Method for producing polyamide resin film

By using recycled monomers to polymerize to prepare polyamide resin films, and combining moisture adjustment and biaxial stretching processes, the problems of insufficient strength, elongation and printability of polyamide resin films in the existing technology are solved, and high-quality recycling rates and excellent packaging material performance.

CN115003735BActive Publication Date: 2024-10-01UNITIKA LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180009922.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-01-24
Filing Date
2021-01-22
Publication Date
2024-10-01
Estimated Expiration
2041-01-22

AI Technical Summary

Technical Problem

The existing technology is difficult to prepare polyamide resin films with excellent strength and elongation, and has deficiencies in printability and recycling rate. In particular, it is difficult to improve the printability and adhesion of packaging films.

Method used

By polymerizing regenerated monomers as raw materials, refining them and using them to make polyamide resin films, adjusting the moisture content of the film before stretching, and combining it with the biaxial stretching process, a polyamide resin film with high printability is prepared. .

Benefits of technology

It achieves the same printability and mechanical properties as new products, improves the recycling rate to more than 50%, is suitable for use as packaging materials, and promotes resource reuse and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003753514310000161
    Figure BDA0003753514310000161
  • Figure BDA0003753514310000201
    Figure BDA0003753514310000201
  • Figure BDA0003753514310000261
    Figure BDA0003753514310000261
Patent Text Reader

Abstract

The present invention aims to provide a method for manufacturing a polyamide resin film, which uses a polyamide resin obtained by polymerizing a regenerated monomer as a recycled raw material to manufacture the polyamide resin film. The solution is a method for manufacturing a polyamide resin film, which is used to manufacture a polyamide resin film, and the manufacturing method is characterized by comprising the following steps: step (1), generating a monomer from a depolymerization raw material (A); step (2), polymerizing a raw material containing the above-mentioned monomer to manufacture a polyamide resin (B); step (3), refining the above-mentioned polyamide resin (B); and step (4), after making an unstretched film using a starting material containing the refined polyamide resin (B), stretching the above-mentioned unstretched film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a polyamide resin film, wherein the polyamide resin film comprises a polyamide resin obtained by using a large amount of recycled raw materials. Background Art

[0002] Environmental issues have long been a concern, but in recent years, awareness of environmental sustainability has been increasing again. In the past, there has been a high demand for recycling of waste resins, which have been used as raw material resins. For example, waste materials generated when manufacturing thermoplastic resin stretch films include trimming waste, slitting waste, and films that are considered defective and not made into products. Generally, these pellets produced by remelting are recycled as remelted resins (raw materials).

[0003] However, in the material recovery, along with the increase of the content of the remelted resin, the content of foreign matter, thermal degradation products etc. also can increase, and the polyamide resin film with large tensile stress in particular, because can become easy to break when stretched, can cause the productivity to decline. And, the control of the amount of additives contained in the remelted resin can be more difficult, causing also local characteristic changes on the film surface, and the situation of poor printing and poor sealing may occur. In this way, the amount of remelted resin in the polyamide resin film can be limited, even if the recovery rate is to be improved, there is also a limit.

[0004] On the other hand, laminated films such as packaging films, which are laminated with a plurality of resin materials such as a printing layer, a barrier layer, an adhesive layer, and a sealant layer, are difficult to separate into the respective materials and are therefore difficult to recycle.

[0005] In this case, a method of depolymerizing waste resin and using it as a monomer (regenerated monomer) is widely known, and this method is also called chemical recycling. In particular, various chemical recycling methods have been proposed for polyamide resins. For example, a method of melting nylon 6, removing metals, and recovering the ε-caprolactam obtained by the depolymerization reaction as a fiber raw material, a raw material for resin, etc. is widely known (Patent Documents 1 and 2).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 7-330718

[0009] Patent document 2: China Publication CN91106147.9 Summary of the invention

[0010] Problems to be solved by the invention

[0011] However, even if the monomers obtained by depolymerizing the polyamide resin as the resin waste are polymerized, a polyamide resin suitable for a film cannot be obtained. In other words, a film excellent in strength and elongation cannot be obtained.

[0012] Moreover, in recent years, various printing methods have been implemented on packaging containers and other product packaging, and the requirements for printed appearance have tended to be increasingly higher. There is still room for improvement in the printability of the film (especially the reproducibility of the light part (low-tone part) in the light and dark expression).

[0013] Therefore, the main purpose of the present invention is to provide a method for manufacturing a polyamide resin film, which uses a polyamide resin obtained by polymerizing a regenerated monomer as a recycled raw material to manufacture a polyamide resin film. In addition, the purpose of the present invention is to provide a polyamide resin film that can exert printability that is equal to or higher than that of existing products.

[0014] Means for solving problems

[0015] The present inventors have made intensive studies in view of the problems of the prior art and, as a result, have found that the above-mentioned object can be achieved by using a specific raw material containing a regenerated monomer for the production of a membrane, thereby completing the present invention.

[0016] In other words, the present invention relates to the following polyamide resin and a method for producing the same.

[0017] 1. A method for producing a polyamide resin film, characterized in that the method for producing a polyamide resin film comprises the following steps:

[0018] Step (1), generating monomers from the depolymerization raw material (A);

[0019] Step (2), polymerizing the raw materials containing the above-mentioned monomers to produce a polyamide resin (B);

[0020] Step (3), purifying the polyamide resin (B); and

[0021] In step (4), an unstretched film is produced using a starting material containing the purified polyamide resin (B), and then the unstretched film is stretched.

[0022] 2. The production method according to item 1 above, wherein the monomer comprises ε-caprolactam.

[0023] 3. The production method according to the above item 1, further comprising the step of adjusting the moisture content of the unstretched film to 2 to 10% by mass before stretching.

[0024] 4. The production method according to item 1 above, wherein a re-melted resin obtained by melting a polyamide resin (excluding the polyamide resin (B)) is contained as part of the starting material and the content thereof is 1% by mass or more.

[0025] 5. The production method according to the above item 1, wherein the relative viscosity ηR of the purified polyamide resin (B) is 2.5 to 4.5.

[0026] 6. The production method according to the above item 1, wherein the depolymerization raw material (A) is at least one of a polyamide 6 resin and an oligomer thereof.

[0027] 7. A polyamide resin film, wherein the 10% gradation portion of the halftone printing applied to the film is 1000 mm 2 The number of bad pixels is less than 100.

[0028] 8. The polyamide resin film according to the above item 7, wherein the caprolactam monomer concentration in the polyamide resin film is 1.6% by mass or less.

[0029] 9. The polyamide resin film according to item 7 above, wherein the contents of terminal amino groups and terminal carboxyl groups in the polyamide resin film are each 80 mmol / kg or less.

[0030] 10. The polyamide resin film as described in item 7 above, wherein the ratio of the minimum value to the maximum value of the film impact strength in an atmosphere of a temperature of 23° C. and a humidity of 50% RH (minimum value / maximum value) is 0.5 to 1.0.

[0031] 11. The polyamide resin film according to item 7 above, comprising a polyamide resin having a full width at half maximum of a temperature drop crystallization peak of 10° C. or more.

[0032] 12. The polyamide resin film as described in the above item 7, which is biaxially stretched.

[0033] 13. A laminated film comprising the polyamide resin film according to any one of items 7 to 12 above, and a sealant resin layer laminated on the polyamide resin film.

[0034] 14. A packaging material comprising the polyamide resin film according to any one of items 7 to 12 above.

[0035] 15. A polyamide resin film produced by the production method according to any one of items 1 to 6 above.

[0036] Effects of the Invention

[0037] According to the present invention, even if the polyamide resin obtained by polymerizing the recycled monomer is used as a recycled raw material, a polyamide resin film that can exhibit printability equal to or better than that of an existing product (new product) can be provided. More specifically, the present invention can provide a polyamide resin film (particularly a biaxially stretched polyamide resin film) that effectively suppresses a partial reduction in printed appearance, a reduction in adhesion, etc. by using a polyamide resin using a recycled monomer as a raw material.

[0038] Furthermore, the polyamide resin film of the present invention has controlled unevenness in impact strength and is excellent in general physical properties such as film elongation, wettability, and haze, and is therefore particularly suitable for use as a packaging material.

[0039] The manufacturing method of the present invention can use resin waste as raw materials, so it can provide, for example, a recycled polyamide resin film with a recycling rate of more than 50%. In this way, it can promote the reuse of resources and thus contribute to environmental protection as a sustainable development technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a schematic diagram showing a method for evaluating the printability of the polyamide resin film of the present invention. DETAILED DESCRIPTION

[0041] 1. Method for producing polyamide resin film

[0042] The manufacturing method of the present invention is a method for manufacturing a polyamide resin film, which is characterized by comprising the following steps:

[0043] Step (1), generating monomers from the depolymerization raw material (A) (depolymerization step);

[0044] Step (2), polymerizing the raw materials containing the above-mentioned monomers to produce a polyamide resin (B) (polymerization step);

[0045] Step (3), purifying the polyamide resin (B) (purifying step); and

[0046] In step (4), an unstretched film is produced using a starting material containing the purified polyamide resin (B), and then the unstretched film is stretched (film forming step).

[0047] Depolymerization process

[0048] In the depolymerization step, monomers are regenerated from the depolymerization raw material (A) (hereinafter, such monomers are referred to as "regenerated monomers").

[0049] As for the regenerated monomer, lactams are particularly preferred, and examples thereof include ε-caprolactam, enantholactam, capryllactam, and lauryl lactam. Among them, ε-caprolactam is particularly preferred.

[0050] The type of the depolymerization raw material (A) is not particularly limited, and in addition to various polyamide resins, various oligomers of polyamide resins can also be used. More specifically, various resins exemplified below for the polyamide resin (B) can be used as examples. In addition, oligomers include chain bodies of about dimers to heptamers and cyclic bodies of about dimers to nonamers.

[0051] In particular, in the present invention, at least one of polyamide 6 resin and its oligomers is preferably used as the depolymerization raw material (A). In particular, polyamide 6 is a resin substantially composed of ε-caprolactam as a monomer unit, and therefore has the advantage of being easy to monomerize and purify and separate.

[0052] The forms of polyamide resin include the switching parts between products during polymerization, the discharged resin scraps at the switching parts until the film product is made into a product, and other scraps such as trimming scraps and slitting scraps generated during film production, and films that are not made into products because they are considered defective products, etc. Using these as raw materials not only helps to produce films with excellent printability, but also contributes to environmental protection through the utilization of waste materials.

[0053] As the form of oligomers, examples include not only highly water-soluble oligomers recovered from purified water generated during purification of polyamide resins, but also filtration residues containing dimers to octamers having low water solubility.

[0054] The method for generating monomers from the depolymerization raw material (A) is not particularly limited as long as the specified monomers can be obtained, but depolymerization reaction of the depolymerization raw material (A) is preferably used. In other words, the depolymerization raw material (A) can be chemically decomposed by depolymerization reaction to obtain a regenerated monomer.

[0055] The method and conditions of the depolymerization reaction are not particularly limited and can be carried out according to known methods. Therefore, for example, a catalyst may be used or not. In addition, the depolymerization may be carried out in the absence of water (dry method) or in the presence of water (wet method). In particular, from the perspective of productivity, the preferred method is to carry out the depolymerization in hot water vapor in the presence of a catalyst. Regarding cyclic oligomers with low water solubility, it is difficult to directly depolymerize them because the hydrolysis rate of the amide bond is slow, but after ring-opening polymerization to form chain molecules, depolymerization is carried out under the above conditions, and the regenerated monomer can still be suitably obtained from the cyclic oligomers.

[0056] Polymerization process

[0057] In the polymerization step, the polyamide resin (B) is produced by polymerizing a raw material containing the above-mentioned monomer (regenerated monomer).

[0058] The above raw materials may be raw materials in which all monomers are composed of recycled monomers, but it is preferred to use new monomers in combination. The new monomers referred to herein are the antonym of recycled monomers, and refer to monomers that have not undergone a depolymerization process of the polymer. Commercially available products may be used as new monomers. For example, commercially available monomers may be used as new monomers.

[0059] The recycled monomer may contain by-products that are difficult to separate. Therefore, compared with the polyamide resin made of only new monomers, the crystallization rate of the polyamide resin made of only recycled monomers can be slightly reduced, and the crystallization rate of the polyamide resin polymerized by using both new monomers and recycled monomers can be further reduced. This crystallization rate is measured by measuring the cooling crystallization temperature (T C ), and the half-maximum full width of the obtained crystallization peak is used as an indicator. The above-mentioned half-maximum full width in the present invention is usually preferably above 10°C, especially above 11°C, and above 12°C is the best. The wider the half-maximum full width, the wider the range of the crystallization rate, and the less likely it is to produce local unevenness of the crystal state on the surface of the film during stretching and crystallization, which can improve the uniformity and thus improve the printability of the low-tone portion. From this point of view, it is preferred to use a polyamide resin polymerized from a recycled monomer and a new monomer. In addition, the upper limit of the above-mentioned half-maximum full width can be set to about 20°C, for example, but is not limited to this.

[0060] The regenerated monomer content in the raw material is not particularly limited, but from the viewpoint of expanding the above-mentioned full width at half maximum, its upper limit is preferably below 90 mass %, and more preferably below 80 mass %. In addition, the lower limit is not particularly limited, but from the viewpoint of improving the recovery ratio, it is preferably above 5 mass %, and particularly preferably above 10 mass %.

[0061] As for the components other than the recycled monomer, it is preferred to use virgin monomers in combination. In this case, the content of the virgin monomers in the above raw materials is usually preferably about 10 to 95% by mass, and more preferably 20 to 90% by mass.

[0062] For example, ε-caprolactam (hereinafter referred to as "C-CL") regenerated by depolymerization reaction of polyamide 6 resin can be used in the monomer in an amount close to 100% by mass, but it is preferred to contain ε-caprolactam (hereinafter referred to as "V-CL") as a new monomer as a monomer other than C-CL.

[0063] In addition, the polyamide resin (B) may be capped as required for the purpose of suppressing the formation of monomers during melting. For this purpose, the above raw materials may contain an additive such as an end-capping agent as required. There is no particular limitation on the end-capping agent, and examples thereof include organic glycidyl esters, dicarboxylic anhydrides, monocarboxylic acids such as benzoic acid, and diamines.

[0064] The polymerization method for preparing the polyamide resin (B) is not particularly limited, and a known monomer polymerization method can be used. As an example, a method can be used in which ε-caprolactam, water, and benzoic acid as an end-capping agent are mixed, heated and pressurized in a polymerization reactor, and then the polymerization reaction is carried out while reducing pressure and dehydrating until the target viscosity is reached.

[0065] Refining process

[0066] The polyamide resin (B) is purified in the purification step to remove monomers contained in the polyamide resin and increase the relative viscosity of the polyamide resin to a desired range, thereby achieving physical properties suitable for film formation.

[0067] The purification method is not limited, but the polyamide resin (B) is preferably purified so that the relative viscosity (25° C.) falls within the range of about 2.5 to 4.5. Therefore, for example, the polyamide resin (B) is preferably purified using hot water at 90 to 100° C. for about 15 to 30 hours.

[0068] As for the purification method itself, a known method such as a method of immersing the polyamide resin (B) in hot water can be adopted. In this case, for example, the polyamide resin (B) can be purified in the form of a molded body such as pellets.

[0069] The purification step may be performed once or twice or more as needed. By performing sufficient purification, the monomers contained in the polyamide resin can be more completely dissolved in hot water, and the monomer content in the purified polyamide resin can be sufficiently reduced.

[0070] The polyamide resin after the purification step is preferably dried as needed. The drying conditions are not particularly limited. For example, hot air drying at about 100 to 130° C. for about 10 to 30 hours may be performed, but the present invention is not limited thereto. More specifically, hot air drying at 110° C. for 20 hours may be performed.

[0071] Film making process

[0072] In the film-forming step, an unstretched film is produced using a starting material containing the purified polyamide resin (B), and then the unstretched film is stretched.

[0073] As for the above-mentioned starting materials, it is sufficient as long as they contain polyamide resin (B), but other components may be included as needed. For example, in order to improve cost-effectiveness and recovery ratio, it may contain remelted resin (D) obtained by melting polyamide resin (but not including the above-mentioned polyamide resin (B)) within the scope that does not hinder the effect of the present invention. In the present invention, regarding the remelted resin (D), from the standpoints of environmental protection and effective use of resources, resin waste materials of polyamide resin (especially polyamide 6 resin) may be appropriately used. More specifically, particles formed after remelting of unstretched scraps, trimming scraps, slitting scraps, defective products, etc. generated when manufacturing polyamide resin films can be cited.

[0074] In the above-mentioned starting material, the content of the remelting resin (D) is not particularly limited, but from the viewpoint of improving the recovery ratio, it is preferably 1% by mass or more, and more preferably 5% by mass or more. On the other hand, the upper limit of the content of the remelting resin (D) is usually 75% by mass or less, especially preferably 65% ​​by mass or less, further preferably 50% by mass or less, and then more preferably 40% by mass or less, wherein 35% by mass or less is the best. The remelting resin has a tendency to increase the amount of molecular chain ends and decrease viscosity, and the stability of quality is not good. If its content is greater than 75% by mass, the relative viscosity of the film raw material decreases, and foreign matter, thermal degradation products, etc. increase, and there is a tendency to produce problems such as fracture when the film is manufactured. In addition, there is a tendency to decrease the mechanical properties of the film such as tensile elongation decrease. In addition, the content of oligomers such as caprolactam monomers and dimers produced in the stretching process increases, and there will be problems such as the increase in the incidence of broken bags caused by the local decrease in printability and the decrease in adhesion in subsequent processes, and there is a concern that practical performance is affected.

[0075] Film scraps, defective products, etc. used as remelted resins usually contain additives such as lubricants and antioxidants, and the above content includes these additives.

[0076] The concentration of additives such as lubricants, antioxidants, etc. used as film scraps and defective products of the remelted resin varies depending on the product. Therefore, the more the content of the remelted resin in the polyamide resin film, the more likely it is that the haze, wetting tension, printability, adhesion, etc. of the obtained film will be partially reduced due to the uneven concentration distribution of the above-mentioned additives. For this reason, when the polyamide resin film is composed of multiple layers, the remelted resin content of the surface layer (outermost layer) is preferably 50% by mass or less, especially 40% by mass or less, and 35% by mass or less is the best.

[0077] On the other hand, even if the remelted resin content is high in the middle layer (a layer other than the outermost layer), it will not affect the properties of the film surface such as wetting tension and printability, so the remelted resin content can be increased to improve the recovery rate. However, because there is a tendency for the film haze to increase and the physical properties such as impact strength to be poor, the remelted resin content in the middle layer is preferably 75% by mass or less. In addition, the lower limit of the remelted resin content in each layer can be set to about 5% by mass, for example, but is not limited thereto.

[0078] As for other components contained in the starting material, for example, a polyamide resin (C) obtained by polymerizing a raw material composed only of virgin monomers without containing a recycled monomer may be contained.

[0079] Regarding the starting material, if a mixture of a polyamide resin (B) obtained by polymerizing only a recycled monomer and a polyamide resin (C) obtained by polymerizing only a virgin monomer as another resin is used and melt-extruded, physical properties similar to those of a polyamide resin (B) polymerized using both recycled monomers and virgin monomers can be obtained. However, from the perspective of obtaining more uniform film surface properties, it is preferred to polymerize both recycled monomers and virgin monomers. In other words, a polyamide resin (B) composed of a polymer containing recycled monomers and virgin monomers as monomer units can be suitably used.

[0080] The relative viscosity of each polyamide resin contained in the starting material is not limited, but is preferably 2.5 to 4.5, and more preferably 2.8 to 4.0. The use of a polyamide resin with a relative viscosity of less than 2.5 makes film formation and stretching difficult, and even if a polyamide resin film can be produced, the mechanical properties may be significantly reduced. In addition, if a polyamide resin with a relative viscosity greater than 4.5 is used, the film forming property of the film may be hindered.

[0081] In the present invention, the relative viscosity is a value measured by dissolving the resin to be measured in 96% sulfuric acid to a sample solution having a concentration of 1.0 g / dl (liquid temperature 25° C.) using an Ubbelohde viscometer.

[0082] Furthermore, one or more kinds of additives such as antioxidants, ultraviolet absorbers, preservatives, antistatic agents, antiblocking agents, inorganic fine particles, etc. may be added to the starting materials as needed within the range that does not adversely affect the film performance.

[0083] In addition, for the purpose of improving the slipperiness of the obtained film, a lubricant may be mixed in the starting material. As for the lubricant, either an inorganic lubricant or an organic lubricant may be used. Specific examples of the lubricant include clay, talc, calcium carbonate, zinc carbonate, wollastonite, silicon dioxide, aluminum oxide, magnesium oxide, calcium silicate, sodium aluminate, calcium aluminate, magnesium aluminum silicate, hollow glass spheres, carbon black, zinc oxide, antimony trioxide, zeolite, hydrotalcite, layered silicate, vinyl bisstearamide, etc. Among them, silicon dioxide is particularly preferred. The content of the lubricant is not particularly limited, but it is appropriately in the range of 0.01 to 0.3% by mass in the starting material.

[0084] The method for making the unstretched film is not limited, and it can be formed by a known film manufacturing method. For example, the melt of the above raw materials can be extruded from a T-die and then cooled on a casting roll to obtain the film. In this case, from the perspective of making the crystallinity of the unstretched film uniform, the actual temperature of the casting roll surface must be accurately managed.

[0085] In the present invention, it is preferred to first perform a moisture adjustment step as needed, adjust the moisture content of the unstretched film to about 2 to 10% by mass (especially 4 to 8% by mass) and then stretch it. If the moisture content is less than 2% by mass, the tensile stress will increase, making it easy for problems such as film breakage to occur. If the moisture content is greater than 10% by mass, the uneven thickness of the unstretched film will increase, and the uneven thickness of the obtained stretched film will also increase.

[0086] In the water content adjustment process, usually, when the water content of the film is low (especially when it is less than 2% by mass), the film is passed through a water content adjustment tank at a temperature of 40 to 90°C, and more preferably through a water content adjustment tank at a temperature of 50 to 80°C, and the passage time is adjusted to adjust the water content of the film. Pure water is usually used in the water content adjustment tank, but dyes, surfactants, plasticizers, etc. may also be contained in the treatment liquid as needed. In addition, the water content may also be adjusted by spraying water vapor. On the other hand, when the water content of the film is high (especially when it is greater than 10% by mass), the water content of the film may be adjusted by passing the film through a drying furnace and adjusting the passage time.

[0087] Next, the unstretched film is stretched. The stretching method is not particularly limited, and any stretching method can be used. In particular, from the perspective of obtaining a film with excellent tensile elongation in both MD and TD directions, biaxial stretching is preferred.

[0088] There is no limitation on the biaxial stretching method, and examples include simultaneous biaxial stretching and sequential biaxial stretching. For example, from the perspective of surface balance to reduce the difference in physical properties such as tensile elongation, elastic modulus, and tensile strength in the MD and TD directions, the simultaneous biaxial stretching method is preferred; from the perspective of improving puncture strength and impact strength, the sequential biaxial stretching method is preferred. Such stretching methods can be appropriately selected according to the desired film properties, uses, etc.

[0089] The stretching ratio can be appropriately set according to the application and the desired physical properties, for example, 2 to 4 times in the MD direction and 2 to 4 times in the TD direction, but it is not limited thereto. The stretching temperature is also not limited, for example, it can be implemented in the range of 40 to 220°C. In particular, when stretching successively, the MD direction stretching is preferably 40 to 80°C, and the TD direction stretching is preferably 80 to 150°C. In addition, when biaxially stretching simultaneously, it is preferably 160 to 220°C.

[0090] The obtained biaxially stretched film is preferably subjected to a short-term heat treatment at a temperature of about 150 to 220° C., if necessary, in order to improve its dimensional stability and suppress its hot water shrinkage.

[0091] The polyamide resin film of the present invention may be subjected to surface treatments such as corona discharge treatment and adhesion-facilitating treatment within the range that does not impair the effects of the present invention. In addition, an adhesion-facilitating layer, barrier coating, printed layer, etc. may be appropriately provided as needed.

[0092] The polyamide resin film of the present invention thus produced can also be provided as a laminated body laminated with other layers as necessary.

[0093] In addition, a film composed of multiple layers can also be formed by simultaneous melt extrusion, lamination, etc. in the production stage of the polyamide resin film. For example, a two-layer structure of a polyamide resin film containing a polyamide 6 resin containing a polymerized recycled monomer and a polyamide 6 resin film containing a remelted resin can be laminated, a two-layer structure of a polyamide resin film containing a polyamide 6 resin containing a polymerized recycled monomer sandwiching a polyamide 6 resin film containing a remelted resin can be used, etc. If the polyamide 6 resin film has a layer structure with an intermediate layer sandwiched therebetween, such as a two-layer structure, the remelted resin content of the intermediate layer can be increased.

[0094] 2. Polyamide resin film

[0095] The present invention comprises a polyamide resin film, characterized in that a 10% gradation portion of a halftone printing applied to the film has a 1000 mm 2 The number of bad pixels is less than 100.

[0096] (1) Composition of polyamide resin film

[0097] The composition of the polyamide resin is not particularly limited, and examples thereof include polyamide 6 resins having lactams such as ε-caprolactam as monomers. Other polyamide resins include polyamide resins obtained by polycondensation of lactams having three or more rings, ω-amino acids, dibasic acids, diamines, and the like.

[0098] More specifically, as for the lactams, in addition to the ε-caprolactam mentioned above, enantholactam, capryllactam, lauryl lactam and the like can be exemplified.

[0099] Examples of ω-amino acids include 6-aminohexanoic acid, 7-aminoheptanoic acid, 9-aminononanoic acid, and 11-aminoundecanoic acid.

[0100] Examples of the dibasic acids include adipic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, hexadecanedioic acid, eicosanedioic acid, eicosadienedioic acid, 2,2,4-trimethyladipic acid, terephthalic acid, isophthalic acid, 2,6-naphthalene dicarboxylic acid, and xylylenedicarboxylic acid.

[0101] Examples of the diamines include ethylenediamine, trimethylenediamine, tetramethylenediamine, hexamethylenediamine, pentamethylenediamine, undecamethylenediamine, 2,2,4 (or 2,4,4)-trimethylhexamethylenediamine, cyclohexanediamine, bis-(4,4′-aminocyclohexyl)methane, meta-xylylenediamine, nonanediamine, and decanediamine.

[0102] Regarding the polymers obtained by polycondensation or the copolymers thereof, for example, polyamide 6, 7, 10, 11, 12, 4.10, 5.6, 6.6, 6.9, 6.10, 6.11, 6.12, 10.10, 6T, 9T, 10T, 6I, MXD6 (poly(m-xylylene adipamide 6), 6 / 6.6, 6 / 12, 6 / 6T, 6 / 6I, 6 / MXD6, etc. can be cited. Among them, polyamide 6 resin is preferred in terms of excellent balance between heat resistance and mechanical properties. In other words, the polyamide resin film of the present invention is preferably a polyamide 6 resin film.

[0103] (2) Physical properties of polyamide resin film

[0104] The polyamide resin film of the present invention has a 1000 mm thick halftone printing 10% gradation portion applied to the film. 2 The number of bad dots is 100 or less, which is printable. The film with such characteristics has a high reproducibility of the printed appearance, especially the light part in the shade, which is advantageous when printing. Regarding the above number, 80 or less is particularly preferred, and 70 or less is further preferred, and 60 or less is the best. If the above number is greater than 100, even in the low-tone part, unevenness can be visually confirmed by looking at it, and individual differences in the pattern can be felt, which may be judged as poor printing. In addition, the lower limit of the above number is 0 as the best, but for example, 30 or so is also acceptable, and is not limited to this.

[0105] The relative viscosity ηR of the polyamide resin film of the present invention is preferably 2.5 to 4.5, and more preferably 2.8 to 4.0. In addition, the relative viscosity in the present invention is a value measured by dissolving the film to be measured in 96% sulfuric acid into a sample solution with a concentration of 1.0 g / dl (liquid temperature 25°C) using an Ubbelohde viscometer. A polyamide resin film with a relative viscosity of less than 2.5 sometimes has significantly reduced mechanical properties, or sometimes has a reduced evaluation of the bag drop test of the laminated film described later. In addition, a polyamide resin film with a relative viscosity greater than 4.5 is sometimes prone to insufficient uniformity of film thickness and uneven mechanical properties.

[0106] The polyamide resin film of the present invention preferably has a thickness accuracy within plus or minus 15% of the target thickness, and more preferably within plus or minus 10%.

[0107] The polyamide resin film of the present invention has an extraction amount of caprolactam monomer of preferably below 1.6% by mass, more preferably below 1.0% by mass, and more preferably below 0.5% by mass, and most preferably below 0.1% by mass. If the extraction amount of caprolactam monomer of the film is greater than 1.6% by mass, the wettability of the polyamide resin film surface can be easily uneven. In addition, the adhesion of the polyamide resin film to other resin layers or ink may be partially reduced, so there may be a situation where practical performance is reduced, such as the situation where the number of times to the broken bag is reduced in the bag drop test.

[0108] The polyamide resin film of the present invention preferably has a terminal amino group content of 80 mmol / kg or less, and particularly preferably has a terminal carboxyl group content of 70 mmol / kg or less. If the terminal amino group content is greater than 80 mmol / kg, the crystallization rate of the film is accelerated, and localized crystallinity unevenness is likely to occur. As a result, not only the printability of the film is reduced locally, but also the tensile elongation is easily reduced, and physical properties such as impact strength may be easily uneven or partially reduced.

[0109] The polyamide resin film of the present invention preferably has a ratio of the minimum value to the maximum value of the film impact strength under an atmosphere of a temperature of 23° C. and a humidity of 50% RH (minimum value / maximum value) of 0.5 to 1.0, more preferably 0.6 to 1.0, and most preferably 0.7 to 1.0. If the ratio is less than 0.5, it is considered that the impact resistance of the film will be partially reduced, and the practicality is poor.

[0110] The polyamide resin film of the present invention preferably has tensile elongations in both MD and TD directions of 60% or more, more preferably 70% or more.

[0111] The haze of the polyamide resin film of the present invention is preferably 10.0% or less, more preferably 7.0% or less, and most preferably 6.0% or less.

[0112] The polyamide resin film of the present invention is preferably a film obtained by the above-mentioned "1. Method for producing polyamide resin film". In other words, it is preferably a film produced by using a raw material containing a recycled monomer. Therefore, the polyamide resin film of the present invention is preferably a stretched film (particularly a biaxially stretched film). In this way, the above-mentioned various physical properties can be obtained more reliably.

[0113] Therefore, the polyamide resin film of the present invention can be constituted by the polyamide resin film of the regenerated monomer that is polymerized separately, can also be the person who mixes two or more, can also be the polyamide resin film that comprises the remelting resin described later.In addition, can be constituted by a single layer, can also be the film that is constituted by multilayer formed by melt extrusion or lamination simultaneously.For example, the polyamide resin film that contains the polyamide resin of the regenerated monomer that is polymerized, with two kinds of two-layer structures of the polyamide resin film that contains the remelting resin, with the polyamide resin film that contains the polyamide resin of the regenerated monomer that is polymerized sandwiching two kinds of three-layer structures of the polyamide resin film that contains the remelting resin, etc. are all OK.If constituted by multilayer, then the outermost layer of at least one side preferably contains the polyamide resin that is polymerized with the regenerated monomer.

[0114] (3) Use of polyamide resin film

[0115] The polyamide resin film of the present invention (especially the biaxially stretched polyamide resin film) obtained as described above has excellent mechanical properties such as tensile elongation, tensile strength, elastic modulus, etc. as a polyamide resin film. In addition, it also has excellent transparency, color tone, wettability, printability, etc., and can therefore be particularly suitably used as a packaging material.

[0116] The polyamide resin film of the present invention can be used alone or in the form of a laminate with other layers, for example, an easy-adhesion layer, a barrier coating layer, a printing layer, an adhesive layer, etc. can be appropriately provided as needed.

[0117] The polyamide resin film of the present invention can be laminated with a sealant layer of polyolefin or the like by a known method such as dry lamination or extrusion lamination to form a laminated film, and the opposing sealants are heat-fused to each other to be used as a packaging bag (bag body). The bag body can be in any form such as a double-side sealed bag, a three-side sealed bag, a gasket bag, a gusset bag, a side-sealed bag, a stand-up bag, a ziplock stand-up bag, etc.

[0118] The packaged article (contents) is also not limited, and the package can be widely used as a packaging material for, for example, food and beverages, pharmaceuticals, cosmetics, chemicals, sundries, and the like.

[0119] The present invention also includes a laminated film comprising the polyamide resin film of the present invention and a sealant resin layer laminated on the polyamide resin film. Such a laminated film is also suitable for use as a packaging material or a packaging body. The polyamide resin film of the present invention has a uniform surface state, and there is little local precipitation of additives or monomers, etc., and there will be no local decrease in tightness, so the resulting packaging body has excellent resistance to bag breakage. For example, when a packaging body filled with water falls and breaks, it will start to break from the part with low strength, and will start to delaminate from the part with low local tightness and break. In contrast, the laminated film of the present invention has the advantage of being less likely to break compared to existing products.

[0120] More specifically, in the bag drop test of the laminated film of the present invention at 25°C and 55% RH, the number of drops until the bag breaks is preferably 50 or more, more preferably 60 or more, and more preferably 70 or more. In addition, the bag drop test is performed by dropping a package filled with 1000 ml of water and 10 ml of air (using two laminated bodies of 200 mm×300 mm and heat-sealed with a width of 10 mm) from a height of 1.2 m.

[0121] Example

[0122] The following examples and comparative examples are given to explain the features of the present invention in more detail, but the scope of the present invention is not limited to the examples.

[0123] 1. About the raw materials used

[0124] The raw materials used in the examples / comparative examples are shown below. Table 1 shows the time required for the polymerization reaction and the total treatment time for purification in the preparation of each raw material, and also shows the relative viscosity (ηR), the cooling crystallization temperature (Tc) and its half-peak full width, and the monomer content (caprolactam content) of the obtained raw materials.

[0125] Raw materials B2~B4

[0126] Resin scraps (resin waste) are used as the raw material for depolymerization (A), and the resin scraps include film scraps or defective products generated when producing polyamide 6 resin film, oligomers generated during the polymerization of polyamide 6 resin, etc. Phosphoric acid is added to the raw material for depolymerization (A), and a depolymerization reaction is carried out under heating by a wet method, and then the regenerated ε-caprolactam "C-CL" is recovered after being treated with activated carbon, concentrated, and distilled for purification. On the other hand, "V-CL" is ε-caprolactam as a new monomer.

[0127] C-CL and V-CL are prepared so as to have the ratio (mass ratio) shown in Table 1, and mixed with water and benzoic acid as a capping agent, and after heating, pressurizing, depressurizing, and dehydrating in a polymerization kettle, a polymerization reaction is carried out until the target viscosity is reached. The polymerization time required for the final target viscosity varies depending on the ratio of CL types. Each polymerization time is shown in Table 1. After the obtained polymer (resin) is made into pellets, it is purified twice by hot water treatment at 95°C for 10 hours and 15 hours, and then dried at 110°C for 20 hours. In this way, a polyamide resin (raw material B2~4) with a relative viscosity of 3.1 is obtained.

[0128] Raw materials B1, B5

[0129] C-CL, water and benzoic acid as a terminal blocking agent were used as raw materials, and polymerization was performed in the same manner as above to prepare pellets, which were purified twice by hot water treatment at 95°C for 10 hours and 15 hours, respectively, and then dried at 110°C for 20 hours. In this way, a polyamide resin (raw material B1) with a relative viscosity of 3.0 was obtained.

[0130] Separately, polymerization was performed under the same conditions as for the polyamide resin (B1) to prepare pellets, which were then purified by hot water treatment at 95°C for 18 hours and then dried at 110°C for 20 hours. In this manner, a polyamide resin (raw material B5) having a relative viscosity of 2.7 was obtained.

[0131] Raw material B6

[0132] The pellets were polymerized under the same conditions as the polyamide resin (B1), purified by hot water treatment at 95°C for 10 hours, and then dried at 110°C for 20 hours. In this way, a polyamide resin (raw material B6) having a relative viscosity of 2.4 was obtained.

[0133] Raw Material C

[0134] V-CL, water and benzoic acid as a terminal blocking agent were used as raw materials, and polymerization was performed in the same process to prepare pellets, which were purified twice by hot water treatment at 95°C for 10 hours and 10 hours, and then dried at 110°C for 20 hours. In this way, a polyamide resin (raw material C) with a relative viscosity of 3.1 was obtained.

[0135] Raw material D

[0136] Film scraps generated during the production of polyamide 6 resin film were crushed, re-melted at 250-290°C and pelletized. The pellets were then dried to obtain a re-melted resin (raw material D). The relative viscosity of the re-melted resin was 2.9.

[0137] Silica masterbatch E (silica-containing polyamide resin, containing 6% by mass of silica)

[0138] The masterbatch is PCM-30 manufactured by Ikegai Manufacturing Co., Ltd., and is fed from the supply port at a ratio of A1030BRF (polyamide 6 resin manufactured by Unitika Co., Ltd.) / silica 1 (manufactured by Fuji Silicia Chemical Co., Ltd., SILICIA 310P, average particle size 1.4 μm) / silica 2 (manufactured by Mizusawa Chemical Industry Co., Ltd., MIZUKASIL P73, average particle size 2.5 μm) = 94.0 / 4.5 / 1.5, and melt-kneaded under the conditions of a barrel temperature of 230°C to 270°C, a screw speed of 200 rpm, and a discharge volume of 10 kg / hour. The resulting melt-kneaded product is pelletized and vacuum dried (80°C × 24 hours). Silica masterbatch E is thus obtained. The relative viscosity of the silica masterbatch is 3.0.

[0139] Table 1

[0140]

[0141] 2. Examples and Comparative Examples

[0142] A film was produced using the raw materials shown in 1. above.

[0143] Example 1

[0144] Regarding the composition of the polyamide resin film, 97.5% by mass of the polyamide resin (raw material B1) of which only C-CL is polymerized and 2.5% by mass of the silica masterbatch are mixed and melt-kneaded in an extruder, supplied to a T-die and discharged in a sheet form, and wound on a metal drum whose temperature has been adjusted to 20°C, and then rolled up after cooling, thereby obtaining an unstretched film with a thickness of about 150 μm. Next, the obtained unstretched film is immersed in a moisture adjustment tank adjusted to 50°C for 1 minute, and the end is held by the clamp of a tenter-type simultaneous biaxial stretching device, and simultaneously biaxially stretched at 180°C with a stretching ratio of 3.0 times in the MD direction and 3.3 times in the TD direction. Then, after heat treatment at 201°C for 4 seconds with a relaxation rate of 5% in the TD direction, it is slowly cooled to room temperature and corona discharge treated on one side. Then, the film is rolled up to obtain a biaxially stretched polyamide resin film with a thickness of 15 μm. The total recovery ratio in this film is 97.5% by mass. The moisture content of the unstretched film was 5% by mass.

[0145] Example 2

[0146] Regarding the composition of the polyamide resin film, a biaxially stretched polyamide resin film having a thickness of 15 μm was prepared in the same manner as in Example 1 except that 97.5% by mass of the polyamide resin (raw material B5) shown in Table 1 was used. The total recovery ratio in this film was 97.5% by mass.

[0147] Embodiment 3, 5, 13

[0148] Regarding the composition of the polyamide resin film, a biaxially stretched polyamide resin film having a thickness of 15 μm was prepared in the same manner as in Example 1, except that 97.5% by mass of each of the polyamide resins (raw material B4), (raw material B3), or (raw material B2) in Table 1 was used as described in Table 2. The total recovery ratios in the film were 87.8% by mass, 39.0% by mass, and 19.5% by mass, respectively.

[0149] Embodiments 4, 11, 18

[0150] Regarding the composition of the polyamide resin film, a biaxially stretched polyamide resin film with a thickness of 15 μm was prepared in the same manner as in Example 1, except that the polyamide resin (raw material B1) in Table 1 and the polyamide resin (raw material C) were formulated in the ratios described in Table 2 and 97.5% by mass of the resin was used.

[0151] Embodiments 6, 7, 9, 10, 16, 17

[0152] Regarding the composition of the polyamide resin film, a biaxially stretched polyamide resin film with a thickness of 15 μm was prepared in the same manner as in Example 1, except that the polyamide resin (raw material B1) in Table 1 was mixed with the polyamide resin (raw material C) and the remelted resin (raw material D) in the ratios shown in Table 2 and 97.5% by mass of the resin was used.

[0153] Example 8

[0154] Regarding the composition of the polyamide resin film, a biaxially stretched polyamide resin film with a thickness of 15 μm was prepared in the same manner as in Example 1, except that the polyamide resin (raw material B3) in Table 1 and the remelted resin (raw material D) were mixed in the ratios shown in Table 2 and 97.5% by mass of the resin was used.

[0155] Embodiment 14, 15

[0156] Regarding the composition of the polyamide resin film, a biaxially stretched polyamide resin film with a thickness of 15 μm was prepared in the same manner as in Example 1, except that the polyamide resin (raw material B2) in Table 1 and the remelted resin (raw material D) were formulated in the ratios described in Table 2 and 97.5% by mass of the resin was used.

[0157] Example 12

[0158] Regarding the composition of the polyamide resin film, the polyamide resin (raw material B1) in Table 1 and the polyamide resin (raw material C) are mixed in the ratio described in Table 2, and 97.5% by mass of the resin is mixed with 2.5% by mass of a silica masterbatch, and an unstretched film is obtained in the same manner as in Example 1. Next, the unstretched film is stretched 2.8 times in the MD direction with a temperature-controlled roller at 55°C, and then held with a clamp, and stretched at a stretching ratio of 3.7 times in the TD direction at 185°C (successive biaxial stretching). Then, after heat treatment at 201°C for 4 seconds with a relaxation rate of 5% in the TD direction, it is slowly cooled to room temperature and corona discharge treated on one side. Then, the film is rolled up to obtain a biaxially stretched polyamide resin film with a thickness of 15 μm. The total recovery rate in this film is 19.5% by mass. In addition, the moisture content of the unstretched film is 0.5% by mass.

[0159] Embodiment 19

[0160] Two kinds of three-layer films were manufactured at a thickness ratio of 1:1:1 as polyamide resin films. The polyamide resin (raw material C) in Table 1 was mixed at a ratio of 25% by mass with the remelted resin (raw material D) at a ratio of 75% by mass, and the resin was configured as an intermediate layer. The polyamide resin (raw material B3) in Table 1 was configured as two outer layers. An unstretched film was prepared in the same manner as in Example 1, except that 2.5% by mass of a silica masterbatch was mixed in each layer and co-extruded, and a biaxially stretched polyamide resin film with a thickness of 15 μm was prepared by simultaneous biaxial stretching. The total recovery ratio in this film was 50.4% by mass.

[0161] Comparative Example 1

[0162] Regarding the composition of the polyamide resin film, a biaxially stretched polyamide resin film having a thickness of 15 μm was prepared in the same manner as in Example 1 except that 97.5 mass % of the polyamide resin (raw material B6) shown in Table 1 was used.

[0163] Comparative Example 2

[0164] Regarding the composition of the polyamide resin film, a biaxially stretched polyamide resin film having a thickness of 15 μm was produced in the same manner as in Example 1 except that 97.5% by mass of the remelted resin (raw material D) was used.

[0165] Comparative Example 3

[0166] Regarding the composition of the polyamide resin film, a biaxially stretched polyamide resin film having a thickness of 15 μm was produced in the same manner as in Example 12 except that 97.5 mass % of the remelted resin (raw material D) was used.

[0167] Comparative Examples 4 and 5

[0168] Regarding the composition of the polyamide resin film, a biaxially stretched polyamide resin film having a thickness of 15 μm was prepared in the same manner as in Example 1, except that the polyamide resin (C) and the remelted resin (D) were mixed in the ratios shown in Table 2 and 97.5% by mass of the resin was used.

[0169] Comparative Example 6

[0170] Regarding the composition of the polyamide resin film, a biaxially stretched polyamide resin film having a thickness of 15 μm was produced in the same manner as in Example 1 except that 97.5 mass % of the polyamide resin (C) was used.

[0171] Comparative Example 7

[0172] Regarding the composition of the polyamide resin film, 97.5% by mass of polyamide resin (raw material C) and 2.5% by mass of masterbatch (E) were mixed and melt-kneaded in an extruder, supplied to a T-die and discharged in a sheet form, and wound on a metal drum that had been temperature-controlled to 20°C, and then rolled up after cooling, thereby obtaining an unstretched film with a thickness of about 150 μm. At this time, it was confirmed that the actual temperature of the metal drum that had been temperature-controlled to 20°C was uneven, and the crystallinity of the unstretched film was also uneven. In addition, a biaxially stretched polyamide resin film with a thickness of 15 μm was obtained in the same manner as in Example 1. The thickness accuracy of the obtained film was confirmed to exceed plus or minus 15%.

[0173] Table 2

[0174]

[0175] Test Example 1

[0176] The following physical properties were investigated for the raw material polyamide resin (raw material B1 to D) and the films obtained in each example and comparative example. The results are shown in Table 3. In addition, for each measurement, a sample was placed in an environment of temperature 23°C × humidity 50% RH for more than 2 hours and measured in an atmosphere of temperature 23°C × humidity 50% RH.

[0177] (1) Relative viscosity ηR

[0178] The raw material polyamide resin (raw material B1 to D) and the films obtained in the examples and comparative examples were used as samples, and the relative viscosity of the sample solutions (liquid temperature 25° C.) dissolved in 96% sulfuric acid to a concentration of 1.0 g / dl was measured using an Ubbelohde viscometer.

[0179] (2) Moisture content

[0180] Take the unstretched film after water absorption treatment or just before stretching, put it into a weighing bottle and dry it, and calculate the mass change before and after drying.

[0181] (3) Caprolactam monomer content

[0182] [Preparation of measurement samples]

[0183] The raw material polyamide resin (raw material B1 to D) and the membrane obtained in each example and comparative example were freeze-ground, 0.5 g was accurately weighed, and taken into a 10 ml headspace bottle, 10 ml of ultrapure water was added, and after sealing with a butyl rubber stopper and an aluminum cap, extraction was performed in a boiling water bath (100° C.) for 2 hours. After cooling, it was filtered with a 0.45 μm disk filter to prepare a measurement sample.

[0184] [Creation of standard curve]

[0185] 0.1 g of caprolactam was dissolved in 100 ml of ultrapure water to prepare a 1000 ppm solution, which was further diluted to prepare 100, 50, 20, 10, 5, and 2 ppm standard solutions, respectively, to prepare a standard curve.

[0186] [HPLC conditions]

[0187] Apparatus: HP1100 HPLC system manufactured by Hewlett Packard Company, column: Waters Pureisil 5 μm C18 4.6mm×250mm (40℃), detector: UV210nm, injection volume: 10μl, flow rate: 0.7ml / min, elution: with methanol / water (volume ratio: 35 / 75) solution for 12 minutes, then switch to methanol / water (volume ratio: 100 / 0) solution for 30 minutes in 3 minutes, then switch to methanol / water (volume ratio: 35 / 75) solution for 20 minutes in 5 minutes.

[0188] [Calculation method]

[0189] The mass of the monomer in the sample was calculated from the monomer concentration of the sample measured under the above conditions, and the value was divided by the mass of the measured sample to be used as the amount of monomer extracted (mass %).

[0190] (4) Cooling crystallization temperature Tc and half-peak full width

[0191] Using a differential scanning calorimeter (power compensation type DSC8000) manufactured by PerkinElmer, 10 mg of the obtained resin was weighed, and the temperature was raised from room temperature to 260°C at a heating rate of 10°C / min, and after being kept at 260°C for 10 minutes, it was cooled to 100°C at a cooling rate of 10°C / min, and the cooling crystallization temperature was measured. In the DSC curve with heat flow (mW) as the vertical axis and temperature as the horizontal axis, the temperature of the peak top during cooling is Tc (°C), a reference line is drawn from the high temperature side, and the interval between two points with an intensity of 1 / 2 of the absolute value of Tc is the half-peak full width (°C).

[0192] (5) Terminal amino content

[0193] The membranes prepared in the examples and comparative examples were dissolved in a solvent (phenol / ethanol = 4 / 1 by volume), and a certain amount of 0.02N hydrochloric acid was added, followed by back titration with 0.02N sodium hydroxide solution.

[0194] (6) Content of terminal carboxyl groups

[0195] The films prepared in the examples and comparative examples were dissolved in benzyl alcohol at 180° C., phenolphthalein indicator was added, and titration was performed with 0.02 N potassium hydroxide ethanol solution.

[0196] (7) Evaluation of the number of bad dots in halftone printing at 10% of the gradation and evaluation of the expansion of the 40% gradation

[0197] [Printing process]

[0198] The diluent NKFS 102 (TOYOINK) was mixed with Rioalpha R39 blue (TOYOINK), and the viscosity (23°C) was adjusted to 15 seconds in a Zahn cup #3, and the printing ink was used. The film was cut longitudinally at a position 500 mm from the center in the TD direction to prepare a printing film roll. The ink was applied to the film using a Helio engraving tone change plate for gravure printing, dried at 50°C for 10 seconds, and rolled up to prepare a printed film.

[0199] This gradation change version has 175 lines (175 dots per inch), and Helio engraving is performed in the order of gradation 10%, 20%, 30%, 40%, and 100% along the MD direction. The depth of each gradation is 2.5μm, 5.0μm, 7.5μm, 10.0μm, and 32.0μm, respectively. The printing length of each gradation in the MD direction is 60mm, and the printing width in the TD direction is 0.8m.

[0200] Rioalpha R39 blue is mainly composed of 10 mass% pigment, 15 mass% synthetic resin, 2.5 mass% silica, 30 mass% ethyl acetate, 15 mass% isopropyl alcohol, 10 mass% propyl acetate, 10 mass% propylene glycol monomethyl ether, and 5 mass% n-propyl alcohol.

[0201] The diluent NKFS102 is mainly composed of 50 mass % of ethyl acetate, 35 mass % of propyl acetate, 10 mass % of isopropanol, and 5 mass % of n-propanol.

[0202] [Evaluation of the number of bad pixels]

[0203] A total of 10 samples were taken from the 10% tone portion of the printed film, and the samples were magnified 8 times using a stereo microscope (Steore Discovery.V12 manufactured by ZEISS) to calculate a total area of ​​1000 mm in the MD direction (20 mm) and the TD direction (50 mm). 2 The number of defective dots (i.e., unprinted portions) within the range (47,500 dots in total) was evaluated in the same manner at 10 sampled locations, and the value with the largest number of defective dots among all 10 locations is shown in Table 3.

[0204] Figure 1 The outline of the measurement method is shown. In the 10% tone printing area, in the MD direction, excluding the 20mm at the upper and lower ends, the remaining 20mm part, and in the TD direction, starting from the position 100mm from the edge of the film, with the 50mm part as the first point, and a total of 10 points at intervals of 30mm are evaluated. In other words, if Figure 1 As shown, 10 locations in a 20 mm×50 mm measurement area a to j were evaluated.

[0205] As for the number of bad dots, in the total (47500) dots, it is practically sufficient to have 100 or less, particularly preferably 80 or less, further preferably 70 or less, and most preferably 60 or less. If the number is greater than 100, even though it is a low-tone portion, unevenness can be visually confirmed by looking at it, and individual differences in the pattern can be felt, which may be judged as poor printing.

[0206] [Expandability Evaluation]

[0207] The 40% gradation portion of the printed film was magnified 20 times using a stereo microscope (Steero Discovery.V12 manufactured by ZEISS), the dot shape was observed, and the dot diameters of any 10 dots were measured. Evaluation was performed in three levels according to the following evaluation criteria.

[0208] (Evaluation Criteria)

[0209] ◎...No problem was observed in the dot shape, and the ratio of the minimum to maximum dot diameter was greater than 0.9 and less than 1.

[0210] ○ ...No problem was observed in the dot shape, and the ratio of the minimum to maximum dot diameter was 0.85 or more and less than 0.9.

[0211] △...Some deformation is observed in the dot shape, and the ratio of the minimum to maximum dot diameter is greater than 0.75 and less than 0.85.

[0212] ×...The dot shape is deformed and the size is also observed to be uneven, and the ratio of the minimum to maximum dot diameter is less than 0.75.

[0213] (8) Impact strength (J)

[0214] Samples of 10 cm wide and 150 cm long were cut from the center of the obtained polyamide resin film and from a position 50 cm to the left and right of the center in the TD direction. A film impact tester manufactured by Toyo Seiki Seisaku-sho Co., Ltd. was used with a 1 / 2-inch hemispherical hammer head with a diameter of The sample was clamped and fixed by a round hole fixture, and the impact strength was measured 15 times for each. The ratio of the minimum value to the maximum value of the impact strength (minimum value / maximum value) is shown in Table 2. The above ratio is preferably 0.5 to 1.0, more preferably 0.6 to 1.0, and further preferably 0.7 to 1.0. If the above ratio is less than 0.5, it is considered that the impact resistance of the film will be partially reduced, and the practicality is poor.

[0215] (10) Tensile elongation (%)

[0216] The tensile elongation was measured using a DSS-500 Autograph manufactured by Shimadzu Corporation in accordance with Japanese Industrial Standard JIS K7127. A sample with a width of 10 mm and a length of 150 mm was cut from the central portion of the obtained polyamide resin film in the TD direction along the MD direction. The measurement was performed under the conditions of a measuring length of 100 mm (distance between clamps) and a tensile speed of 500 mm / min, and the result was obtained according to the following formula.

[0217] Tensile elongation (%) = Distance moved by the clamp at break (mm) / Distance between original clamps (100mm) × 100

[0218] (11) Haze (%)

[0219] The center portion of the film in the TD direction was measured using a haze meter (NDH4000) manufactured by Nippon Denshoku Co., Ltd. in accordance with Japanese Industrial Standard JIS K7136.

[0220] (12) Wetting tension (mN / m)

[0221] Based on Japanese Industrial Standard JIS K6768, the corona treated surface of the film was measured using mixed solution No. 36.0-54.0 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). The wetting tension was measured at 5 locations in the TD direction, 200 mm apart from the center to both ends. The measurement was performed at 50 locations in the MD direction at intervals of 1 m. The minimum and maximum values ​​of the 50 wetting tension measurement values ​​are shown in Table 3. A wetting tension of 44 mN / m or more is generally practical, and 46 mN / m or more is particularly preferred.

[0222] (13) Bag break resistance (bag drop test)

[0223] [Lamination process]

[0224] A urethane adhesive (DIC Corporation, DICDRY LX-401A / SP-60) was applied in a dry coating amount of 3.0 g / m 2 The adhesive was applied to the film surface and then heat treated at 80°C. Then, an unstretched polyethylene film (TUX MCS, 50 μm, manufactured by Mitsui Chemicals Tohcello) was dry-laminated on the heat-treated adhesive surface at a nip pressure of 490 kPa on a metal roll heated to 80°C. The adhesive was then aged as recommended to obtain a laminated film.

[0225] [Production of bag samples]

[0226] Cut the laminated film into two pieces of 200mm×300mm, put the polyethylene films together, and heat-seal the three sides with a width of 10mm to make a three-side sealed bag. The heat-sealing condition is 160℃×1 second. Fill 1000ml of water into the three-side sealed bag, exhaust the air in the bag, heat-seal the remaining side with a width of 10mm, use a syringe to seal 10ml of air, and heat-seal again to make a sealed test sample. The heat-sealing condition is 160℃×1 second. Adding a small amount of air will increase the damage caused by water to the bag, and the test conditions are more stringent than when there is only water.

[0227] [Bag test]

[0228] The following test A and test B are alternately performed on the prepared test sample until the test sample breaks, and the number of drops of test A or test B until the bag breaks is measured. Test A is to drop the prepared test sample from a height of 1.2 m above a horizontally placed 0.5 mm thick smooth stainless steel plate (SUS plate) with its lower end and make one side of the film surface of the test sample hit the SUS plate; Test B is to drop it so that the short side of one side of the test sample hits the SUS plate.

[0229] In addition, although the test sample has two film surfaces and two short sides, it was dropped so that the same film surface or the same short side hit the SUS plate.

[0230] The test was conducted at 23°C and 50% RH with n=3 samples, and the minimum number of drops until the bag broke is shown in Table 3. Under these conditions, the number of drops until the bag broke is practically required to be 50 or more, preferably 60 or more, and more preferably 70 or more.

[0231] Table 3

[0232]

[0233] These results demonstrate that the biaxially stretched polyamide resin films of Examples 1 to 19 are polyamide resin films made of polyamide resin obtained from polymerized recycled monomers, and therefore have excellent printability in low-tone portions, and uneven impact strength is also controlled. There are no problems with general physical properties such as film elongation, wettability, and haze, and the film also demonstrates excellent practical performance in the bag drop test.

[0234] The raw material used in Comparative Example 1 has a low relative viscosity, and the mechanical properties of the obtained film are reduced, especially the impact strength is low. Therefore, breakage failure occurs in the subsequent process, and normal printing cannot be performed.

[0235] Comparative Examples 2, 4, and 5 do not contain polyamide resin polymerized with recycled monomers. The amount of terminal amino or carboxyl groups from the remelted resin is large, and it is believed that the crystallization rate of the film raw material is accelerated, so that the crystallization state of the surface is locally uneven, resulting in reduced printability of low-tone parts and reduced local adhesion in the bag drop test, making it easy to break the bag. In addition, it can be seen that the elongation is reduced and the impact strength is uneven, which is believed to be caused by impurities in the remelted resin.

[0236] Comparative Example 3 used the same raw materials as Comparative Example 2 and performed sequential stretching. As a result, the monomer content in the film increased. Therefore, the printability of the low-tone portion was locally reduced, and the result of the bag drop test was also poor. It was also found that the elongation was reduced and the impact strength was uneven, which was believed to be caused by impurities in the remelted resin.

[0237] Comparative Example 6 is a film obtained using a polyamide resin composed only of new monomers. No problems were observed in general physical properties and practical performance, but the reproducibility of printability in low-tone areas was inferior to that of the film using recycled monomers.

[0238] Comparative Example 7 uses a polyamide resin composed only of new monomers, but the temperature control of the casting roll is insufficient, resulting in uneven crystallinity on the surface of the unstretched film, and thus uneven crystallinity on the surface of the stretched film, resulting in reduced printability of the low-tone portion. In addition, it was observed that the accuracy of the film thickness after stretching was greater than 15%, resulting in uneven impact strength and elongation.

Claims

1. A method for producing a polyamide resin film, characterized in that: The method for producing the polyamide resin film comprises the following steps: Step (1), generating a monomer containing ε-caprolactam from a depolymerization raw material A, wherein the depolymerization raw material A is at least one of a polyamide 6 resin and an oligomer thereof; Step (2), polymerizing a raw material containing the monomer to produce a polyamide resin B having a half-maximum width of a crystallization peak of 10° C. or more; Step (3), purifying the polyamide resin B so that the relative viscosity ηR of the purified polyamide resin B is 2.5 to 4.5; and In step (4), an unstretched film is produced using the starting material containing the purified polyamide resin B, and then the unstretched film is stretched.

2. The manufacturing method according to claim 1, wherein: The method further includes the step of adjusting the moisture content of the unstretched film to 2% by mass to 10% by mass before stretching.

3. The manufacturing method according to claim 1, wherein: As a part of the starting materials, a re-melted resin obtained by melting a polyamide resin excluding the polyamide resin B is contained in an amount of 1% by mass or more.

4. The manufacturing method according to claim 1, wherein: The relative viscosity ηR of the purified polyamide resin B is 2.8 to 4.

0.

5. A biaxially stretched polyamide resin film, wherein: 1000mm of 10% gradation of halftone printing applied to film 2 The number of bad spots is less than 100, the caprolactam monomer concentration in the polyamide resin film is less than 1.6 mass%, the contents of terminal amino groups and terminal carboxyl groups in the polyamide resin film are less than 80 mmol / kg respectively, and the polyamide resin includes a half-peak full width of a cooling crystallization peak of more than 10°C.

6. The polyamide resin film according to claim 5, wherein The caprolactam monomer concentration in the polyamide resin film is 0.1 mass % or less.

7. The polyamide resin film according to claim 5, wherein The contents of the terminal amino group and the terminal carboxyl group in the polyamide resin film are each 70 mmol / kg or less.

8. The polyamide resin film according to claim 5, wherein the ratio of the minimum value to the maximum value of the film impact strength in an atmosphere of a temperature of 23°C and a humidity of 50%RH, that is, minimum value / maximum value, is 0.5 to 1.

0.

9. The polyamide resin film according to claim 5, wherein A polyamide resin having a temperature drop crystallization peak and a full width at half maximum of 11°C or more. 10 . The polyamide resin film according to claim 5 , which has a haze of 10.0% or less.

11. The polyamide resin film according to claim 5, which has a relative viscosity ηR at 25°C of 2.5 to 4.

5. 12 . A laminated film comprising the polyamide resin film according to claim 5 , and a sealant resin layer laminated on the polyamide resin film. 13 . A packaging material comprising the polyamide resin film according to claim 5 . 14 . A polyamide resin film produced by the production method according to claim 1 .