A porous thermal insulation material of wood powder and silicon dioxide composite nanoparticle stacked bed and its preparation method
By combining wood powder with nano-silica particles, cold-pressing them, and then sintering and carbonizing them in a vacuum, a wood powder-silica composite nano-particle stacked bed thermal insulation material is formed, which solves the performance problems of traditional thermal insulation materials during high-temperature molding and achieves High porosity, low thermal conductivity and heat shrink resistance improve thermal insulation performance and cost performance.
Patent Information
- Application Number
- CN202211070311.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-02
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-09-02
AI Technical Summary
Traditional powder-based porous insulation materials face problems such as low molding rate, high-temperature shrinkage, increased density, and reduced porosity during high-temperature molding, which leads to increased thermal conductivity and damage to thermal insulation performance. Adding fiber materials increases costs and has low cost performance.
Wood powder and nano-silica particles are combined, uniformized by ball milling and then cold-pressed and carbonized under vacuum sintering conditions to form a wood powder-silica composite nano-particle accumulation bed porous thermal insulation material, using low-cost wood fiber to enhance mechanics. performance and reduce heat shrinkability.
It achieves high porosity, low thermal conductivity and thermal shrinkage resistance, improves the service life and insulation performance of thermal insulation materials, reduces production costs and environmental pollution, and improves cost performance.
Smart Images

Figure CN115255350B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic non-metallic materials, and specifically relates to a silicon dioxide composite thermal insulation material and a preparation method thereof, and particularly relates to a wood powder silicon dioxide composite nanoparticle stacked bed porous thermal insulation material and a preparation method thereof. Background Art
[0002] Porous super insulation material refers to a super insulation material with high porosity and extremely low thermal conductivity. This material has the advantages of low thermal conductivity, high porosity, low cost, simple process, high temperature resistance, etc. It is an ideal insulation material and has important use value for improving energy utilization, resolving energy crisis, and promoting economic development.
[0003] At present, traditional powder-based porous thermal insulation materials are formed by pressing after mixing individual powders, but most of them face problems such as low forming rate, severe high-temperature shrinkage (the volume shrinkage of 10nm silica particles can be as high as 15% at 750°C), increased density, and reduced porosity. If a large pressure cold pressing is used to improve the forming rate, the large pressure will lead to increased density, resulting in a series of negative optimizations that reduce the material performance, such as a sharp increase in the thermal conductivity of the material, thereby damaging the thermal insulation performance of the material. Therefore, most new porous thermal insulation materials will add some fibrous materials to the powder material to improve the performance of the thermal insulation material, but they will also face problems such as increased material density and decreased porosity due to shrinkage of powder material particles, and the fiber material with better performance improvement is relatively expensive, which greatly reduces the cost-effectiveness of the new thermal insulation material. Summary of the invention
[0004] The purpose of the present invention is to provide a wood powder silica composite nanoparticle stacked bed porous insulation material and a preparation method thereof, the method can simplify the production process, improve the yield, reduce production costs, and reduce pollution to the environment; the prepared insulation material can have the advantages of high porosity, low thermal conductivity, and stronger resistance to heat shrinkage, and can improve the service life and insulation performance of the insulation material in a medium temperature environment.
[0005] In order to achieve the above object, the present invention provides a method for preparing a porous thermal insulation material of a wood powder and silicon dioxide composite nanoparticle stacked bed, comprising the following steps:
[0006] (1) collecting wood powder generated by cutting wood, screening and treating to obtain wood powder with a particle size of 53 to 104 μm, and drying for later use;
[0007] (2) drying the nano-silicon dioxide particles with a particle size of 10 to 60 nm, and then placing them in a ball mill at room temperature with the wood powder obtained in step (1) at a mass ratio of (4 to 19):1, and mixing them evenly to obtain a wood powder and silicon dioxide mixed powder;
[0008] (3) Under room temperature, weigh an appropriate amount of wood flour and silicon dioxide mixed powder and put it into a mold, and use a cold pressing method to press and mold a cake-shaped wood flour and silicon dioxide composite porous material;
[0009] (4) Placing the cake-shaped wood powder-silica composite porous material in a tubular furnace, vacuum sintering and carbonizing it at a temperature of 600 to 750° C. for 180 to 300 minutes to obtain a wood powder-silica composite nanoparticle stacked bed porous insulation material.
[0010] Preferably, the drying process of the wood powder in step (1) and the nano-silicon dioxide particles in step (2) is: placing them in a vacuum drying oven at 50 to 80° C. and drying them for 6 to 12 hours.
[0011] Preferably, in step (2), the ball mill is used for ball milling at a speed of 80 to 180 r / min for 180 to 360 min.
[0012] Preferably, in step (3), the pressing pressure is 10 MPa and the holding time is 60 to 120 seconds.
[0013] Preferably, in step (4), the temperature rise rate of the tube furnace is 5 to 10° C. / min.
[0014] In order to achieve the purpose of the invention, the present invention also provides a method for preparing a wood powder silicon dioxide composite nanoparticle packed bed porous thermal insulation material, and a wood powder silicon dioxide composite nanoparticle packed bed porous thermal insulation material.
[0015] The present invention uses easily available and inexpensive wood fiber as reinforcing fiber. After carbonization, not only can the mechanical properties be enhanced and the thermal shrinkage be reduced, but also the volume of the wood fiber is greatly reduced after carbonization, a large number of pores are created, and the overall density of the material is reduced while the thermal insulation performance is enhanced. At the same time, the price of wood fiber is very low, so the final product prepared by the present invention has a very high cost performance.
[0016] Compared with the prior art, the thermal conductivity of the wood powder silicon dioxide composite nanoparticle stacked bed porous insulation material prepared by the present invention is 0.04342-0.0492 Wm -1 K -1 The shrinkage is 6.1-11.36% and the density is 0.3323-0.3778 g·cm -3. It can be seen that the nanoparticle stacked bed porous insulation material prepared by the present invention has the advantages of high porosity, low thermal conductivity, and stronger resistance to heat shrinkage, which can improve the service life and thermal insulation performance of the insulation material in a medium temperature environment. The present invention utilizes the wood powder waste generated by cutting wood, and prepares porous insulation materials based on nano-silicon dioxide powder. It has the advantages of low cost, simple process, environmental protection, high yield rate, and large-scale production. In addition, through the composite structure of wood fiber and particles, the internal pore size is reduced and the structural performance is enhanced. Compared with the single powder stacked porous insulation material, the wood powder silica composite nanoparticle stacked porous insulation material has stronger resistance to heat shrinkage, which improves the service life and thermal insulation performance of the insulation material in a medium temperature environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 These are SEM images of the thermal insulation material prepared in Example 1, (a) 10 μm scale, (b) 20 μm scale, and (c) 50 μm scale;
[0018] Figure 2 These are SEM images of the thermal insulation material obtained in Example 2, (a) 10 μm scale, (b) 25 μm scale, and (c) 200 μm scale. DETAILED DESCRIPTION
[0019] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.
[0020] Embodiment 1
[0021] A method for preparing a porous thermal insulation material of a wood powder and silicon dioxide composite nanoparticle stacked bed, comprising the following steps:
[0022] (1) collecting wood powder generated by cutting wood, screening and processing to obtain wood powder with a particle size of about 74 μm, placing the wood powder in a vacuum drying oven at 50° C. and drying for 6 h for later use;
[0023] (2) placing the nano-silicon dioxide particles with a particle size of 10 nm in a vacuum drying oven at 50° C. and drying for 6 h, then placing them in a ball mill at room temperature with the wood powder obtained in step (1) at a mass ratio of 19:1, and ball milling them at a speed of 80 r / min for 360 min, and mixing them evenly to obtain a wood powder-silicon dioxide mixed powder;
[0024] (3) Under room temperature, weigh an appropriate amount of wood flour and silicon dioxide mixed powder and put it into a mold, and press it into a cake-shaped wood flour and silicon dioxide composite porous material by cold pressing; the pressing pressure is 10 MPa, and the holding time is 60 s;
[0025] (4) The cake-shaped wood powder-silica composite porous material is placed in a tubular furnace and vacuum sintered and carbonized for 300 minutes at a temperature of 600°C. The temperature rise rate of the tubular furnace is 10°C / min, and a wood powder-silica composite nanoparticle stacked bed porous insulation material is obtained.
[0026] from Figure 1 (a) shows clearly that there is carbonized wood chips inside the sample. Figure 1 In (b), it can be seen that the added wood chips are carbonized and attached to multiple silica deposits, which enhances the microstructural properties of the insulation material and creates a large number of closed pores, thereby improving the insulation performance. Figure 1 (c) It can be seen that there are a large number of attachment structures inside the material, which can enhance the overall structure and thermal insulation performance of the material. The wood powder silica composite nanoparticle stacked bed porous thermal insulation material prepared in this embodiment has a lower thermal shrinkage rate than pure silica thermal insulation material, and has a longer medium and high temperature service life. The thermal conductivity of the thermal insulation material prepared in this embodiment is 0.04342W / (m·K) (a decrease of 16.67% compared to the thermal conductivity of pure silica thermal insulation material without adding sawdust); the shrinkage rate is 6.1% (a decrease of 13.47% compared to the shrinkage rate of pure silica thermal insulation material without adding sawdust); the density is 0.3323g·cm -3 (The density dropped by 4% compared to before sintering).
[0027] Embodiment 2
[0028] A method for preparing a porous thermal insulation material of a wood powder and silicon dioxide composite nanoparticle stacked bed, comprising the following steps:
[0029] (1) collecting wood powder generated by cutting wood, screening and processing to obtain wood powder with a particle size of about 74 μm, placing the wood powder in a vacuum drying oven at 50° C. and drying for 12 h for later use;
[0030] (2) placing the nano-silicon dioxide particles with a particle size of 10 nm in a vacuum drying oven at 80° C. and drying for 12 h, then placing them in a ball mill at room temperature with the wood powder obtained in step (1) at a mass ratio of 4:1, and ball milling them at a speed of 180 r / min for 180 min, and mixing them evenly to obtain a wood powder-silicon dioxide mixed powder;
[0031] (3) Under room temperature, weigh an appropriate amount of wood flour and silicon dioxide mixed powder and put it into a mold, and press it into a cake-shaped wood flour and silicon dioxide composite porous material by cold pressing; the pressing pressure is 10 MPa, and the holding time is 120 s;
[0032] (4) The cake-shaped wood powder-silica composite porous material is placed in a tubular furnace and vacuum sintered and carbonized for 180 minutes at a temperature of 750°C. The temperature rise rate of the tubular furnace is 5°C / min, and a wood powder-silica composite nanoparticle stacked bed porous insulation material is obtained.
[0033] from Figure 2 In (a), it can be observed that a large number of silica particle aggregates are attached to the wood fiber carbide, which enhances the structural performance and generates a large number of pores, thereby improving the thermal insulation performance. Figure 2 In (b), it can be observed that there are pores in the material due to the reduction in volume after the carbonization of wood fibers, and there are a large number of wood fiber carbonizations in the pores, which play a role in supporting the pores and enhancing the structural performance; Figure 2 (c) It can be seen that there are a large number of similar pore structures inside the material, which can improve the overall structure and thermal insulation performance of the material. The wood powder silica composite nanoparticle stacked bed porous thermal insulation material prepared in this embodiment has a lower thermal shrinkage rate than pure silica thermal insulation material, and has a longer medium and high temperature service life. The thermal conductivity of the thermal insulation material prepared in this embodiment is 0.0492W / (m·K) (4.4% lower than the thermal conductivity of pure silica thermal insulation material without adding sawdust); the shrinkage rate is 11.36% (11.1% lower than the shrinkage rate of pure silica thermal insulation material without adding sawdust); the density is 0.3378g·cm -3 (Compared with before sintering, the density decreased by 17.04%).
[0034] Embodiment 3
[0035] A method for preparing a porous thermal insulation material of a wood powder and silicon dioxide composite nanoparticle stacked bed, comprising the following steps:
[0036] (1) collecting wood powder generated by cutting wood, screening and processing to obtain wood powder with a particle size of about 74 μm, placing the wood powder in a vacuum drying oven at 50° C. and drying for 12 h for later use;
[0037] (2) placing the nano-silicon dioxide particles with a particle size of 60 nm in a vacuum drying oven at 50° C. and drying for 12 h, then placing them in a ball mill at room temperature with the wood powder obtained in step (1) at a mass ratio of 4:1, and ball milling them at a speed of 180 r / min for 360 min, and mixing them evenly to obtain a wood powder-silicon dioxide mixed powder;
[0038] (3) Under room temperature, weigh an appropriate amount of wood flour and silicon dioxide mixed powder and put it into a mold, and press it into a cake-shaped wood flour and silicon dioxide composite porous material by cold pressing; the pressing pressure is 10 MPa, and the holding time is 60 s;
[0039] (4) The cake-shaped wood powder-silica composite porous material is placed in a tubular furnace and vacuum sintered and carbonized for 300 minutes at a temperature of 750°C. The temperature rise rate of the tubular furnace is 5°C / min, and a wood powder-silica composite nanoparticle stacked bed porous insulation material is obtained.
[0040] The wood powder silicon dioxide composite nanoparticle stacked bed porous thermal insulation material prepared in this embodiment has a lower thermal shrinkage rate than pure nano silicon dioxide thermal insulation material, and has a longer medium and high temperature service life. The thermal conductivity of the thermal insulation material prepared in this embodiment is 0.04884W / (m·K) (6.35% lower than the thermal conductivity of the pure silicon dioxide thermal insulation material without adding sawdust); the shrinkage rate is 9.58% (9% lower than the shrinkage rate of the pure silicon dioxide thermal insulation material without adding sawdust); the density is 0.3498g·cm -3 (Compared with before sintering, the density is reduced by 17.02%).
[0041] Embodiment 4
[0042] A method for preparing a porous thermal insulation material of a wood powder and silicon dioxide composite nanoparticle stacked bed, comprising the following steps:
[0043] (1) collecting wood powder generated by cutting wood, screening and processing to obtain wood powder with a particle size of about 74 μm, placing the wood powder in a vacuum drying oven at 80° C. and drying for 6 h for later use;
[0044] (2) placing the nano-silicon dioxide particles with a particle size of 10 nm in a vacuum drying oven at 50° C. and drying for 6 h, then placing them in a ball mill at room temperature with the wood powder obtained in step (1) at a mass ratio of 19:1, and ball milling them at a speed of 80 r / min for 180 min, and mixing them evenly to obtain a wood powder-silicon dioxide mixed powder;
[0045] (3) Under room temperature, weigh an appropriate amount of wood flour and silicon dioxide mixed powder and put it into a mold, and press it into a cake-shaped wood flour and silicon dioxide composite porous material by cold pressing; the pressing pressure is 10 MPa, and the holding time is 120 s;
[0046] (4) The cake-like wood powder-silica composite porous material is placed in a tubular furnace and vacuum sintered and carbonized for 180 minutes at a temperature of 750°C. The temperature rise rate of the tubular furnace is 10°C / min, and a wood powder-silica composite nanoparticle stacked bed porous insulation material is obtained.
[0047] The wood powder silicon dioxide composite nanoparticle stacked bed porous thermal insulation material prepared in this embodiment has a lower thermal shrinkage rate than pure silicon dioxide thermal insulation material, and has a longer medium and high temperature service life. The thermal conductivity of the thermal insulation material prepared in this embodiment is 0.0485W / (m·K) (7% lower than the thermal conductivity of the pure silicon dioxide thermal insulation material without adding sawdust); the shrinkage rate is 9.09% (13.65% lower than the shrinkage rate of the pure silicon dioxide thermal insulation material without adding sawdust); the density is 0.3778g·cm -3 (The density is reduced by 5% compared to before sintering).
Claims
1. A method for preparing a porous thermal insulation material of wood powder and silicon dioxide composite nanoparticles packed bed, characterized in that: The following steps are involved: (1) collecting wood powder generated by cutting wood, screening and treating to obtain wood powder with a particle size of 53 to 104 μm, and drying for later use; (2) drying the nano-silicon dioxide particles with a particle size of 10 to 60 nm, and then placing them in a ball mill at room temperature with the wood powder obtained in step (1) at a mass ratio of (4 to 19):1, and mixing them evenly to obtain a wood powder and silicon dioxide mixed powder; (3) Under room temperature, weigh an appropriate amount of wood flour and silicon dioxide mixed powder and put it into a mold, and use a cold pressing method to press and mold a cake-shaped wood flour and silicon dioxide composite porous material; (4) Placing the cake-shaped wood powder-silica composite porous material in a tubular furnace, vacuum sintering and carbonizing it at a temperature of 600 to 750° C. for 180 to 300 minutes to obtain a wood powder-silica composite nanoparticle stacked bed porous insulation material.
2. The method for preparing a wood powder-silicon dioxide composite nanoparticle packed bed porous thermal insulation material according to claim 1, characterized in that: The drying process of the wood powder in step (1) and the nano-silicon dioxide particles in step (2) is as follows: placing them in a vacuum drying oven at 50 to 80° C. and drying them for 6 to 12 hours.
3. The method for preparing a wood powder-silicon dioxide composite nanoparticle packed bed porous thermal insulation material according to claim 1 or 2, characterized in that: In step (2), the ball mill is milled at a speed of 80 to 180 r / min for 180 to 360 min.
4. The method for preparing a wood powder-silicon dioxide composite nanoparticle packed bed porous thermal insulation material according to claim 1 or 2, characterized in that: In step (3), the pressing pressure is 10 MPa and the holding time is 60 to 120 seconds.
5. The method for preparing a wood powder-silicon dioxide composite nanoparticle packed bed porous thermal insulation material according to claim 1, characterized in that: In step (4), the temperature rise rate of the tubular furnace is 5 to 10°C / min. 6 . A wood powder-silicon dioxide composite nanoparticle packed bed porous thermal insulation material prepared by the method for preparing a wood powder-silicon dioxide composite nanoparticle packed bed porous thermal insulation material according to any one of claims 1 to 5.
Citation Information
Patent Citations
High-temperature Resistant Lightweight Thermal Insulation Material with Dual-pore Structure and Preparation Method Thereof
US20190300447A1