A TOPCon battery electrode structure and its preparation method and application

By adopting a composite structure of nickel seed layer and aluminum electrode layer in TOPCon batteries, the problems of high silver paste cost and poor aluminum paste effect are solved, efficient ohmic contact and battery stability are achieved, process is simplified and resources are reduced Consumption.

CN115064600BActive Publication Date: 2024-11-15NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202210499880.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-06
Publication Date
2024-11-15
Estimated Expiration
2042-05-06

AI Technical Summary

Technical Problem

The use of silver paste on the back electrode of the existing TOPCon battery leads to high cost and limited silver resources. The aluminum paste is not effective in the n-type TOPCon battery, resulting in the destruction of passivation and poor ohmic contact.

Method used

Using a composite metal structure between the nickel seed layer and the aluminum electrode layer, the nickel seed layer forms a good ohmic contact with the doped polysilicon, and the nickel seed layer is deposited on the polysilicon through electroless plating technology to prevent the penetration of aluminum slurry and protect the passivation performance. .

Benefits of technology

It reduces battery costs, improves battery efficiency and stability, simplifies process complexity, realizes the feasibility of silver paste replacement, and maintains the chemical stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115064600B_ABST
    Figure CN115064600B_ABST
Patent Text Reader

Abstract

The present invention provides an electrode structure of a TOPCon battery, comprising a back electrode and a front electrode, wherein the back electrode is disposed on a first passivation layer on the back of a crystalline silicon substrate, and the front electrode is disposed on a second passivation layer on the front of the crystalline silicon substrate, and any one of the back electrode and the front electrode comprises a nickel seed layer and an aluminum electrode layer, wherein the nickel seed layer is superimposed on the first passivation layer or the second passivation layer, and the aluminum electrode layer is superimposed on the nickel seed layer. The present invention provides an electrode structure of a TOPCon battery, wherein a composite metal structure of a nickel seed layer and an aluminum electrode layer is used to replace the silver electrode in the prior art, and the nickel seed layer can form a good ohmic contact with doped polysilicon.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cells, and in particular to an electrode structure of a TOPCon cell, a preparation method thereof and an application thereof. Background Art

[0002] Tunneling oxide passivation contact technology (TOPCon) is a crystalline silicon solar cell proposed by the Fraunhofer Institute in Germany in 2013. The TOPCon structure has excellent surface passivation performance and can effectively improve the efficiency of the cell. In the production of crystalline silicon solar cells, an important process is the production of the back electrode. The electrode plays the role of collecting and conducting current in the solar cell. However, the back of the TOPCon cell currently uses phosphorus-doped n-type doped polysilicon, which requires silver paste to form a good contact.

[0003] Most of the existing n-type TOPCon cells use silver paste on the back. Due to the high unit price of silver, the cost of n-type TOPCon cells using silver paste on the back is significantly increased, resulting in its cost per kilowatt-hour still being higher than the current mainstream PERC cells in the industry, affecting mass production and promotion. In addition, as a precious metal, the abundance of silver in the earth's crust is significantly lower than that of aluminum, and the annual global silver production is very limited. When silicon-based solar cells develop to an annual output of more than terawatts, the global silver production will be difficult to meet the needs of the photovoltaic industry, which will cause the silver price to rise further.

[0004] Therefore, there is a technical solution in the prior art to directly use aluminum paste to replace silver paste. However, the application effect of aluminum paste on n-type TOPCon is not good for the following two reasons:

[0005] 1) During sintering, silicon atoms will quickly dissolve into Al, causing the polysilicon to be penetrated and the passivation effect to be completely destroyed.

[0006] 2) Al may penetrate to a depth of several microns or more than ten microns below the surface of the silicon wafer, and it is difficult for Al to form a good ohmic contact with the n-type silicon wafer. Summary of the invention

[0007] The present invention aims to solve one of the technical problems in the related art to at least some extent. To this end, an electrode structure of a TOPCon battery is provided, which uses a composite metal structure of a nickel seed layer and an aluminum electrode layer to replace the silver electrode in the prior art, and the nickel seed layer can form a good ohmic contact with doped polysilicon.

[0008] To solve the above problems, the present invention provides an electrode structure of a TOPCon battery, including a back electrode and a front electrode, the back electrode is placed on a first passivation layer on the back side of a crystalline silicon substrate, and the front electrode is placed on a second passivation layer on the front side of the crystalline silicon substrate, and either the back electrode or the front electrode includes a nickel seed layer and an aluminum electrode layer, the nickel seed layer is superimposed on the first passivation layer or the second passivation layer, and the aluminum electrode layer is superimposed on the nickel seed layer.

[0009] Compared with the prior art, the nickel seed layer in the above-mentioned battery structure is very dense and can effectively block the penetration of aluminum paste, thereby protecting the good passivation performance of the TOPCon structure.

[0010] Optionally, a tunneling oxide layer and a doped polysilicon layer are provided between the crystalline silicon substrate and the first passivation layer. When the doped polysilicon layer is n-type phosphorus-doped polysilicon, the main component of the nickel seed layer on the first passivation layer is NiP. x When the doped polysilicon layer is p-type boron-doped polysilicon, the main component of the nickel seed layer on the first passivation layer is NiB x .

[0011] Optionally, the first passivation layer is composed of a composite of an aluminum oxide layer and a silicon nitride layer, and a side of the aluminum oxide layer away from the silicon nitride layer is composited with the doped polysilicon layer.

[0012] Optionally, when the doped polysilicon layer is n-type phosphorus-doped polysilicon, the main component of the nickel seed layer on the second passivation layer is NiP. x When the doped polysilicon layer is p-type boron-doped polysilicon, the main component of the nickel seed layer on the second passivation layer is NiB x .

[0013] Optionally, the nickel seed layer has a thickness of 100-5000 nm.

[0014] Optionally, the nickel seed layer contains one or more trace elements of chromium, copper, tin, silver and sulfur.

[0015] Optionally, the sum of the masses of the trace elements accounts for 0.01-1% of the total mass of the nickel seed layer.

[0016] A second object of the present invention is to provide a method for preparing an electrode structure of a TOPCon battery.

[0017] A method for preparing an electrode structure of a TOPCon battery as described above comprises the following steps:

[0018] S1, preparing a tunneling oxide layer, a doped polysilicon layer and a first passivation layer on the back side of the crystalline silicon substrate, and preparing a doped emitter and a second passivation layer on the front side of the crystalline silicon substrate;

[0019] S2, performing a groove process on the first passivation layer or the second passivation layer;

[0020] S3, forming a nickel seed layer in the groove opened in S2 by chemical nickel plating and annealing;

[0021] S4. Forming an aluminum electrode layer on the nickel seed layer by screen printing and sintering.

[0022] Compared with the prior art, the preparation method of the above battery structure has the following advantages:

[0023] (1) A nickel seed layer is plated on the doped polysilicon layer by chemical plating technology. A nickel seed layer is plated on the doped polysilicon layer by chemical plating technology. By adjusting the composition of the seed layer and annealing, a good ohmic contact can be formed with the doped polysilicon.

[0024] (2) The chemical nickel plating seed layer is very dense and can effectively block the penetration of aluminum paste, thereby protecting the good passivation performance of the TOPCon structure.

[0025] (3) Chemical nickel plating has the property of self-alignment and only deposits on polysilicon, which helps to simplify the process complexity. In addition, the cost of chemical nickel plating seed layer material is low and easy to achieve mass production.

[0026] (4) The electrode structure still maintains screen-printed aluminum paste, which has higher production capacity and lower cost than electroplating. The electrode uses nickel and aluminum metals, which have good chemical stability and can effectively maintain the stability of the battery.

[0027] Optionally, the annealing temperature in step S3 is 150-600°C and the annealing time is 5-15 minutes.

[0028] Optionally, the sintering temperature in step S4 is 400-600°C and the sintering time is 1-2 minutes.

[0029] A third object of the present invention is to provide a crystalline silicon cell using the electrode structure of a TOPCon cell.

[0030] A crystalline silicon cell employs the electrode structure of any of the above-mentioned TOPCon cells.

[0031] Optionally, the crystalline silicon cell comprises, from bottom to top, a back electrode, a first passivation layer, a doped polysilicon layer, a tunneling oxide layer, a crystalline silicon substrate, a doped emitter, a second passivation layer and a front electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a schematic diagram of the structure of the TOPCon battery in Example 1 of the present invention;

[0033] Figure 2 Schematic diagram of the structure of the TOPCon battery in Example 2 of the present invention. DETAILED DESCRIPTION

[0034] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] In this embodiment, the tunneling oxide layer 2 on the back of the crystalline silicon substrate 1 is also called an ultra-thin silicon oxide layer, which is essentially an ultra-thin dielectric layer, which can be a SiOx layer or a silicon oxynitride layer; its thickness is less than 5nm, and in a specific embodiment, the thickness of the tunneling oxide layer 2 is 1.2-2.2nm. The tunneling oxide layer 2 can allow the majority carriers to tunnel to the heavily doped polysilicon layer 3, effectively preventing the minority carriers from recombination, and at the same time, the heavily doped polysilicon layer 3 can prevent the metal from directly contacting the substrate, reducing the deep level defect recombination introduced by the metal.

[0036] Furthermore, in this embodiment, the preparation method of the tunneling oxide layer 2 includes: thermal nitric acid oxidation method, rapid thermal oxidation method (RTO), ultraviolet ozone method (UV / O3), ozone deionized water method (DIO3), thermal oxidation method, PECVD-N2O method, mixed acid oxidation method and the like, aiming to prepare an ultra-thin, high-quality silicon oxide layer with low interface defect state density.

[0037] In this embodiment, the first passivation layer 4 is a SiNx layer or a composite layer of a SiNx layer and an AlOx layer or a composite layer of a SiNx layer and a SiOx layer.

[0038] Furthermore, in a specific embodiment, the first passivation layer 4 is AlO x With SiN x Composite composition, AlO x Stay away from SiN x One side is combined with the doped polysilicon layer 3. SiN x As a protective layer, it can reduce the high temperature damage caused by sintering. At the same time, the hydrogenated SiN x During the sintering process, the hydrogen it carries can also passivate the polysilicon.

[0039] Combination Figure 1As shown, the electrode structure of the TOPCon battery in this embodiment includes a back electrode 5 and a front electrode 8, the back electrode 5 is placed on the first passivation layer 4 on the back of the crystalline silicon substrate 1, and the front electrode 8 is placed on the second passivation layer 7 on the front of the crystalline silicon substrate 1. Any of the back electrode 5 and the front electrode 8 includes a nickel seed layer 51, 81 and an aluminum electrode layer 52, 82, that is, the back electrode 5 includes a nickel seed layer 51 and an aluminum electrode layer 52, and the front electrode 8 is a conventional electrode, or the front electrode 8 includes a nickel seed layer 81 and an aluminum electrode layer 82, and the back electrode 5 is a conventional electrode. The nickel seed layers 51, 81 are superimposed on the first passivation layer 4 or the second passivation layer 7, and the aluminum electrode layers 52, 82 are superimposed on the nickel seed layers 51, 81.

[0040] Specifically, a tunneling oxide layer 2 and a doped polysilicon layer 3 are provided between the crystalline silicon substrate 1 and the first passivation layer 4. When the doped polysilicon layer 3 is n-type phosphorus-doped polysilicon, the main component of the nickel seed layer 51 on the first passivation layer 4 is NiP. x When the doped polysilicon layer 3 is p-type boron-doped polysilicon, the main component of the nickel seed layer 51 on the first passivation layer 4 is NiB x .

[0041] Specifically, the first passivation layer 4 is composed of a composite of an aluminum oxide layer and a silicon nitride layer, and a side of the aluminum oxide layer away from the silicon nitride layer is composited with the doped polysilicon layer 3 .

[0042] Specifically, the thickness of the nickel seed layers 51 and 81 is 100-5000 nm.

[0043] Specifically, the nickel seed layer 51 , 81 contains one or more trace elements of chromium, copper, tin, silver and sulfur, and the sum of the masses of the trace elements accounts for 0.01-1% of the total mass of the nickel seed layer 51 , 81 .

[0044] The trace element added in this embodiment is specifically sulfur. During the cathode reaction of chemical plating, trace sulfite ions contained in the plating solution have the opportunity to be reduced to sulfur atoms and doped into the nickel plating layer, wherein chemical plating includes electro-assisted chemical plating, light-assisted chemical plating, and sensitized chemical plating.

[0045] The method for preparing the electrode structure of the TOPCon battery in this embodiment comprises the following steps:

[0046] S1, preparing a tunneling oxide layer 2, a doped polysilicon layer 3 and a first passivation layer 4 on the back side of a crystalline silicon substrate 1, and preparing a doped emitter 6 and a second passivation layer 7 on the front side of the crystalline silicon substrate 1;

[0047] S2, performing a groove process on the first passivation layer 4 or the second passivation layer 7;

[0048] S3, forming nickel seed layers 51, 81 in the grooves opened in S2 by chemical nickel plating and annealing;

[0049] S4. Forming aluminum electrode layers 52 and 82 on the nickel seed layers 51 and 81 by screen printing and sintering.

[0050] In step S2, when the first passivation layer 4 is grooved, an electrode grid profile is formed on the surface of the first passivation layer 4, and the doped polysilicon layer 3 is exposed at the bottom of the groove. When the second passivation layer 7 is grooved, an electrode grid profile is formed on the surface of the second passivation layer 7, and the doped emitter 6 layer is exposed at the bottom of the groove.

[0051] Specifically, the specific process of the preparation method of the electrode structure of the TOPCon battery is as follows:

[0052] 1) Al2O3 / SiN on the back x The stacked layers are opened to expose the doped polysilicon layer 3 at the bottom. The opening method can usually be laser opening, or patterning can be formed by photolithography, spraying, printing, etc., and then the opening is formed by etching.

[0053] 2) Under the induction of light field, electric field, or sensitizer, a nickel seed layer 51 is directly deposited on the doped polysilicon by chemical plating. The main component of the nickel layer is NiP x , and also includes other necessary trace elements to adjust the film properties. If it is n-type phosphorus-doped polysilicon, NiP is usually used. x Generally speaking, the thickness of the nickel layer is between 100nm and 5000nm. It should be noted that the nickel layer is only deposited on the polysilicon layer, and not on the SiN x No deposition will occur on the layer surface, which has a self-alignment effect.

[0054] 3) According to different requirements, annealing treatment is performed at 150-600°C for different times, and nitrogen-hydrogen mixed gas is usually used as a protective atmosphere, so that the nickel seed layer 51 forms a good ohmic contact with the doped polysilicon. Alternatively, according to process requirements, the nickel seed layer 51 is directly deposited without annealing, and then sintered together with the aluminum electrode layer 52 to form a good ohmic contact.

[0055] 4) Subsequently, aluminum paste is printed on the nickel layer on the back by screen printing, and then sintered in a chain furnace to form a good ohmic contact between the aluminum paste and the nickel layer.

[0056] Example 1

[0057] The n-type crystalline silicon substrate 1 is cleaned, and a tunneling oxide layer 2 is prepared on the back side by thermal oxidation. Then, 100nm of heavily doped phosphorus amorphous silicon is prepared on the back side of the silicon oxide by PECVD, and annealed at 880-920℃ for different times to form a doped polysilicon layer 3 and a TOPCon structure. On the surface of the n-type heavily doped polysilicon, a 2000nm thick nickel-phosphorus alloy is prepared by chemical plating, and then annealed under nitrogen-hydrogen mixed gas protection at 150-450℃ to test the contact resistivity. After testing, the contact resistivity distribution is 0.1-5mΩcm2, which meets the application requirements of battery contact resistivity.

[0058] Example 2

[0059] N-type silicon wafers are passivated on both sides with TOPCon, and the thickness of polysilicon is 100-300nm. The implicit open circuit voltage iVoc of the original passivated wafer is 730mV, and the corresponding single-sided saturation current density is 6fA / cm2. On one surface of n-type heavily doped polysilicon, a 500-3000nm thick nickel-phosphorus alloy is prepared by chemical plating, and then annealed under nitrogen-hydrogen mixed gas protection at 150-250℃, followed by screen printing of aluminum paste on it, and sintering at 700-800℃.

[0060] According to tests, the saturation current density of the metal contact area after sintering is 30-200fA / cm2, which meets the requirements of battery applications.

[0061] Example 3

[0062] First, the n-type crystalline silicon substrate 1 is cleaned, and then the double-sided texture of the n-type crystalline silicon substrate 1 is formed, and the boron is diffused on the single side of the front surface of the n-type crystalline silicon substrate 1 to form a doped emitter 6, that is, a boron emitter. The non-boron diffused surface is subjected to acid etching to remove the boron coating layer and the texture surface, and a tunneling oxide layer 2 is prepared on the back by thermal oxidation. Then, 100nm of heavily doped phosphorus amorphous silicon is prepared on the back silicon oxide by PECVD; annealing is performed at a high temperature of 880-920℃ for different times to form a doped polysilicon layer 3, a pn junction and a TOPCon structure, and aluminum oxide and silicon nitride are used to cover and deposit the front and rear surfaces, and a first passivation layer 4 is formed on the surface of the doped polysilicon layer 3, and a second passivation layer 7 is formed on the surface of the doped emitter 6. Then, the first passivation layer 4 is laser-opened, and an electrode grid outline is formed on the surface of the first passivation layer 4, and the doped polysilicon layer 3 is exposed at the bottom of the groove. A 2000nm undoped nickel-phosphorus alloy layer is prepared in the tank by chemical plating, and annealed at 150-450°C to form a nickel seed layer 51. Then, an aluminum electrode layer 52 is printed on the nickel alloy by screen printing, followed by belt furnace sintering. At the same time, a silver electrode is prepared on the surface of the second passivation layer 7 by screen printing, and finally a finished battery is obtained.

[0063] After testing, it was verified that the average efficiency of the battery was greater than 23.3%.

[0064] Example 4

[0065] First, the n-type crystalline silicon substrate 1 is cleaned, and then the double-sided texture of the n-type crystalline silicon substrate 1 is formed, and the boron is diffused on the single side of the front surface of the n-type crystalline silicon substrate 1 to form a doped emitter 6, that is, a boron emitter. The non-boron diffused surface is subjected to acid etching to remove the boron coating layer and the texture surface, and a tunneling oxide layer 2 is prepared on the back by thermal oxidation. Then, 100nm of heavily doped phosphorus amorphous silicon is prepared on the back silicon oxide by PECVD; annealing is performed at a high temperature of 880-920℃ for different times to form a doped polysilicon layer 3, a pn junction and a TOPCon structure, and aluminum oxide and silicon nitride are used to cover and deposit the front and rear surfaces, and a first passivation layer 4 is formed on the surface of the doped polysilicon layer 3, and a second passivation layer 7 is formed on the surface of the doped emitter 6. Then, the first passivation layer 4 is laser-opened, and an electrode grid outline is formed on the surface of the first passivation layer 4, and the doped polysilicon layer 3 is exposed at the bottom of the groove. A 2000nm nickel-phosphorus alloy layer doped with 0.01-0.1% sulfur is prepared in a tank by chemical plating, and annealed at 150-450°C to form a nickel seed layer 51. Then, an aluminum electrode layer 52 is printed on the undoped nickel alloy by screen printing, followed by belt furnace sintering. At the same time, a silver electrode is prepared on the surface of the second passivation layer 7 by screen printing, and finally a finished battery is obtained.

[0066] After testing, it was verified that the average efficiency of the battery is greater than 24%.

[0067] Example 5

[0068] First, the n-type crystalline silicon substrate 1 is cleaned, and then the double-sided texture of the n-type crystalline silicon substrate 1 is formed, and the boron is diffused on the single side of the front surface of the n-type crystalline silicon substrate 1 to form a doped emitter 6, that is, a boron emitter. The non-boron diffused surface is subjected to acid etching to remove the boron coating layer and the texture surface, and a tunneling oxide layer 2 is prepared on the back by thermal oxidation. Then, 100nm of heavily doped phosphorus amorphous silicon is prepared on the back silicon oxide by PECVD; annealing is performed at 880-920℃ for different times to form a doped polysilicon layer 3, a pn junction and a TOPCon structure, and aluminum oxide and silicon nitride are used to cover and deposit the front and back surfaces, and a first passivation layer 4 is formed on the surface of the doped polysilicon layer 3, and a second passivation layer 7 is formed on the boron emitter. Then, the second passivation layer 7 is laser-opened to form an electrode grid outline, and the doped emitter 6 layer is exposed at the bottom of the groove. A 2000nm undoped nickel-phosphorus alloy layer is prepared in the groove by chemical plating, and annealing is performed at 150-450℃ to form a nickel seed layer 81. Then, an aluminum electrode layer 82 is printed on the nickel alloy by screen printing, followed by belt furnace sintering. At the same time, a silver electrode is prepared on the back of the first passivation layer 4 by screen printing, and finally a finished battery is obtained.

[0069] After testing, it was verified that the average efficiency of the battery was about 23.5%.

[0070] Example 6

[0071] First, the n-type crystalline silicon substrate 1 is cleaned, and then the double-sided n-type crystalline silicon substrate 1 is textured, and the front surface of the n-type crystalline silicon substrate 1 is single-sidedly expanded with boron to form a doped emitter 6, that is, a boron emitter. The non-boron-expanded surface is acid-etched to remove the boron-plated layer and the textured surface, and a tunneling oxide layer 2 is prepared on the back by thermal oxidation. Then, 100nm of heavily doped phosphorus amorphous silicon is prepared on the back silicon oxide by PECVD; annealing is performed at 880-920℃ for different times to form a doped polysilicon layer 3, a pn junction and a TOPCon structure, and aluminum oxide and silicon nitride are used to cover and deposit the front and rear surfaces, and a first passivation layer 4 is formed on the surface of the doped polysilicon layer 3, and a second passivation layer 7 is formed on the boron emitter. Then, the second passivation layer 7 is laser-opened to form an electrode grid outline, and the doped emitter 6 layer is exposed at the bottom of the groove. A 2000nm nickel-phosphorus alloy layer doped with 0.01-0.1% sulfur is prepared by chemical plating, and annealed at 150-450°C to form a nickel seed layer 81. Then, an aluminum electrode layer 82 is printed on the undoped nickel alloy by screen printing, followed by belt furnace sintering. At the same time, a silver electrode is prepared on the back of the first passivation layer 4 by screen printing, and finally a finished battery is obtained.

[0072] After testing, it was verified that the average efficiency of the battery was about 24.1%.

[0073] Comparative Example 1

[0074] First, the n-type crystalline silicon substrate 1 is cleaned, and then the n-type crystalline silicon substrate 1 is textured on both sides, and the front surface of the n-type crystalline silicon substrate 1 is single-sidedly expanded with boron. The non-boron-expanded surface is acid-etched to remove the boron-plated layer and the texture surface, and a tunneling oxide layer 2 is prepared on the back by thermal oxidation. Then, 100nm of heavily doped phosphorus amorphous silicon is prepared on the back silicon oxide by PECVD; annealing is performed at 880-920℃ for different times to form a doped polysilicon layer 3, a pn junction and a TOPCon structure, and aluminum oxide and silicon nitride are used to cover and deposit the front and back surfaces, and a first passivation layer 4 is formed on the surface of the doped polysilicon layer 3. Then, a hole is opened by laser, and then an aluminum paste electrode layer is printed at the opening position by screen printing, and then a belt furnace sintering process is performed. At the same time, the front side is screen printed to prepare the electrode.

[0075] After testing, it was verified that the average efficiency of the battery was about 18.7%.

[0076] Comparative Example 2

[0077] First, the n-type crystalline silicon substrate 1 is cleaned, and then the double-sided n-type crystalline silicon substrate 1 is textured, and the front surface of the n-type crystalline silicon substrate 1 is single-sidedly boron-diffused, and the non-boron-diffused surface is acid-etched to remove the boron-plated layer and the texture surface, and a tunneling oxide layer 2 is prepared on the back by thermal oxidation, and then 100nm of heavily doped phosphorus amorphous silicon is prepared on the back silicon oxide by PECVD; annealing is performed at 880-920℃ for different times to form a doped polysilicon layer 3, a pn junction and a TOPCon structure, and aluminum oxide and silicon nitride are used to cover and deposit the front and back surfaces, and a first passivation layer 4 is formed on the surface of the doped polysilicon layer 3. Then, a silver paste electrode layer is printed on the first passivation layer by screen printing, and then a belt furnace sintering process is performed. At the same time, the front side is screen printed to prepare electrodes.

[0078] After testing, it was verified that the average efficiency of the battery was about 23.8%.

[0079] Although the disclosure is disclosed as above, the protection scope of the disclosure is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the disclosure, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. An electrode structure of a TOPCon cell, comprising a back electrode (5) and a front electrode (8), wherein the back electrode (5) is disposed on a first passivation layer (4) on the back side of a crystalline silicon substrate (1), and the front electrode (8) is disposed on a second passivation layer (7) on the front side of the crystalline silicon substrate (1), characterized in that: Any one of the back electrode (5) and the front electrode (8) comprises a nickel seed layer (51, 81) and an aluminum electrode layer (52, 82); the nickel seed layer (51, 81) is superimposed on the first passivation layer (4) or the second passivation layer (7); the aluminum electrode layer (52, 82) is superimposed on the nickel seed layer (51, 81); the nickel seed layer (51, 81) contains trace element sulfur, the mass of which accounts for 0.01-1% of the total mass of the nickel seed layer (51, 81); and a tunneling oxide layer (2) and a doped polysilicon layer (3) are provided between the crystalline silicon substrate (1) and the first passivation layer (4).

2. The electrode structure of a TOPCon battery according to claim 1, characterized in that: When the doped polysilicon layer (3) is n-type phosphorus-doped polysilicon, the main component of the nickel seed layer (51) on the first passivation layer (4) is NiP. x When the doped polysilicon layer (3) is p-type boron-doped polysilicon, the main component of the nickel seed layer (51) on the first passivation layer (4) is NiB x .

3. The electrode structure of a TOPCon battery according to claim 2, characterized in that: The first passivation layer (4) is a silicon nitride layer or a composite layer of a silicon nitride layer and an aluminum oxide layer or a composite layer of a silicon nitride layer and a silicon oxide layer.

4. The electrode structure of a TOPCon battery according to claim 1, characterized in that: When the doped polysilicon layer (3) is n-type phosphorus-doped polysilicon, the main component of the nickel seed layer (81) on the second passivation layer (7) is NiP. x When the doped polysilicon layer (3) is p-type boron-doped polysilicon, the main component of the nickel seed layer (81) on the second passivation layer (7) is NiB x .

5. The electrode structure of a TOPCon battery according to claim 1, characterized in that: The thickness of the nickel seed layer (51, 81) is 100-5000 nm.

6. A method for preparing an electrode structure of a TOPCon battery as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: S1, preparing a tunneling oxide layer (2), a doped polysilicon layer (3) and a first passivation layer (4) on the back side of a crystalline silicon substrate (1), and preparing a doped emitter (6) and a second passivation layer (7) on the front side of the crystalline silicon substrate (1); S2, performing a groove process on the first passivation layer (4) or the second passivation layer (7); S3, forming a nickel seed layer (51, 81) in the groove opened in S2 by chemical nickel plating and annealing; S4. Forming an aluminum electrode layer (52, 82) on the nickel seed layer (51, 81) by screen printing and sintering.

7. A crystalline silicon battery, characterized in that: The electrode structure of the TOPCon battery described in any one of claims 1 to 5 is applied.

Citation Information

Patent Citations

  • Back contact type solar cell and manufacturing process thereof

    CN101478009A

  • Silicon solar cell with novel n type back junction design, and preparation method thereof

    CN111509072A

  • Electrode metallization method of passivation contact battery, battery, assembly and system

    CN113611774A

  • Solar cell and preparation method thereof

    CN114005908A

  • Back contact solar cell, and Manufacturing method thereof

    KR1020100096819A