat affected width W1 of the heat affected portion 48A (the heat affected portion 48A is not formed on the blade body 45 ) (YES), the process proceeds to step S3 and a repair process is performed.

[0142] On the other hand, if it is determined that the distance N1 is smaller than the heat affected width W1 of the heat affected portion 48A (the heat affected portion 48A is formed on the blade body 45 ) (No), the process proceeds to step S4 .

[0143] In step S4, the turbine rotor blade 37B (blade) in which the crack 69 has occurred is discarded.

[0144] (Effect of determining whether to repair the platform)

[0145] In this way, when the distance N1 from the end 69A of the crack 69 closest to the blade body 45 to the terminal end 48E of the fillet portion 48 is greater than the heat affected width W1, by performing a repair process (including the first welding process and the second welding process described later), the formation of the heat affected portion 48A on the blade body 45 can be suppressed, so that the repaired turbine blade 37B (blade) can be reused.

[0146] Next, refer to Figures 9 to 17 The method for repairing a blade according to the first embodiment ( Figure 7 The repair process of step S3 shown in FIG. Figures 9 to 17 In, with Figure 1 to Figure 6 The same structural parts are marked with the same symbols.

[0147] like Fig. 9 The process shown in FIG. 1 starts. Then, in step S5, as shown in FIG. Fig.10 As shown, remove Figure 8 The thermal barrier coating 58 is shown. Thus, one side 62b of the platform body 62 is exposed.

[0148] (Notch Forming Step)

[0149] Next, in step S6, remove Fig.10 The crack-containing region P of the platform body 62 before repair shown in the figure includes the crack 69. Fig.11 As shown, a notch portion 63 is formed, and the notch portion 63 extends from the end surface 62a of the platform body 62 toward the blade body 45 (refer to Figure 3 ) is recessed and includes a first region 71 located on the blade body 45 side and a second region 72 located closer to the end surface 62a of the platform body 62 than the first region 71. In step S6, the notch portion 63 is formed by, for example, cutting.

[0150] In step S6 , the second region 72 is formed so that the length L2 of the second region 72 is within the range of 1.0 mm to 3.0 mm.

[0151] If the length L2 of the second region 72 is set to be less than 1.0 mm, the thickness of the second welding material 82 filling the second region 72 is less than 1.0 mm. Fig.14 ) becomes too thin, making it difficult to suppress the generation of cracks 69 in the second welding material 82 during operation.

[0152] Furthermore, due to the first welding material 81 (reference Fig.14) is compared to the second welding material 82, which has a higher strength against thermal fatigue. Therefore, in terms of structural design, in order to ensure sufficient strength against the repeated thermal stress generated in the end of the platform 47 during operation, it is preferred to increase the thickness of the second welding material 82.

[0153] Among them, if the length L2 of the second region 72 is greater than 3.θmm, the thickness of the second welding material 82 is greater than 3.0mm. Therefore, the portion of the cracks 69 caused by the welding operation that is prone to occur in the repaired portion after welding increases, and the heat-affected portion 48A of the base material also becomes larger, which is not preferred relative to the welding cracks generated after the repair.

[0154] Therefore, by forming the second region 72 so that the length L2 thereof is within the range of 1.0 mm to 3.0 mm, the crack 69 can be suppressed from being generated on the end surface 62a of the stage 47 during operation and the crack 69 can be suppressed from being generated during welding work.

[0155] In addition, the length L2 of the second region 72 is preferably set within a range of 1.5 mm to 2.5 mm, and more preferably set within a range of 1.5 mm to 2.0 mm.

[0156] In step S6 , the penetration portion 74 penetrating the platform body 62 in the thickness direction of the platform body 62 and the non-penetration portion 75 not penetrating the platform body 62 are formed in the first region 71 .

[0157] (Effect of forming a non-penetrating portion)

[0158] Thus, by forming the non-penetrating portion 75 that does not penetrate the platform body 62 in the first region 71, when the first region 71 is welded using the first welding material 81, the non-penetrating portion 75 can function as a supporting portion for supporting the molten first welding material 81. Thus, welded deposition using the first welding material 81 can be easily performed.

[0159] (First welding process)

[0160] Next, in step S7, Fig.12 and Fig.13 As shown, by overlay welding using the first welding material 81 having higher weldability than the second welding material 82 , the first region 71 is filled with the first welding material 81 (first welding step).

[0161] In this stage, if Fig.13 As shown, the first welding material 81 protrudes from one surface 62 b and the other surface 62 c of the platform body 62 .

[0162] As the first welding material 81 , for example, the above-described Inconel 625 can be used.

[0163] At this time, if Fig.12 As shown, it is preferable to perform build-up welding using the first welding material 81 with the tip 63A of the notch portion 63 located on the blade body 45 side facing downward.

[0164] (Effect of performing the first welding step by making the end of the notch portion face downward)

[0165] In this way, by placing the tip 63A of the notch 63 on the blade body 45 side at the lower side for cladding welding of the first welding material 81 , the tip 63A of the notch 63 can function as a supporting surface for supporting the first welding material 81 , thereby facilitating the first welding process.

[0166] (Second welding process)

[0167] Next, in step S8, Fig.14 and Fig.15 As shown, by overlay welding using a second welding material 82 having a higher high temperature strength than the first welding material 81, the second region 72 is filled with the second welding material 82 (second welding step).

[0168] In this stage, if Fig.15 As shown, the second welding material 82 protrudes from one surface 62 b and the other surface 62 c of the platform body 62 .

[0169] When Inconel 625 is used as the first welding material 81 , as the second welding material 82 , for example, MGA1400 (general casting alloy), No. 14, MGA2400 (general casting alloy) described above, etc. can be used.

[0170] At this time, if Fig.14 As shown, it is preferable to perform build-up welding using the second welding material 82 with the tip 63A of the notch portion 63 located on the blade body 45 side facing downward.

[0171] (Effect of performing the second welding step by making the end of the notch portion face downward)

[0172] In this way, by making the end 63A of the notch portion 63 located on the blade body 45 side the lower side for cladding welding of the second welding material 82, the end surface of the first welding material 81 can function as a supporting portion for supporting the second welding material 82, thereby easily performing the second welding process.

[0173] (Finishing process)

[0174] Next, in step S9, Fig.16 and Fig.17As shown, by removing the first welding material 81 and the second welding material 82 protruding from one surface 62b and the other surface 62c of the platform body 62, a first welding portion 65 composed of the first welding material 81 is formed in the first region 71, and a second welding portion 66 composed of the second welding material 82 is formed in the second region 72.

[0175] The first welding portion 65 includes a first surface 65 a that is flush with the first surface 62 b of the platform body 62 and another surface 65 b that is flush with the other surface 62 c .

[0176] The second welded portion 66 includes a first surface 66 a flush with the first surface 62 b of the platform body 62 and another surface 66 b flush with the other surface 62 c .

[0177] For the finishing process, for example, a grinder can be used.

[0178] (Thermal barrier coating forming step)

[0179] Next, in step S10, the turbine blade 37B is repaired by forming a thermal barrier coating 58 on the portion where the thermal barrier coating 58 was removed in step S5, thereby completing the repair. Figure 2 and Figure 3 The repaired turbine blade 37B is shown. Then, Fig. 9 The shown processing ends.

[0180] (Operation and Effect of Blade Repair Method of First Embodiment)

[0181] As described above, by overlay welding the first region 71 located on the blade body 45 side of the notch 63 with the first welding material 81 having higher weldability than the second welding material 82 , the crack 69 caused by the welding operation can be suppressed from occurring in the first region 71 .

[0182] The crack 69 formed in the platform 47 is first formed on the end surface 62 a of the platform 47 and then expands into the platform 47 .

[0183] Therefore, by surfacing the second region 72 located closer to the end surface 62a of the platform 47 than the first region 71 in the notch 63 with the second welding material 82 having a higher high temperature strength than the first welding material 81, it is possible to suppress the generation of cracks 69 in the second welded portion 66 during operation. Thus, it is possible to suppress the generation of cracks 69 in the repaired portion during operation.

[0184] Furthermore, if the range less than 1.0 mm from the end surface 62a of the platform 47 toward the blade body 45 is set as the second region 72, the thickness M1 of the second weld portion 66 (second welding material 82) formed in the second region 72 becomes too thin, making it difficult to suppress the generation of cracks 69 in the second welding material 82 during operation.

[0185] Furthermore, if the range exceeding 3.0 mm from the end face 62a of the platform 47 toward the blade body 45 is set as the second region 72, the proportion of the second welding material 82 becomes higher, and thus the generation of cracks 69 caused by the welding operation becomes more. Therefore, by setting the region in the range of 1.0 mm or more and 3.0 mm or less from the end face 62a of the platform 47 toward the blade body 45 as the second region 72, the generation of cracks 69 (not shown) caused by the welding operation can be suppressed, and the generation of cracks 69 during operation can also be suppressed.

[0186] Furthermore, by defining the second region 72 as a range of 1.5 mm to 2.5 mm from the end surface 62 a of the platform 47 toward the blade body 45 , the occurrence of the crack 69 caused by the welding work can be further suppressed.

[0187] Furthermore, by defining the second region 72 as a range of 1.5 mm to 2.0 mm from the end surface 62 a of the platform 47 toward the blade body 45 , the occurrence of the crack 69 caused by the welding work can be further suppressed.

[0188] In the first embodiment, the case of repairing the platform 47 constituting the turbine blade 37B as one of the blades is described as an example. However, for example, the turbine blade 38 having the crack 69 in the shroud may be repaired by the above-mentioned method.

[0189] As mentioned above, although the preferred embodiment of the present invention has been described in detail, the present invention is not limited to the specific embodiment involved in the present invention, and various modifications and changes can be made within the scope of the gist of the present invention described in the claims.

[0190] [Note]

[0191] The method of repairing the blade (turbine blade 37B), the blade (turbine blade 37B), and the gas turbine 10 described in each embodiment can be understood as follows, for example.

[0192] (1) In a method for repairing a blade (turbine blade 37B) according to a first embodiment, the blade (turbine blade 37B) comprises: a blade body 45 arranged in a combustion gas flow path 41 in which the combustion gas flows and having a blade shape; and a platform 47 provided at one end of the blade body 45 in a blade height direction Dwh and extending in a blade width direction Dwp including a direction perpendicular to the blade height direction Dwh to partition a portion of an edge of the combustion gas flow path 41. The repair method repairs a crack 69 formed from an end face 62a of the platform 47 in the blade width direction Dwp toward the blade body 45 for the blade (turbine blade 37B). The repair method comprises: a notch forming step of forming a notch 63, wherein the notch 63 is formed from the platform 47 by removing a crack-containing region P including the crack 69 in the platform 47 before repair. The end face 62a of 47 is recessed toward the blade body 45, and includes a first region 71 located on the side of the blade body 45 and a second region 72 located on the side of the end face 62a of the platform 47 closer to the first region 71; a first welding process, by using a first welding material 81 for surfacing, the first region 71 is filled with the first welding material 81; and a second welding process, after the first welding process, by using a second welding material 82 for surfacing, the second region 72 is filled with the second welding material 82, the high-temperature strength of the second welding material 82 is higher than the high-temperature strength of the first welding material 81, the weldability of the first welding material 81 is higher than the weldability of the second welding material 82, and the second region 72 is a region in the range of 1.0 mm or more and 3.0 mm or less from the end face 62a of the platform 47 toward the blade body 45.

[0193] Generally, as characteristics of welding materials, material strength and weldability are contradictory, and this becomes prominent particularly when high temperature strength is required.

[0194] That is, welding materials with high creep or high-temperature LCF strength have poor weldability and are prone to cracking after welding.

[0195] On the other hand, materials with good weldability have relatively low high temperature strength and are less likely to crack after welding.

[0196] Furthermore, a difficult-to-weld material with low weldability such as the second welding material 82 requires an increased amount of heating during welding, so the base material is easily affected by the heat during welding, and cracks are easily generated in the heat affected zone (HAZ).

[0197] If the range of the second region 72 is set to be less than 1.0 mm from the end surface 62a of the platform 47 toward the blade body 45, the thickness of the second welding material 82 filling the second region 72 is less than 1.0 mm. The thickness of the second welding material 82 becomes too thin, making it difficult to suppress the generation of cracks 69 in the second welding material 82 during operation.

[0198] Furthermore, since the second welding material 82 is stronger against thermal fatigue than the first welding material 81, in terms of structural design, it is preferred to increase the thickness of the second welding material 82 in order to ensure sufficient strength against repeated thermal stresses generated in the end of the platform 47 during operation.

[0199] Among them, if the range of the second region 72 from the end face 62a of the platform 47 toward the blade body 45 is greater than 3.0 mm, the thickness of the second welding material 82 is greater than 3.0 mm. Therefore, the portion of cracks 69 caused by the welding operation that is prone to occur in the repaired portion after welding increases, and the heat-affected portion 48A of the base material also becomes larger. Therefore, it is not preferred relative to the welding cracks generated after the repair.

[0200] Therefore, by setting the second region 72 to be an area within a range of 1.0 mm to 3.0 mm from the end surface 62a of the platform 47 toward the blade body 45, cracks 69 can be suppressed from occurring on the end surface 62a of the platform 47 during operation and during welding operations.

[0201] (2) The method for repairing a blade (turbine blade 37B) according to the second embodiment is the method for repairing a blade (turbine blade 37B) according to (1), wherein the connection portion between the blade body 45 and the platform 47 constitutes a fillet portion 48 for the flow of the combustion gas, the surface 48a of the fillet portion 48 is set as a gas passage surface 47a of the platform 47 which is a part of the edge of the combustion gas flow path 41 and gradually becomes a curved surface of the blade surface of the blade body 45, one of the two ends of the fillet portion 48 in the blade width direction Dwp, which is arranged on the blade body 45 side, is a terminal end 48E of the fillet portion 48, and when the width of the heat-affected portion 48A affected by the heat during the build-up welding of the first welding material 81 is set as a heat-affected width W1, the first welding process and the second welding process can be implemented when the distance N1 from the end 69A of the crack 69 closest to the blade body 45 to the terminal end 48E of the fillet portion 48 is greater than the heat-affected width W1.

[0202] In this way, when the distance N1 from the end 69A of the crack 69 closest to the blade body 45 to the terminal end 48E of the fillet portion 48 is greater than the heat affected width W1, by performing a repair process (including the first welding process and the second welding process), the formation of the heat affected portion 48A on the blade body 45 can be suppressed, so that the repaired blade (turbine blade 37B) can be reused.

[0203] (3) A method for repairing a blade (turbine blade 37B) according to a third aspect is the method for repairing a blade (turbine blade 37B) according to (2), wherein the heat affected width W1 may be 3 mm.

[0204] In this way, the heat-affected width W1 can be set to 3 mm.

[0205] (4) The method for repairing a blade (turbine blade 37B) involved in the fourth embodiment is the method for repairing a blade (turbine blade 37B) described in any one of (1) to (3), wherein, in the notch forming step, a through portion 74 that penetrates the platform 47 along the thickness direction of the platform 47 to remove the crack 69 and a non-through portion 75 that does not penetrate the platform 47 can be formed in the first region 71.

[0206] Thus, by forming the non-penetrating portion 75 that does not penetrate the platform 47 in the first region 71, when the first region 71 is welded using the first welding material 81, the non-penetrating portion 75 can function as a supporting portion for supporting the molten first welding material 81. Thus, welded surface using the first welding material 81 can be easily performed.

[0207] (5) The method for repairing a blade (turbine blade 37B) involved in the fifth embodiment is the method for repairing a blade (turbine blade 37B) described in any one of (1) to (4), wherein, in the first welding step, the end 63A of the notch portion 63 located on the side of the blade body 45 is placed on the lower side for cladding welding of the first welding material 81, and in the second welding step, the end 63A of the notch portion 63 located on the side of the blade body 45 is placed on the lower side for cladding welding of the second welding material 82.

[0208] Thus, by placing the first welding material 81 with the tip 63A of the notch 63 on the blade body 45 side facing downward, the tip 63A of the notch 63 can function as a support surface for supporting the first welding material 81. Thus, the first welding step can be easily performed.

[0209] Furthermore, by placing the tip 63A of the notch 63 on the blade body 45 side downward to perform build-up welding of the second welding material 82, the end surface of the first welding material 81 can function as a support for the second welding material 82. Thus, the second welding step can be easily performed.

[0210] (6) The blade involved in the sixth embodiment (turbine blade 37B) comprises: a blade body 45, which is arranged in a combustion gas flow path 41 where the combustion gas flows and has a blade shape; and a platform 47, which is provided at one end of the blade body 45 in the blade height direction Dwh and extends in a blade width direction Dwp including a direction perpendicular to the blade height direction Dwh to partition a portion of the edge of the combustion gas flow path 41, wherein the platform 47 has: a notch portion 63, which is recessed from the end face 62a of the platform 47 toward the blade body 45 by removing a crack-containing region P where a crack 69 is generated, and includes a first region 71 located on the blade body 45 side and a second region 72 located on the end face 62a side of the platform 47 closer to the first region 71. 2 regions 72; a first welding portion 65, which is configured in a manner to fill the first region 71 and is composed of a first welding material 81; and a second welding portion 66, which is configured in a manner to fill the second region 72 and is composed of a second welding material 82, the high-temperature strength of the second welding material 82 is higher than the high-temperature strength of the first welding material 81, the weldability of the first welding material 81 is higher than the weldability of the second welding material 82, and when the end face (one end face 66c) of the second welding portion 66 configured on the end face 62a side of the platform 47 is taken as a reference, the thickness M1 of the second welding portion 66 in the direction from the end face (one end face 66c) of the second welding portion 66 toward the blade body 45 is greater than 1.0 mm and less than 3.0 mm.

[0211] Generally, as characteristics of welding materials, material strength and weldability are contradictory, and this becomes prominent particularly when high temperature strength is required.

[0212] That is, welding materials with high creep or high-temperature LCF strength have poor weldability and are prone to cracking after welding.

[0213] On the other hand, materials with good weldability have relatively low high temperature strength and are less likely to crack after welding.

[0214] Furthermore, a difficult-to-weld material with low weldability such as the second welding material 82 requires an increased amount of heating during welding, so the base material is easily affected by the heat during welding, and cracks are easily generated in the heat affected zone (HAZ).

[0215] If the thickness M1 of the second weld portion 66 formed of the second welding material 82 is set to less than 1.0 mm, the thickness M1 of the second weld portion 66 becomes too thin, and it is difficult to suppress the generation of the crack 69 in the second weld portion 66 during operation.

[0216] Furthermore, since the second welding material 82 is stronger against thermal fatigue than the first welding material 81, in terms of structural design, it is preferred to increase the thickness M1 of the second welding portion 66 in order to ensure sufficient strength against repeated thermal stresses generated in the end of the platform 47 during operation.

[0217] If the thickness M1 of the second weld portion 66 is greater than 3.0 mm, the portion of the repaired portion that is prone to cracks 69 caused by the welding operation increases after welding, and the heat-affected portion 48A of the base material also becomes larger, which is not preferred with respect to welding cracks generated after repair.

[0218] Therefore, by setting the thickness M1 of the second weld portion 66 to be within the range of 1.0 mm to 3.0 mm, it is possible to suppress the occurrence of cracks 69 on the end surface 62 a of the stage 47 during operation and to suppress the occurrence of cracks 69 during welding work.

[0219] (7) The blade (turbine blade 37B) involved in the seventh embodiment is the blade (turbine blade 37B) of (6), wherein the first region 71 has a through portion 74 that penetrates the platform 47 along the thickness direction of the platform 47 and a non-through portion 75 that does not penetrate the platform 47, and the through portion 74 can be formed in a manner that removes the position where the crack 69 is formed.

[0220] Thus, by providing the first region 71 with the non-penetrating portion 75 that does not penetrate the platform 47, when the first region 71 is welded using the first welding material 81, the non-penetrating portion 75 can function as a supporting portion that supports the molten first welding material 81. Thus, welded deposition using the first welding material 81 can be easily performed.

[0221] (8) The blade (turbine blade 37B) involved in the eighth embodiment is a blade (turbine blade 37B) of (6) or (7), wherein the connection portion between the blade body 45 and the platform 47 constitutes a fillet portion 48 for the flow of the combustion gas, the surface of the fillet portion 48 is set as a gas passage surface 47a of the platform 47 which is a part of the edge of the combustion gas flow path 41 and gradually becomes a curved surface of the blade surface of the blade body 45, one of the two ends of the fillet portion 48 in the blade width direction Dwp, which is arranged on the blade body 45 side, is a terminal end 48E of the fillet portion 48, and the fillet portion 48 has a heat-affected portion 48A formed by the heat effect during the build-up welding of the first welding material 81, and the heat-affected portion 48A can be arranged on the side of the end face 62a of the platform 47 closer to the terminal end 48E of the fillet portion 48.

[0222] Thus, by arranging the heat affected portion 48A closer to the end surface 62a of the terrace 47 than the terminal end 48E of the fillet portion 48, it is possible to suppress the heat affected portion 48A from being formed on the blade 45. Thus, it is possible to suppress the performance degradation of the blade 45 caused by the heat affected portion 48A.

[0223] (9) The gas turbine 10 according to the ninth aspect includes a turbine rotor blade (37B) and / or a turbine stationary blade (38) as the blade (turbine rotor blade 37B) according to any one of (6) to (8).

[0224] In this way, the gas turbine 10 can include turbine rotor blades (37B) and / or turbine stationary blades (38) as blades.

[0225] Industrial Applicability

[0226] The invention relates to a blade repair method, a blade and a gas turbine.

[0227] According to the present invention, it is possible to suppress the occurrence of cracks on the end surface of the platform of the blade during operation and the occurrence of cracks during welding work.

[0228] Explanation of symbols

[0229] 10-gas turbine, 11-compressor, 12-combustor, 13-turbine, 15-generator, 21-compressor rotor, 21a, 31a-outer circumference, 23-compressor moving blade layer, 24-compressor casing, 24a, 34a-inner circumference, 25-compressor stationary blade layer, 27-compressor moving blade, 28-compressor stationary blade, 30-rotor, 31-turbine rotor, 33-turbine moving blade layer, 34-turbine casing body, 35-turbine static blade layer, 37, 37A, 37B-turbine moving blades, 38-turbine static blades, 41-combustion gas flow path, 45-blade body, 45A-leading edge, 45B-trailing edge, 47-platform, 47a-gas passage surface, 48-fillet, 48A-heat-affected part, 48E-terminal end, 48S-starting end, 49-shaft mounting portion, 51-pressure side blade wall, 51a-pressure surface, 52-negative pressure side blade sheet wall, 52a-negative pressure surface, 54-top plate, 57-metal substrate, 58-thermal barrier coating, 62-platform body, 62a-end surface, 62b, 65a, 66a-one surface, 62c, 65b, 66b-the other surface, 63-notch, 63A, 69A-end, 65-first welding part, 66-second welding part, 66c-one end surface, 66d-the other end surface, 69-crack, 71-first region, 72-the second region, 74-the penetrating part, 75-the non-penetrating part, 81-the first welding material, 82-the second welding material, 85-the shank, 86-the blade root, Ar-the axis line, Dc-the circumferential direction, Dr-the radial direction, Dri-the radial inner side, Dro-the radial outer side, Dwp-the blade width direction, Dwh-the blade height direction, L1, L2-the length, M1-the thickness, N1-the distance, P-the crack-containing area, W1-the heat affected width.

Claims

1. A method for repairing a blade, wherein: The blade comprises: a blade body, which is arranged in a combustion gas flow path where the combustion gas flows and is in a blade shape; and a platform, which is provided at one end of the blade body in a blade height direction and extends in a blade width direction including a direction perpendicular to the blade height direction to partition a portion of an edge of the combustion gas flow path, wherein the repair method repairs a crack formed from an end surface of the platform in the blade width direction toward the blade body, the repair method comprising: a notch forming step of forming a notch, wherein the notch is recessed from the end surface of the platform toward the blade body by removing a crack-containing region containing the crack in the platform before repair, and includes a first region located on the blade body side and a second region located closer to the end surface side of the platform than the first region; In a first welding step, the first region is filled with the first welding material by cladding welding using the first welding material; and a second welding step, after the first welding step, by cladding welding using a second welding material to fill the second region with the second welding material; The high temperature strength of the second welding material is higher than the high temperature strength of the first welding material, The weldability of the first welding material is higher than the weldability of the second welding material. The second region is a region in a range of 1.0 mm to 3.0 mm from the end surface of the platform toward the blade body. The connection between the blade body and the platform forms a fillet for the flow of the combustion gas. The surface of the fillet portion is a curved surface in which the gas passage surface of the platform that defines a portion of the edge of the combustion gas flow path gradually becomes the blade surface of the blade body. Of the two ends of the fillet portion in the blade width direction, one end disposed on the blade body side is a terminal end of the fillet portion. When the width of the heat-affected portion affected by the heat during cladding of the first welding material is set as the heat-affected width, the first welding process and the second welding process are performed when the distance from the end of the crack closest to the blade body to the terminal end of the fillet portion is greater than the heat-affected width.

2. The method for repairing a blade according to claim 1, wherein: The heat affected width is 3 mm.

3. The blade repair method according to claim 1 or 2, wherein: In the notch forming step, a penetration portion that penetrates the terrace in a thickness direction of the terrace to remove the crack and a non-penetration portion that does not penetrate the terrace are formed in the first region.

4. The blade repair method according to claim 1 or 2, wherein: In the first welding step, the first welding material is overlaid with the distal end of the notch portion located on the blade body side facing downward. In the second welding step, the second welding material is overlaid with the tip of the notch portion located on the blade body side facing downward.

5. A blade comprising: a blade body, which is arranged in a combustion gas flow path where the combustion gas flows and has a blade shape; and A platform is provided at one end of the blade body in the blade height direction and extends in a blade width direction including a direction perpendicular to the blade height direction to define a portion of the edge of the combustion gas flow path, wherein: The platform has a notch portion that is recessed from the end surface of the platform toward the blade body by removing a crack-containing region where cracks have occurred, and includes a first region located on the blade body side and a second region located closer to the end surface side of the platform than the first region; a first welding portion arranged to fill the first region and composed of a first welding material; and The second welding portion is arranged in a manner to fill the second region and is composed of a second welding material. The high temperature strength of the second welding material is higher than the high temperature strength of the first welding material, The weldability of the first welding material is higher than the weldability of the second welding material. When the end surface of the second weld portion disposed on the end surface side of the platform is used as a reference, the thickness of the second weld portion in the direction from the end surface of the second weld portion toward the blade body is 1.0 mm or more and 3.0 mm or less. The connection between the blade body and the platform forms a fillet for the flow of the combustion gas. The surface of the fillet portion is a curved surface in which the gas passage surface of the platform that defines a portion of the edge of the combustion gas flow path gradually becomes the blade surface of the blade body. Of the two ends of the fillet portion in the blade width direction, one end disposed on the blade body side is a terminal end of the fillet portion. The fillet portion has a heat-affected zone formed by the heat effect of the first welding material during build-up welding. The heat-affected portion is arranged on an end surface side of the terrace relative to a terminal end of the fillet portion.

6. The blade according to claim 5, wherein: The first region has a penetrating portion penetrating the platform in the thickness direction of the platform and a non-penetrating portion not penetrating the platform. The penetration portion is formed by removing a position where the crack is formed. 7 . A gas turbine comprising a turbine rotor blade and / or a turbine stationary blade as the blade according to claim 5 or 6 .