A method for preparing micro-nano composite structures by droplet forming based on electric field action
Through the droplet molding method of electric field, corona discharge and ionic wind are used to form a micro-nano droplet array. Combined with vapor condensation and interfacial tension, the flexible morphology regulation and curing of the micro-nano composite structure is achieved, and the existing technology is solved The problems of complex process and single materials have achieved low-cost and simple preparation of micro-nano composite structures.
Patent Information
- Application Number
- CN202210547989.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-18
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-05-18
AI Technical Summary
The existing micro-nano composite structure preparation technology has the problem of complex process, relying on precision equipment and special materials, and the laser swelling method is inefficient and cannot be directly applied to optical performance regulation.
The droplet molding method based on electric field action is adopted to form a micro-nano droplet array through corona discharge and ionic wind action, and combine vapor condensation and interface tension to achieve flexible morphological regulation and curing of the micro-nano composite structure.
It realizes simple and low-cost preparation of micro-nano composite structures, and flexible regulation of process parameters, solves the problems of complex preparation process of micro-nano composite structures and the applicability of single materials, and improves the flexibility and controllability of structural morphology.
Smart Images

Figure CN115043374B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a technology for preparing micro-nano structures on the surface of organic colloids, and in particular to a method for preparing micro-nano composite structures by a droplet forming method based on electric field action. Background Art
[0002] Driven by the application demands of micro-nano composite structures in optoelectronics and imaging, their fabrication techniques have also been studied. Currently, the predominantly used two-step mold imprinting technique involves the separate imprinting of primary microstructures and secondary nanostructures. The imprinting process for both micro and nanostructures involves mold fabrication and imprint molding. Mold fabrication creates the micro / nanostructures on the mold, while imprint molding transfers the mold pattern to the polymer surface. However, mold fabrication for micro / nanostructures is complex and costly, relying on expensive precision equipment. Furthermore, the composite of micro and nanostructures requires specialized materials (temperature-reversible materials) or specialized structures (flexible molds). Other researchers have proposed using nanoimprinting to fabricate nanostructures, followed by laser swelling to fabricate microstructures. The laser swelling method, which uses lasers to fabricate microstructures one by one, is inefficient and only applicable to specialized material systems (PMMA doped with methyl red to achieve laser absorptivity control), making it incapable of directly manipulating optical properties. In addition, some scholars have proposed using photolithography reflow to prepare microstructures, then preparing nanostructures through nanosphere self-assembly, and finally obtaining micro-nano composite structures through two imprint transfers. The process is complex and the preparation of large-area single-layer nanosphere films is very challenging.
[0003] Existing technologies for fabricating micro-nano composite structures still have numerous shortcomings. The separate fabrication steps for microstructures and nanostructures significantly increase the complexity of the process. The fabrication of micro-nanoimprint molds relies on precision equipment and is only suitable for specialized materials or structures. The emerging laser swelling method suffers from low efficiency and limited material compatibility. Therefore, developing low-cost, simpler technologies for fabricating micro-nano composite structures is of vital importance. Summary of the Invention
[0004] The object of the present invention is to provide a method for preparing a micro-nano composite structure by a droplet forming method based on electric field action, which can achieve flexible regulation of the morphology parameters of the micro-nano composite structure.
[0005] The object of the present invention is achieved like this:
[0006] A first preparation method of a micro-nano composite structure by a droplet forming method based on electric field action is characterized by comprising the following steps:
[0007] A. Prepare a lower electrode, place the lower electrode on a temperature-controlled platform, and cover the surface of the lower electrode with a first polymer, wherein the first polymer is in a liquid state;
[0008] B. Prepare the upper electrode and use a DC power supply to apply voltage between the upper and lower electrodes. By applying an electric field between electrodes with large curvature differences, corona discharge is achieved. Gas molecules are ionized to generate charges that move toward the lower electrode under the action of Coulomb force. Figure 1 As shown in (a); the charge accumulates on the surface of the non-conductive first polymer, and the electric field force drives the first polymer to flow, so that the first polymer is patterned, and the micron-scale first polymer droplet formation is achieved, as shown Figure 1 As shown in (b); after the ionic wind action is stabilized, the first polymer microdroplet array is finally obtained, as shown in Figure 1 As shown in (c); by changing the electric field effect such as voltage, upper and lower electrode spacing and gel layer thickness, the morphology of the first polymer microdroplet is adjusted to affect the effect of charge on the polymer;
[0009] C. Prepare a vapor atmosphere control system, and adjust the temperature of the first polymer micro-droplet array through the refrigeration effect of the temperature control platform, so that the temperature of the first polymer micro-droplet array is lower than the ambient temperature, resulting in a decrease in the fluidity of the first polymer, and a conformal effect on the first polymer micro-droplet array. At the same time, the vapor condenses and nucleates on the surface of the first polymer micro-droplet array. The upper electrode is needle-shaped and the lower electrode is plate-shaped. The electric field effect is introduced in the needle-plate electrode configuration with a large difference in curvature to achieve corona discharge. The charge injection and compound effect generated by the discharge avoid the aggregation of droplets in the condensation nucleation process, and the regulation of the condensation nucleation process of the second nano-droplet is achieved, and finally the second nano-droplet array is obtained, such as Figure 2 As shown; for the formation of the second nanodroplet, the electric field effect can be controlled by changing the voltage, electrode shape and electrode spacing; the lower electrode with the first polymer microdroplet array on the temperature control platform is placed in a water vapor atmosphere controlled by humidified airflow in a humidity control system. After condensation for a set time, the vapor self-assembles into a second nanodroplet array on the surface of the first polymer microdroplet array. Due to the effect of surface tension, part of the second nanodroplet array enters the interior of the first polymer microdroplet array, as shown Figure 3 As shown in (a); wherein the second nanodroplet is immiscible with the first polymer;
[0010] D. preparing a substrate and covering the surface of the substrate with a second polymer, wherein the second polymer is immiscible with the first polymer and the second nanodroplet;
[0011] E. Covering the second polymer on the substrate on the first polymer microdroplet array with the second nanodroplet array, introducing the second polymer to replace the air layer, changing the original first polymer-second nanodroplet-air three-phase interface into a first polymer-second nanodroplet-second polymer three-phase interface, and changing the morphology of the second nanodroplet through interfacial tension to form a stable first polymer-second nanodroplet-second polymer three-phase interface, such as Figure 3 As shown in (b);
[0012] F. Curing the first polymer until it is completely cured to obtain a first microstructure array. Due to the imprinting effect of the second nanodroplet array, a curved second nanostructure array corresponding to the second nanodroplet array is obtained on the surface of the first polymer microstructure array;
[0013] G. Peeling off the substrate, removing the second nanodroplet array and the second polymer on the surface of the first polymer microstructure array, and obtaining a micro-nano composite structure array, such as Figure 3 As shown in (c) in .
[0014] Furthermore, the material of the lower electrode in step A is one of ITO conductive glass, conductive graphite, aluminum, copper, or glass, ceramic, silica gel, and polystyrene with a patterned electrode on the surface, and the patterned electrode is a periodic structure array with a circle, triangle, square, or regular hexagonal pattern; when the lower electrode is a patterned electrode, the charge moves only to the area of the patterned electrode, thereby achieving the effect of applying ion wind to a specific area, such as Figure 4 As shown in (a); the charges accumulate on the surface of the first polymer, and the electric field force drives the first polymer to flow, as shown in Figure 4 As shown in (b); after the ion wind action is stable, the microstructure array distribution is the same as the pattern distribution of the patterned electrode, and the period is equal, and finally the first polymer concave droplet array corresponding to the electrode pattern of the lower electrode is obtained, as shown in FIG. Figure 4 As shown in (c) in the figure; by changing the pattern size and distribution in the patterned electrode, the charge space distribution is affected, thereby achieving the morphology control of the first polymer microdroplet.
[0015] Furthermore, the upper electrode described in step B is a needle tip electrode or a needle tip electrode array, the distance between the upper electrode and the lower electrode is adjustable within 5mm-200mm, and a voltage is applied using a DC power supply, and the voltage adjustment range is continuously adjustable within 1000V-15000V; or, a graphic through-hole template is provided between the upper electrode and the lower electrode, and the graphic through-hole template has a periodic structure array of circular, triangular, square or regular hexagonal shapes; the charge moves only from the through-hole area of the graphic through-hole template to the lower electrode, thereby realizing a graphic ion wind effect, such as Figure 5As shown in (a) in FIG; after the charges pass through the through hole, they accumulate on the surface of the first polymer, and the electric field force drives the first polymer to flow, as shown in FIG. Figure 5 As shown in (b); after the ion wind action is stable, the microstructure array distribution is the same as the pattern distribution of the patterned through-hole template, and the period is equal, and finally the first polymer convex droplet array corresponding to the pattern of the patterned through-hole template is obtained, as shown in FIG. Figure 5 As shown in (c) in the figure, the morphology of the first polymer microdroplet is adjusted by changing the pattern size and distribution in the patterned through-hole template.
[0016] Furthermore, the vapor atmosphere control system described in step C can realize the vapor atmosphere and ensure the control of the vapor atmosphere concentration. The vapor atmosphere is one or more of water, methanol, ethanol, ethylene glycol or propylene glycol, and the concentration control range of the vapor atmosphere is 10%~90%; the control range of the control temperature Tc of the temperature control platform is -20~300°C, the condensation time of the second nanodroplet is 1~30min, and the diameter of the obtained second nanodroplet is 0.1~10μm.
[0017] Furthermore, the material of the substrate in step D is one of glass, silica gel, polystyrene, polycarbonate or polymethyl methacrylate high light transmittance materials.
[0018] Furthermore, the first polymer described in step A is covered on the surface of the lower electrode by dot coating, spraying or spin coating, and the thickness of the first polymer is 5~1000μm, and the first polymer is a liquid dielectric polymer at room temperature and pressure; the second polymer described in step D is covered on the surface of the substrate by dot coating, spraying or spin coating, and the thickness of the second polymer is 5~1000μm, and the first polymer is a liquid polymer at room temperature and pressure.
[0019] Furthermore, the first polymer is a UV-curable polymer, the second polymer is a non-UV-curable polymer, and the corresponding curing method in step F is to completely cure the first polymer by UV lamp irradiation, and the curing time is 1 to 30 minutes; or, the first polymer in step A is a heat-curable polymer, and the second polymer is a non-heat-curable polymer, and the corresponding curing method in step F is to completely cure the first polymer by heat curing, and the curing time is 10 to 300 minutes.
[0020] A second preparation method of a micro-nano composite structure using a droplet forming method based on electric field action is characterized by comprising the following steps:
[0021] A. Prepare a lower electrode, place the lower electrode on a temperature-controlled platform, and cover the surface of the lower electrode with a first polymer, wherein the first polymer is in a liquid state;
[0022] B. Prepare the upper electrode and use a DC power supply to apply voltage between the upper and lower electrodes. By applying an electric field between electrodes with large curvature differences, corona discharge is achieved. Gas molecules are ionized to generate charges that move toward the lower electrode under the action of Coulomb force. Figure 1 As shown in (a); the charge accumulates on the surface of the non-conductive first polymer, and the electric field force drives the first polymer to flow, so that the first polymer is patterned, and the micron-scale polymer droplet formation is achieved, as shown in FIG. Figure 1 As shown in (b); after the ionic wind action is stabilized, the first polymer microdroplet array is finally obtained, as shown in Figure 1 As shown in (c); by changing the electric field effect such as voltage, upper and lower electrode spacing and gel layer thickness, the morphology of the first polymer microdroplet is adjusted to affect the effect of charge on the polymer;
[0023] C. Prepare a vapor atmosphere control system, and adjust the temperature of the first polymer micro-droplet array through the refrigeration effect of the temperature control platform, so that the temperature of the first polymer micro-droplet array is lower than the ambient temperature, resulting in a decrease in the fluidity of the first polymer, and a conformal effect on the first polymer micro-droplet array. At the same time, the vapor condenses and nucleates on the surface of the first polymer micro-droplet array. The upper electrode is a needle electrode, and the lower electrode is a plate electrode. The needle-plate electrode configuration with a large curvature difference introduces an electric field to achieve corona discharge. The charge injection and compound effect generated by the discharge avoid the convergence of droplets in the condensation nucleation process. By regulating the droplet condensation nucleation process, the second nano-droplet formation at the nanoscale is achieved, such as Figure 2 As shown; for the formation of the second nanodroplet, the electric field effect can be controlled by changing the voltage, electrode shape and electrode spacing; the lower electrode with the first polymer microdroplet array on the temperature control platform is placed in a water vapor atmosphere controlled by humidified airflow in a humidity control system. After condensation for a set time, the vapor self-assembles into a second nanodroplet array on the surface of the first polymer microdroplet array. Due to the effect of surface tension, part of the second nanodroplet array enters the interior of the first polymer microdroplet array, as shown Figure 3 As shown in (a); wherein the second nanodroplet is immiscible with the first polymer;
[0024] D. preparing a substrate and covering the surface of the substrate with a second polymer, wherein the second polymer is immiscible with the first polymer and the second nanodroplet;
[0025] E. Covering the second polymer on the substrate on the first polymer microdroplet array with the second nanodroplet array, introducing the second polymer to replace the air layer, changing the original first polymer-second nanodroplet-air three-phase interface into a first polymer microdroplet-second nanodroplet-second polymer three-phase interface, and changing the morphology of the second nanodroplet through interfacial tension to form a stable first polymer-second nanodroplet-second polymer three-phase interface, such as Figure 3 As shown in (b);
[0026] F. Curing the second polymer until it is completely cured to obtain a first microstructure array. Due to the imprinting effect of the second nanodroplet array, a curved second nanostructure array corresponding to the second nanodroplet array is obtained on the surface of the first polymer microstructure array;
[0027] G. Peeling off the substrate, removing the second nanodroplet array and the first polymer on the surface of the second polymer microstructure array, and obtaining a micro-nano composite structure array, such as Figure 3 As shown in (c) in .
[0028] Furthermore, the lower electrode material in step A is one of ITO conductive glass, conductive graphite, aluminum, copper, or glass, ceramic, silicone, and polystyrene with a patterned electrode on the surface, and the patterned electrode has a periodic structural array of circular, triangular, square, or regular hexagonal shapes; when the lower electrode is a patterned electrode, the charge moves only to the patterned electrode area, thereby achieving the effect of applying ion wind to a specific area, such as Figure 4 As shown in (a); the charges accumulate on the surface of the first polymer, and the electric field force drives the first polymer to flow, as shown in Figure 4 As shown in (b); after the ion wind action is stable, the microstructure array distribution is the same as the pattern distribution of the patterned electrode, and the period is equal, and finally the first polymer concave droplet array corresponding to the electrode pattern of the lower electrode is obtained, as shown in FIG. Figure 4 As shown in (c) in the figure; by changing the pattern size and distribution in the patterned electrode, the charge space distribution is affected, thereby achieving the morphology control of the first polymer microdroplet.
[0029] Furthermore, the upper electrode described in step B is a needle tip electrode or a needle tip electrode array, the distance between the upper electrode and the lower electrode is adjustable within 5mm-200mm, and a voltage is applied using a DC power supply, and the voltage adjustment range is continuously adjustable within 1000V-15000V; or, a graphic through-hole template is provided between the upper electrode and the lower electrode, and the graphic through-hole template has a periodic structure array of circular, triangular, square or regular hexagonal shapes; the charge moves only from the through-hole area of the graphic through-hole template to the lower electrode, thereby realizing a graphic ion wind effect, such as Figure 5As shown in (a) in FIG; after the charges pass through the through hole, they accumulate on the surface of the first polymer, and the electric field force drives the first polymer to flow, as shown in FIG. Figure 5 As shown in (b); after the ion wind action is stable, the microstructure array distribution is the same as the pattern distribution of the patterned through-hole template, and the period is equal, and finally the first polymer convex droplet array corresponding to the pattern of the patterned through-hole template is obtained, as shown in FIG. Figure 5 As shown in (c) in the figure, the morphology of the first polymer microdroplet is adjusted by changing the pattern size and distribution in the patterned through-hole template.
[0030] Furthermore, the vapor atmosphere control system described in step C can realize the vapor atmosphere and ensure the control of the vapor atmosphere concentration. The vapor atmosphere is one or more of water, methanol, ethanol, ethylene glycol or propylene glycol, and the concentration control range of the vapor atmosphere is 10%~90%; the control range of the control temperature Tc of the temperature control platform is -20~300°C, the condensation time of the second nanodroplet is 1~30min, and the diameter of the obtained second nanodroplet is 0.1~10μm.
[0031] Furthermore, the material of the substrate in step D is one of glass, silica gel, polystyrene, polycarbonate or polymethyl methacrylate high light transmittance materials.
[0032] Furthermore, the first polymer described in step A is covered on the surface of the lower electrode by dot coating, spraying or spin coating, and the thickness of the first polymer is 5~1000μm, and the first polymer is a liquid dielectric polymer at room temperature and pressure; the second polymer described in step D is covered on the surface of the substrate by dot coating, spraying or spin coating, and the thickness of the second polymer is 5~1000μm, and the second polymer is a liquid polymer at room temperature and pressure.
[0033] Furthermore, the second polymer is a UV-curable polymer, the first polymer is a non-UV-curable polymer, and the corresponding curing method in step F is to completely cure the second polymer by UV lamp irradiation, and the curing time is 1 to 30 minutes; or, the second polymer in step D is a heat-curable polymer, the first polymer is a non-heat-curable polymer, and the corresponding curing method in step F is to completely cure the second polymer by heating curing, and the curing time is 10 to 300 minutes.
[0034] The present invention uses the ionic wind effect of corona discharge induced by electric field action to realize the formation of polymer droplet array, and then condenses and self-assembles on the surface of the first polymer micro-droplet array through the active refrigeration vapor condensation method of charge injection composite action to obtain a second nano-droplet array, then introduces a second polymer, and finally solidifies the first or second polymer to obtain a first microstructure array. Due to the imprinting effect of the second nano-droplet array, a curved second nanostructure array corresponding to the second nano-droplet array is obtained on the surface of the first microstructure array, thereby obtaining a micro-nano composite structure array. By adjusting the corresponding process parameters, flexible control of the morphology parameters of the micro-nano composite structure array can be achieved.
[0035] Compared with the existing technology, the above technical solution proposed in the present invention has the following characteristics: the preparation of micro-nano composite structure arrays is realized by using micro-nano composite droplet molding, and the flexible regulation of micro-nano composite structure morphology parameters is realized by adjusting the micro-nano composite droplet molding process parameters. This technical solution has the advantages of simple process, low cost and flexible and controllable micro-nano composite structure morphology, which solves the problems of complex micro-structure and nanostructure distribution preparation process of current micro-nano composite structure preparation methods, dependence of micro / nano imprint mold preparation on precision equipment, and only applicable to special materials or structures. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 Schematic diagram of the principle of ion wind forming microstructure in the preparation method of micro-nano composite structure, where Figure 1 (a) is a schematic diagram of the ion wind motion principle. Figure 1 (b) is a schematic diagram of the principle of the first polymer morphology change. Figure 1 (c) is a schematic diagram of the microstructure forming principle;
[0037] Figure 2 Schematic diagram of the second nanodroplet forming principle in the micro-nano composite structure preparation method;
[0038] Figure 3 Schematic diagram of the principle of regulating the morphology of the second nanodroplet by the second polymer in the preparation method of the micro-nano composite structure, wherein Figure 3 (a) is a schematic diagram of the second nanodroplet sinking into the first polymer droplet. Figure 3 (b) is a schematic diagram of the principle of the second nanodroplet morphology change. Figure 3 (c) is a schematic diagram of the micro-nano composite structure prepared by curing the second polymer. Figure 3 (d) is a schematic diagram of the micro-nano composite structure prepared by curing the first polymer;
[0039] Figure 4 Schematic diagram of the principle of controlling the morphology of the ion wind-molded microstructure by the patterned electrode in the preparation method of the micro-nano composite structure. Figure 4 (a) is a schematic diagram of the ion wind motion principle. Figure 4 (b) is a schematic diagram of the principle of the first polymer morphology change. Figure 4 (c) is a schematic diagram of the microstructure forming principle;
[0040] Figure 5 Schematic diagram of the principle of controlling the morphology of ion wind-molded microstructures by using a patterned through-hole template in the preparation method of micro-nano composite structures. Figure 5 (a) is a schematic diagram of the ion wind motion principle. Figure 5 (b) is a schematic diagram of the principle of the first polymer morphology change. Figure 5 (c) is a schematic diagram of the microstructure forming principle;
[0041] Figure 6 This is a schematic diagram before the action of ion wind in step 2 of the experimental process of the method for preparing a micro-nano composite structure in Example 1 of the present invention;
[0042] Figure 7 This is a schematic diagram of the process after the ion wind acts in step 2 of the experimental process in the method for preparing a micro-nano composite structure in Example 1 of the present invention;
[0043] Figure 8 Schematic diagram of water droplet condensation in step 3 of the experimental process of the method for preparing a micro-nano composite structure in Example 1 of the present invention;
[0044] Figure 9 Schematic diagram of step 4 of the experimental process in the method for preparing a micro-nano composite structure in Example 1 of the present invention;
[0045] Figure 10 Schematic diagram of step 5 of the experimental process in the method for preparing a micro-nano composite structure in Example 1 of the present invention;
[0046] Figure 11 Schematic diagram of step 6 of the experimental process of the method for preparing a micro-nano composite structure in Example 1 of the present invention;
[0047] Figure 12 Schematic diagram of the micro-nano composite structure array obtained in the method for preparing a micro-nano composite structure in Example 1 of the present invention;
[0048] Figure 13 This is a schematic diagram before the action of ion wind in step 2 of the experimental process of the method for preparing a micro-nano composite structure in Example 2 of the present invention;
[0049] Figure 14 A top view of a patterned through-hole template in a method for preparing a micro-nano composite structure;
[0050] Figure 15 This is a schematic diagram of the process after the ion wind acts in step 2 of the experimental process in the method for preparing a micro-nano composite structure in Example 2 of the present invention;
[0051] Figure 16Schematic diagram of water droplet condensation in step 3 of the experimental process of the method for preparing a micro-nano composite structure in Example 2 of the present invention;
[0052] Figure 17 Schematic diagram of step 4 of the experimental process of the method for preparing a micro-nano composite structure in Example 2 of the present invention;
[0053] Figure 18 Schematic diagram of step 5 of the experimental process in the method for preparing a micro-nano composite structure in Example 2 of the present invention;
[0054] Figure 19 Schematic diagram of step 6 of the experimental process of the method for preparing a micro-nano composite structure in Example 2 of the present invention;
[0055] Figure 20 Schematic diagram of the micro-nano composite structure array obtained in the method for preparing a micro-nano composite structure in Example 2 of the present invention;
[0056] Figure 21 This is a schematic diagram before the action of ion wind in step 2 of the experimental process in the method for preparing a micro-nano composite structure in Example 3 of the present invention;
[0057] Figure 22 A top view of a patterned electrode in a method for preparing a micro-nano composite structure;
[0058] Figure 23 This is a schematic diagram of the process after the ion wind acts in step 2 of the experimental process in the method for preparing a micro-nano composite structure in Example 3 of the present invention;
[0059] Figure 24 Schematic diagram of water droplet condensation in step 3 of the experimental process of the method for preparing a micro-nano composite structure in Example 3 of the present invention;
[0060] Figure 25 Schematic diagram of step 4 of the experimental process in the method for preparing a micro-nano composite structure in Example 3 of the present invention;
[0061] Figure 26 Schematic diagram of step 5 of the experimental process in the method for preparing a micro-nano composite structure in Example 3 of the present invention;
[0062] Figure 27 Schematic diagram of step 6 of the experimental process of the method for preparing a micro-nano composite structure in Example 3 of the present invention;
[0063] Figure 28 Schematic diagram of the micro-nano composite structure array obtained in the method for preparing a micro-nano composite structure in Example 3 of the present invention;
[0064] Figure 29 Schematic diagram of water droplet condensation in step 3 of the experimental process of the method for preparing a micro-nano composite structure in Example 4 of the present invention;
[0065] Figure 30Schematic diagram of step 6 of the experimental process of the method for preparing a micro-nano composite structure in Example 4 of the present invention;
[0066] Figure 31 Schematic diagram of the micro-nano composite structure array obtained in the method for preparing a micro-nano composite structure in Example 4 of the present invention;
[0067] Figure 32 Schematic diagram of step 6 of the experimental process in the method for preparing a micro-nano composite structure in Example 5 of the present invention;
[0068] Figure 33 Schematic diagram of the micro-nano composite structure array obtained in the method for preparing a micro-nano composite structure in Example 5 of the present invention;
[0069] Figure 34 Schematic diagram of step 6 of the experimental process of the method for preparing a micro-nano composite structure in Example 6 of the present invention;
[0070] Figure 35 Schematic diagram of the micro-nano composite structure array obtained in the method for preparing a micro-nano composite structure in Example 6 of the present invention;
[0071] Figure 36 This is a schematic diagram of step 2 of the experimental process in the method for preparing a micro-nano composite structure in Example 7 of the present invention. DETAILED DESCRIPTION
[0072] The present invention will be further described below with reference to the embodiments and accompanying drawings.
[0073] Example 1:
[0074] like Figure 6-12 As shown, a method for preparing a micro-nano composite structure by a droplet forming method based on electric field action includes the following steps:
[0075] 1. Prepare a lower electrode 101, ground the lower electrode 101, and place the lower electrode 101 on a temperature-controlled platform 102. Spin-coat the surface of the lower electrode 101 with a first polymer 104 to obtain a first polymer 104 with a thickness of 5 μm. The first polymer is a thermosetting polymer.
[0076] 2. Prepare an upper electrode 103, which is a needle-tip electrode. Place the upper electrode 103 100 mm above the lower electrode 101. Use a DC power supply 106 to apply a voltage of 15,000 V between the upper electrode 103 and the lower electrode 101. The upper electrode 103 is the positive electrode. This causes the first polymer 104 to deform under the action of the ionic wind generated by the electric field, resulting in a first polymer microdroplet array 105 with a convex morphology and a droplet diameter of 10 μm.
[0077] 3. The lower electrode 101 having the first polymer micro-droplet array 105 on the temperature control platform 102 is placed in a water vapor atmosphere controlled by a vertical humidified airflow 107 in a humidity control system. The temperature of the first polymer micro-droplet array 105 is regulated by the refrigeration effect of the temperature control platform 102, so that the temperature of the first polymer micro-droplet array 105 is lower than the ambient temperature, thereby causing water vapor to condense and form nuclei on the surface of the first polymer micro-droplet array 105. The electric field between the lower electrode 101 and the upper electrode 103 prevents the aggregation of droplets during the condensation nucleation process, thereby achieving nanoscale droplet formation. After a condensation time of 1 minute, the water vapor self-assembles on the surface of the first polymer micro-droplet array 105 into a uniformly distributed second nano-droplet array 108 with a diameter of 0.1 μm. Due to the effect of surface tension, the second nano-droplet array 108 partially enters the interior of the first polymer micro-droplet array 105. The ambient temperature Ta is controlled to be 20° C., the water vapor atmosphere concentration is controlled to be 90%, and the control temperature Tc of the temperature control platform 102 is -20° C.
[0078] 4. Prepare a substrate 109, which is a PMMA plate. Spin-coat the second polymer 110 on the surface of the substrate 109 to form a 200 μm thick second polymer 110 on the substrate 109. The second polymer 110 is a UV-curable polymer.
[0079] 5. Covering the second polymer 110 on the substrate 109 on the first polymer microdroplet array 105 having the second nanodroplet array 108, wherein the second polymer 110 faces downward. Under the action of surface tension, the second nanodroplet array 108 on the surface of the first polymer microdroplet array 105 is pressed into the interior of the second polymer 110, forming a stable first polymer-second nanodroplet-second polymer three-phase interface;
[0080] 6. The second polymer 110 is completely cured by irradiation with an ultraviolet lamp 112, thereby obtaining a curved second nanostructure array corresponding to the second nanodroplet array 108 on the surface of the first polymer microdroplet array 105, wherein the ultraviolet irradiation energy is 3W / cm 2 , curing time is 20min;
[0081] 7. Peel the substrate 109 from the surface of the lower electrode 101, and clean the surface of the second polymer 110 on the surface of the substrate 109 with acetone and deionized water respectively to remove the second nanodroplet array 108 and the first polymer microdroplet array 105, finally obtaining a micro-nano composite structure array 111.
[0082] Example 2:
[0083] like Figure 13-20As shown, a method for preparing a micro-nano composite structure by a droplet forming method based on electric field action includes the following steps:
[0084] 1. Prepare a lower electrode 201, ground the lower electrode 201, and place the lower electrode 201 on a temperature-controlled platform 202. Spray a first polymer 204 onto the surface of the lower electrode 201 to obtain a first polymer 204 having a thickness of 50 μm. The first polymer is a thermosetting polymer.
[0085] 2. Prepare an upper electrode 203, which is a needle-tip electrode array. Place the upper electrode 203 200 mm above the lower electrode 201. Set a patterned through-hole template 213 between the upper and lower electrodes. The patterned through-hole template 213 has a circular structure array with a regular quadrilateral periodic distribution, a structure diameter of 150 μm, a structure spacing of 100 μm, and an array period of 4. Use a DC power supply 206 to apply a voltage of 9000 V between the upper electrode 203 and the lower electrode 201. The needle-tip electrode is the positive electrode. The first polymer 204 is deformed by the ion wind generated by the electric field, resulting in a concave first polymer micro-droplet array 205 with an array period of 4, a droplet diameter of 150 μm, and a droplet spacing of 100 μm.
[0086] 3. The lower electrode 201 having the first polymer micro-droplet array 205 on the temperature control platform 202 is placed in a glycerol vapor atmosphere controlled by a horizontal humidified airflow 207 in a humidity control system. The temperature of the first polymer micro-droplet array 205 is regulated by the cooling effect of the temperature control platform 202, so that the temperature of the first polymer micro-droplet array 205 is lower than the ambient temperature, thereby causing the glycerol vapor to condense and form nuclei on the surface of the first polymer micro-droplet array 205. The electric field between the lower electrode 201 and the upper electrode 203 prevents the aggregation of droplets during the condensation nucleation process, thereby achieving nanoscale droplet formation. After a condensation time of 15 minutes, the glycerol vapor self-assembles on the surface of the first polymer micro-droplet array 205 into a uniformly distributed second nano-droplet array 208 with a diameter of 5 μm. Due to surface tension, the second nano-droplet array 208 partially enters the interior of the first polymer micro-droplet array 205. The ambient temperature Ta is controlled to be 20° C., the glycerol vapor atmosphere concentration is controlled to be 70%, and the control temperature Tc of the temperature control platform 202 is controlled to be −10° C.
[0087] 4. Prepare a substrate 209, which is a PC board. Spin-coat the second polymer 210 on the surface of the substrate 209 to obtain a second polymer 210 with a thickness of 500 μm on the substrate 209.
[0088] 5. Covering the second polymer 210 on the substrate 209 on the first polymer microdroplet array 205 having the second nanodroplet array 208, wherein the second polymer 210 faces downward. Under the action of surface tension, the second nanodroplet array 208 on the surface of the first polymer microdroplet array 205 is pressed into the interior of the second polymer 210, forming a stable first polymer-second nanodroplet-second polymer three-phase interface;
[0089] 6. The second polymer 210 is completely cured by irradiation with an ultraviolet lamp 212, thereby obtaining a curved second nanostructure array corresponding to the second nanodroplet array 208 on the surface of the first polymer microdroplet array 205, wherein the ultraviolet irradiation energy is 4W / cm 2 , curing time is 15min;
[0090] 7. Peel the substrate 209 from the surface of the lower electrode 201, and clean the surface of the second polymer 210 on the surface of the substrate 209 with acetone and deionized water respectively to remove the second nanodroplet array 208 and the first polymer microdroplet array 205, finally obtaining a micro-nano composite structure array 211.
[0091] Example 3:
[0092] like Figure 21-28 As shown, a method for preparing a micro-nano composite structure by a droplet forming method based on electric field action includes the following steps:
[0093] 1. Prepare a lower electrode 301 and ground it. The lower electrode 301 is glass with a patterned electrode 313 on its surface. The patterned electrode 313 has a regular hexagonal periodically distributed circular structure array with a structure diameter of 100 μm, a structure spacing of 100 μm, and a period number of 3. Ground the patterned electrode 313. Place the lower electrode 301 on a temperature-controlled platform 302 and apply a first polymer 304 to the surface of the lower electrode 301 using a spot coating method to obtain a first polymer 304 with a thickness of 250 μm. The first polymer is a thermosetting polymer.
[0094] 2. Prepare an upper electrode 303, which is a needle-tip electrode. Place the upper electrode 303 5 mm above the lower electrode 301. Use a DC power supply 306 to apply a voltage of 1000 V between the upper electrode 303 and the lower electrode 301. The needle-tip electrode is the positive electrode. This causes the first polymer 304 to deform under the action of the ionic wind generated by the electric field, resulting in a concave first polymer microdroplet array 305 with an array period of 3, a droplet diameter of 100 μm, and a droplet spacing of 70 μm.
[0095] 3. The lower electrode 301 with the first polymer micro-droplet array 305 on the temperature control platform 302 is placed in an ethylene glycol vapor atmosphere controlled by a vertical humidified air flow 307 in the humidity control system. The temperature of the first polymer micro-droplet array 505 is regulated by the refrigeration effect of the temperature control platform 302, so that the temperature of the first polymer micro-droplet array 305 is lower than the ambient temperature, thereby causing the ethylene glycol vapor to condense and form nuclei on the surface of the first polymer micro-droplet array 305; the electric field between the lower electrode 301 and the upper electrode 303 is used to avoid During the condensation nucleation process, droplets converge to form nanoscale droplets. After 30 minutes of condensation, ethylene glycol vapor self-assembles on the surface of the first polymer micro-droplet array 305 into a uniformly distributed second nano-droplet array 308 with a diameter of 10 μm. Due to surface tension, the second nano-droplet array 308 partially enters the interior of the first polymer micro-droplet array 305. The ambient temperature Ta is controlled at 20°C, the ethylene glycol vapor concentration is controlled at 10%, and the control temperature Tc of the temperature control platform 302 is -20°C.
[0096] 4. Prepare a substrate 309, which is a glass plate. Spin-coat the second polymer 310 on the surface of the substrate 309 to obtain a second polymer 310 with a thickness of 100 μm on the substrate 309;
[0097] 5. Covering the second polymer 310 on the substrate 309 on the first polymer microdroplet array 305 having the second nanodroplet array 308, wherein the second polymer 310 faces downward. Under the action of surface tension, the second nanodroplet array 308 on the surface of the first polymer microdroplet array 305 is pressed into the interior of the second polymer 310, forming a stable first polymer-second nanodroplet-second polymer three-phase interface;
[0098] 6. The second polymer 310 is completely cured by irradiation with an ultraviolet lamp 312, thereby obtaining a curved second nanostructure array corresponding to the second nanodroplet array 308 on the surface of the first polymer microdroplet array 305, wherein the ultraviolet irradiation energy is 5W / cm 2 , curing time is 10min;
[0099] 7. The substrate 309 is peeled off from the surface of the lower electrode 301, and the surface of the second polymer 310 on the surface of the substrate 309 is cleaned with acetone and deionized water respectively to remove the second nanodroplet array 308 and the first polymer microdroplet array 305, thereby finally obtaining a micro-nano composite structure array 311.
[0100] Example 4:
[0101] like Figures 29-31As shown, a method for preparing a micro-nano composite structure by droplet forming based on electric field action, steps 1, 2, 4, and 5 are the same as those in Example 1, and the steps different from Example 1 are:
[0102] 3. The lower electrode 401 having the first polymer micro-droplet array 405 on the temperature control platform 402 is placed in an atmosphere of ethylene glycol and glycerol mixed vapor controlled by a horizontal humidified airflow 407 in a humidity control system. The temperature of the first polymer micro-droplet array 405 is regulated by the refrigeration function of the temperature control platform 402, so that the temperature of the first polymer micro-droplet array 405 is lower than the ambient temperature, thereby causing the ethylene glycol and glycerol mixed vapor to condense and form nuclei on the surface of the first polymer micro-droplet array 405. The electric field between the lower electrode 401 and the upper electrode 403 prevents the droplets from converging during the condensation nucleation process. Nanoscale droplet formation is achieved; after a 3-minute condensation time, the ethylene glycol and glycerol mixed vapor self-assembles on the surface of the first polymer micro-droplet array 405 into a uniformly distributed second nano-droplet array 408 with a diameter of 0.5 μm. Due to the effect of surface tension, the second nano-droplet array 408 partially enters the interior of the first polymer micro-droplet array 405; wherein, the ambient temperature Ta is controlled at 20°C, the volume ratio of ethylene glycol vapor to glycerol vapor in the mixed vapor is 1:1, the atmosphere concentration of the ethylene glycol and glycerol mixed vapor is controlled at 90%, and the control temperature Tc of the temperature control platform 402 is -5°C;
[0103] 6. Completely solidify the first polymer micro-droplet array 405 by using the temperature control platform 402, thereby obtaining a curved second nanostructure array corresponding to the second nano-droplet array 408 on the surface of the first polymer micro-droplet array 405. The ambient temperature Ta is controlled at 20°C, the control temperature Tc of the temperature control platform 402 is 70°C, and the curing time is 300 minutes.
[0104] 7. The substrate 409 is peeled off from the surface of the lower electrode 401. The surface of the first polymer micro-droplet array 405 on the surface of the lower electrode 401 is cleaned with acetone and deionized water respectively, and the second nano-droplet array 408 and the second polymer 410 are removed to finally obtain a micro-nano composite structure array 411.
[0105] Example 5:
[0106] like Figures 32-33 As shown, a method for preparing a micro-nano composite structure by droplet forming based on electric field action, steps 1-5 are the same as those in Example 2, and the steps different from Example 2 are:
[0107] 6. Completely solidify the first polymer micro-droplet array 505 by using the temperature control platform 502, thereby obtaining a curved second nanostructure array corresponding to the second nano-droplet array 508 on the surface of the first polymer micro-droplet array 505. The ambient temperature Ta is controlled at 20°C, the control temperature Tc of the temperature control platform 502 is 110°C, and the curing time is 200 minutes.
[0108] 7. The substrate 509 is peeled off from the surface of the lower electrode 501. The surface of the first polymer micro-droplet array 505 on the surface of the lower electrode 501 is cleaned with acetone and deionized water respectively, and the second nano-droplet array 508 and the second polymer 510 are removed to finally obtain a micro-nano composite structure array 511.
[0109] Example 6:
[0110] like Figures 34-35 As shown, a method for preparing a micro-nano composite structure by droplet forming based on electric field action, steps 1-5 are the same as those in Example 3, and the steps different from Example 3 are:
[0111] 6. Completely solidify the first polymer micro-droplet array 605 by using the temperature control platform 602, thereby obtaining a curved second nanostructure array corresponding to the second nano-droplet array 608 on the surface of the first polymer micro-droplet array 605. The ambient temperature Ta is controlled at 20°C, the control temperature Tc of the temperature control platform 602 is controlled at 90°C, and the curing time is 300 minutes.
[0112] 7. The substrate 609 is peeled off from the surface of the lower electrode 601. The surface of the first polymer micro-droplet array 605 on the surface of the lower electrode 601 is cleaned with acetone and deionized water respectively, and the second nano-droplet array 608 and the second polymer 610 are removed to finally obtain a micro-nano composite structure array 611.
[0113] Example 7:
[0114] like Figure 36 As shown, a method for preparing a micro-nano composite structure by droplet forming based on electric field action, steps 1, 3-7 are the same as those in Example 5, and the steps different from Example 5 are:
[0115] 2. Prepare the upper electrode 703, which is a needle-tip electrode array. Place the upper electrode 703 100 mm above the lower electrode 701. Set the patterned through-hole template 713 between the upper and lower electrodes. The patterned through-hole template 713 has a circular structure array with a regular quadrilateral periodic distribution, a structure diameter of 150 μm, a structure spacing of 100 μm, and an array period number of 4. Use a DC power supply 706 to apply a voltage of 14,000 V between the upper electrode 703 and the lower electrode 701. The needle-tip electrode is the negative pole and is grounded, so that the first polymer 704 is deformed under the action of the ion wind generated by the electric field, obtaining a concave first polymer micro-droplet array 705 with an array period number of 4, a droplet diameter of 150 μm, and a droplet spacing of 100 μm.
[0116] The above embodiments are intended only to illustrate the design concepts and features of the present invention. Their purpose is to enable those skilled in the art to understand the contents of the present invention and implement them accordingly. The scope of protection of the present invention is not limited to the above embodiments. Therefore, any equivalent changes or modifications made based on the principles and design concepts disclosed in the present invention are within the scope of protection of the present invention.
Claims
1. A method for preparing a micro-nano composite structure by droplet forming based on electric field action, characterized in that: The following steps are involved: A. prepare a lower electrode, place the lower electrode on a temperature-controlled platform, and cover the surface of the lower electrode with a first polymer, wherein the first polymer is in a liquid state; B. preparing an upper electrode, applying an electric field between the upper electrode and the lower electrode, and patterning the first polymer layer through the generated ion wind to obtain a first polymer micro-droplet array; The upper electrode is a needle tip electrode or a needle tip electrode array, the distance between the upper electrode and the lower electrode is adjustable within 5mm-200mm, a voltage is applied using a DC power supply, and the voltage adjustment range is continuously adjustable within 1000V-15000V; or, a graphic through-hole template is provided between the upper electrode and the lower electrode; C. Prepare a steam atmosphere control system, achieve temperature regulation of the first polymer micro-droplet array through the refrigeration effect of the temperature control platform, so that the temperature of the first polymer micro-droplet array is lower than the ambient temperature, introduce an electric field effect through the configuration of the upper electrode and the lower electrode to achieve corona discharge, place the lower electrode with the first polymer micro-droplet array on the temperature control platform in a water vapor atmosphere controlled by humidified airflow in the humidity control system, and after the steam condenses after a set time, self-assemble into a second nano-droplet array on the surface of the first polymer micro-droplet array, wherein the second nano-droplet is incompatible with the first polymer; The vapor atmosphere control system can realize the vapor atmosphere and control the concentration range of the vapor atmosphere to be 10% to 90%, and the vapor atmosphere is one or more of water, methanol, ethanol, ethylene glycol or glycerol; the control range of the control temperature Tc of the temperature control platform is -20 to 300°C, the condensation time of the second nanodroplet is 1 to 30 min, and the diameter of the obtained second nanodroplet is 0.1 to 10 μm; D. preparing a substrate, and covering the surface of the substrate with a second polymer, wherein the second polymer is immiscible with the first polymer and the second nanodroplet; E. Covering the second polymer on the substrate on the first polymer microdroplet array having the second nanodroplet array to form a stable first polymer-second nanodroplet-second polymer three-phase interface; F. Curing the first polymer until it is completely cured to obtain a first microstructure array, and due to the imprinting effect of the second nanodroplet array, a curved second nanostructure array corresponding to the second nanodroplet array is obtained on the surface of the first polymer microdroplet array; G. Peeling off the substrate, removing the second nanodroplet array and the second polymer on the surface of the first polymer microstructure array, and obtaining a micro-nano composite structure array.
2. The method for preparing a micro-nano composite structure by droplet forming based on electric field action according to claim 1, characterized in that: The lower electrode material described in step A is one of ITO conductive glass, conductive graphite, aluminum, copper, or glass, ceramic, silica gel, and polystyrene with a patterned electrode on the surface.
3. The method for preparing a micro-nano composite structure by droplet forming based on electric field action according to claim 1, characterized in that: The material of the substrate in step D is one of glass, silica gel, polystyrene, polycarbonate or polymethyl methacrylate high light transmittance materials.
4. The method for preparing a micro-nano composite structure by droplet forming based on electric field action according to claim 1, characterized in that: The first polymer described in step A is covered on the surface of the lower electrode by dot coating, spray coating or spin coating, the thickness of the first polymer is 5~1000μm, and the first polymer is a liquid dielectric polymer at room temperature and pressure; the second polymer described in step D is covered on the surface of the substrate by dot coating, spray coating or spin coating, the thickness of the second polymer is 5~1000μm, and the second polymer is a liquid polymer at room temperature and pressure.
5. The method for preparing a micro-nano composite structure by droplet forming based on electric field action according to claim 1, characterized in that: The first polymer is a UV-curable polymer, the second polymer is a non-UV-curable polymer, and the corresponding curing method in step F is to completely cure the first polymer by UV light irradiation, and the curing time is 1 to 30 minutes; or, the first polymer is a heat-curable polymer, the second polymer is a non-heat-curable polymer, and the corresponding curing method in step F is to completely cure the first polymer by heating curing, and the curing time is 10 to 300 minutes.
6. A method for preparing a micro-nano composite structure by droplet forming based on electric field action, characterized in that: The following steps are involved: A. prepare a lower electrode, place the lower electrode on a temperature-controlled platform, and cover the surface of the lower electrode with a first polymer, wherein the first polymer is in a liquid state; B. preparing an upper electrode, applying an electric field between the upper electrode and the lower electrode, and patterning the first polymer layer through the generated ion wind to obtain a first polymer micro-droplet array; The upper electrode is a needle tip electrode or a needle tip electrode array, the distance between the upper electrode and the lower electrode is adjustable within 5mm-200mm, a DC power supply is used to apply voltage, and the voltage adjustment range is continuously adjustable within 1000V-15000V; or, a graphic through-hole template is provided between the upper electrode and the lower electrode; C. Prepare a steam atmosphere control system, achieve temperature regulation of the first polymer micro-droplet array through the refrigeration effect of the temperature control platform, so that the temperature of the first polymer micro-droplet array is lower than the ambient temperature, introduce an electric field effect through the configuration of the upper electrode and the lower electrode to achieve corona discharge, place the lower electrode with the first polymer micro-droplet array on the temperature control platform in a water vapor atmosphere controlled by humidified airflow in the humidity control system, and after the steam condenses after a set time, self-assemble into a second nano-droplet array on the surface of the first polymer micro-droplet array, wherein the second nano-droplet is incompatible with the first polymer; The vapor atmosphere control system can realize the vapor atmosphere and control the concentration range of the vapor atmosphere to be 10% to 90%, and the vapor atmosphere is one or more of water, methanol, ethanol, ethylene glycol or glycerol; the control range of the control temperature Tc of the temperature control platform is -20 to 300°C, the condensation time of the second nanodroplet is 1 to 30 min, and the diameter of the obtained second nanodroplet is 0.1 to 10 μm; D. preparing a substrate, and covering the surface of the substrate with a second polymer, wherein the second polymer is immiscible with the first polymer and the second nanodroplet; E. Covering the second polymer on the substrate on the first polymer microdroplet array having the second nanodroplet array to form a stable first polymer-second nanodroplet-second polymer three-phase interface; F. Curing the second polymer until it is completely cured to obtain a first microstructure array. Due to the imprinting effect of the second nanodroplet array, a curved second nanostructure array corresponding to the second nanodroplet array is obtained on the surface of the first polymer microstructure array; G. Peeling off the substrate, removing the second nanodroplet array and the first polymer on the surface of the second polymer microstructure array, and obtaining a micro-nano composite structure array.
7. The method for preparing a micro-nano composite structure by droplet forming based on electric field action according to claim 6, characterized in that: The lower electrode material described in step A is one of ITO conductive glass, conductive graphite, aluminum, copper, or glass, ceramic, silica gel, and polystyrene with a patterned electrode on the surface.
8. The method for preparing a micro-nano composite structure by droplet forming based on electric field action according to claim 6, characterized in that: The material of the substrate in step D is one of glass, silica gel, polystyrene, polycarbonate or polymethyl methacrylate high light transmittance materials.
9. The method for preparing a micro-nano composite structure by droplet forming based on electric field action according to claim 6, characterized in that: The first polymer described in step A is covered on the surface of the lower electrode by dot coating, spray coating or spin coating, and the thickness of the first polymer is 5~1000μm, and the first polymer is a liquid dielectric polymer at room temperature and pressure; the second polymer described in step D is covered on the surface of the substrate by dot coating, spray coating or spin coating, and the thickness of the second polymer is 5~1000μm, and the second polymer is a liquid polymer at room temperature and pressure.
10. The method for preparing a micro-nano composite structure by droplet forming based on electric field action according to claim 6, characterized in that: The second polymer is a UV-curable polymer, the first polymer is a non-UV-curable polymer, and the corresponding curing method in step F is to completely cure the second polymer by UV light irradiation, and the curing time is 1 to 30 minutes; or, the second polymer is a heat-curable polymer, the first polymer is a non-heat-curable polymer, and the corresponding curing method in step F is to completely cure the second polymer by heating curing, and the curing time is 10 to 300 minutes.