Epitaxial wafer preparation method for improving light emitting diode epitaxial wafer flying
Through step-by-step speed regulation and ammonia instead of hydrogen, the problem of substrate warping in the preparation of light-emitting diode epitaxial sheets is solved, the integrity and photoelectric performance of the epitaxial sheets are improved, and the high-quality preparation process is ensured.
Patent Information
- Application Number
- CN202210695932.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-20
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-06-20
AI Technical Summary
During the preparation of light emitting diode epitaxial sheets, the substrate is prone to warping and causing the epitaxial sheet to fly, which affects the preparation quality and photoelectric performance.
The step-by-step speed regulation is used to adjust the speed of the graphite disk, and ammonia is introduced into the reaction chamber to replace hydrogen, stabilize the substrate, reduce the risk of warping, and adjust the pressure and temperature in the reaction chamber before growing the epitaxial layer to ensure the substrate stability.
It effectively avoids substrate warping, improves the integrity and photoelectric properties of the epitaxial sheet, reduces the occurrence of epitaxial sheet flying sheets, and improves the preparation quality.
Smart Images

Figure CN115274938B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of optoelectronic manufacturing technology, and in particular to a method for preparing an epitaxial wafer for improving the flying wafer of a light emitting diode epitaxial wafer. Background Art
[0002] Light-emitting diode (Micro LED) is a semiconductor electronic component that can emit light. Light-emitting diode has the characteristics of self-luminescence, high brightness, high contrast, high responsiveness and power saving.
[0003] In the related art, a light-emitting diode epitaxial wafer includes a substrate and an epitaxial layer stacked on the substrate. During the preparation of the epitaxial wafer, before growing the epitaxial layer on the substrate, the substrate is usually placed in a graphite disk and hydrogen is introduced into the graphite disk to clean the substrate surface.
[0004] However, due to the etching effect of hydrogen, the substrate is likely to warp during the hydrogen treatment process; and because the graphite disk will rotate during the subsequent growth of the epitaxial layer, the warped epitaxial wafer is likely to fly out of the graphite disk under the action of centrifugal force, resulting in flying wafers, which is not conducive to the preparation of epitaxial wafers. Summary of the invention
[0005] The disclosed embodiment provides a method for preparing an epitaxial wafer for improving the flying of light-emitting diode epitaxial wafers, which can effectively improve the problem of the flying of epitaxial wafers caused by the warping of the substrate during the process of growing the epitaxial layer.
[0006] The technical solution is as follows:
[0007] On the one hand, an embodiment of the present disclosure provides a method for preparing an epitaxial wafer for improving the flying of light-emitting diode epitaxial wafers, the method comprising: placing a substrate into a graphite disk in a reaction chamber; introducing ammonia gas into the reaction chamber; adjusting the rotation speed of the graphite disk by at least one step-by-step speed regulation until the rotation speed of the graphite disk meets the set rotation speed, the step-by-step speed regulation comprising a first stage, a second stage, a third stage and a fourth stage executed in sequence, in the first stage, the rotation speed of the graphite disk is controlled to increase, in the second stage, the rotation speed of the graphite disk is controlled to decrease, in the third stage, the rotation speed of the graphite disk is controlled to increase, in the fourth stage, the rotation speed of the graphite disk is controlled to remain unchanged, in the same step-by-step speed regulation, the maximum rotation speed of the graphite disk in the first stage is less than the maximum rotation speed of the graphite disk in the third stage; and growing an epitaxial layer on the substrate.
[0008] Optionally, in the same step speed regulation, the maximum speed of the graphite disk in the first stage is 0 to 30 rpm higher than the minimum speed of the graphite disk in the second stage; the maximum speed of the graphite disk in the first stage is 0 to 70 rpm lower than the maximum speed of the graphite disk in the third stage.
[0009] Optionally, the set speed is 120rpm to 150rpm; the adopting at least one step-by-step speed regulation to adjust the speed of the graphite disk until the speed of the graphite disk meets the set speed includes: performing the first step-by-step speed regulation on the graphite disk, in the first step-by-step speed regulation, in the first stage, controlling the speed of the graphite disk to increase to V1, in the second stage, controlling the speed of the graphite disk to decrease to V2, in the third stage, controlling the speed of the graphite disk to increase to V3, and in the fourth stage, controlling the speed of the graphite disk to maintain at V3, V3>V1>V2, 40rpm≤V1≤60rpm pm, 30rpm≤V2≤40rpm, 60rpm≤V3≤80rpm; the graphite disk is subjected to the second step-by-step speed regulation, in which the rotational speed of the graphite disk is controlled to increase to V4 in the first stage, the rotational speed of the graphite disk is controlled to decrease to V5 in the second stage, the rotational speed of the graphite disk is controlled to increase to V6 in the third stage, and the rotational speed of the graphite disk is controlled to be maintained at V6 in the fourth stage, V6>V4>V5, 80rpm≤V4≤100rpm, 80rpm≤V5≤90rpm, 120rpm≤V6≤150rpm.
[0010] Optionally, in the first step-by-step speed regulation, the duration of the first stage is 1 min to 2 min, the duration of the second stage is 1.5 min to 3 min, the duration of the third stage is 2 min to 4 min, and the duration of the fourth stage is 1.5 min to 3 min.
[0011] Optionally, in the second step speed regulation, the duration of the first stage is 2 minutes to 3 minutes, the duration of the second stage is 2.5 minutes to 4 minutes, the duration of the third stage is 3 minutes to 4 minutes, and the duration of the fourth stage is 2.5 minutes to 4 minutes.
[0012] Optionally, the flow rate of ammonia gas introduced into the reaction chamber is 100 sccm to 500 sccm.
[0013] Optionally, before introducing ammonia gas into the reaction chamber, the process includes: adjusting the pressure in the reaction chamber to 600 torr to 800 torr.
[0014] Optionally, before growing the epitaxial layer on the substrate, the method includes: adjusting the temperature in the reaction chamber to 800° C. to 1200° C. and maintaining the temperature for a set period of time to remove ammonia in the reaction chamber.
[0015] Optionally, the set duration is 3 minutes to 6 minutes.
[0016] Optionally, growing an epitaxial layer on the substrate comprises: sequentially growing a buffer layer, a GaN layer, an n-type layer, an active layer, an electron blocking layer and a p-type layer on the substrate.
[0017] The beneficial effects brought by the technical solution provided by the embodiments of the present disclosure include at least:
[0018] The disclosed embodiment provides a method for preparing an epitaxial wafer. When pre-treating a substrate, ammonia as a reaction gas is first introduced into the reaction chamber. Since ammonia is one of the reaction gases, it can stabilize the substrate when it flows onto the substrate through the gas flow. Moreover, replacing hydrogen with ammonia can also effectively avoid the etching effect of hydrogen, thereby preventing the substrate from warping significantly.
[0019] Then, the speed of the graphite disk is increased to meet the speed requirement of growing the epitaxial layer. When increasing the speed of the graphite disk, at least one step-by-step speed regulation is adopted until the speed of the graphite disk meets the set speed. Among them, the step-by-step speed regulation includes four stages. In the first stage, the speed of the graphite disk is increased first, in the second stage, the speed of the graphite disk is reduced, and in the third stage, the speed of the graphite disk is increased again, and the maximum speed of the graphite disk in the third stage is ensured to be greater than the maximum speed of the first stage, and finally the speed of the graphite disk is stabilized. In this way, the warping effect of the centrifugal force on the substrate is reduced by slightly increasing the speed, and the speed will be reduced again in the second stage in order to release the warping change of the substrate when the speed is increased. Finally, the speed is increased in the third and fourth stages, which can achieve the required set speed without causing a large change in the warping of the substrate. In this way, the problem of warping of the substrate and the flying of the epitaxial wafer caused by the flying of the epitaxial wafer in the process of growing the epitaxial layer can be greatly improved, the integrity and appearance quality of the epitaxial wafer can be improved, the situation of the epitaxial wafer flying and damaging the graphite disk can be avoided, and the optoelectronic performance of the epitaxial wafer can be guaranteed. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the technical solutions in the embodiments of the present disclosure, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0021] Figure 1 is a flow chart of a method for preparing an epitaxial wafer provided in an embodiment of the present disclosure;
[0022] Figure 2 is a flow chart of another epitaxial wafer preparation method provided by an embodiment of the present disclosure;
[0023] Figure 3 It is a schematic diagram of the structure of an epitaxial wafer provided in an embodiment of the present disclosure.
[0024] The descriptions of the marks in the figure are as follows:
[0025] 10. Substrate; 11. Buffer layer; 12. GaN layer; 13. n-type layer; 14. Active layer; 15. Electron blocking layer; 16. p-type layer. DETAILED DESCRIPTION
[0026] In order to make the objectives, technical solutions and advantages of the present disclosure more clear, the embodiments of the present disclosure will be further described in detail below with reference to the accompanying drawings.
[0027] Unless otherwise defined, the technical terms or scientific terms used herein shall have the usual meanings understood by persons with ordinary skills in the field to which the present disclosure belongs. The words "first", "second", "third" and similar words used in the patent application specification and claims of the present disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, words such as "one" or "one" do not indicate a quantity limitation, but indicate the existence of at least one. Words such as "include" or "comprise" and similar words mean that the elements or objects appearing before "include" or "comprise" include the elements or objects listed after "include" or "comprise" and their equivalents, and do not exclude other elements or objects. Words such as "connect" or "connected" and similar words are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right", "top", "bottom" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.
[0028] Figure 1 1 is a flow chart of a method for preparing an epitaxial wafer provided in an embodiment of the present disclosure. Figure 1 As shown, the epitaxial wafer preparation method comprises:
[0029] Step 101: Place the substrate into a graphite plate in a reaction chamber.
[0030] Step 102: Introduce ammonia gas into the reaction chamber.
[0031] Step 103: adjusting the rotation speed of the graphite disk by at least one step-wise speed regulation until the rotation speed of the graphite disk meets the set rotation speed.
[0032] Among them, the step-by-step speed regulation includes the first stage, the second stage, the third stage and the fourth stage which are executed in sequence. In the first stage, the rotation speed of the graphite disk is controlled to increase, in the second stage, the rotation speed of the graphite disk is controlled to decrease, in the third stage, the rotation speed of the graphite disk is controlled to increase, and in the fourth stage, the rotation speed of the graphite disk is controlled to remain unchanged. The maximum rotation speed of the graphite disk in the first stage is less than the maximum rotation speed of the graphite disk in the third stage.
[0033] Step 104: growing an epitaxial layer on the substrate.
[0034] The disclosed embodiment provides a method for preparing an epitaxial wafer. When pre-treating a substrate, ammonia as a reaction gas is first introduced into the reaction chamber. Since ammonia is one of the reaction gases, it can stabilize the substrate when it flows onto the substrate through the gas flow. Moreover, replacing hydrogen with ammonia can also effectively avoid the etching effect of hydrogen, thereby preventing the substrate from warping significantly.
[0035] Then, the speed of the graphite disk is increased to meet the speed requirement of growing the epitaxial layer. When increasing the speed of the graphite disk, at least one step-by-step speed regulation is adopted until the speed of the graphite disk meets the set speed. Among them, the step-by-step speed regulation includes four stages. In the first stage, the speed of the graphite disk is increased first, in the second stage, the speed of the graphite disk is reduced, and in the third stage, the speed of the graphite disk is increased again, and the maximum speed of the graphite disk in the third stage is ensured to be greater than the maximum speed of the first stage, and finally the speed of the graphite disk is stabilized. In this way, the warping effect of the centrifugal force on the substrate is reduced by slightly increasing the speed, and the speed will be reduced again in the second stage in order to release the warping change of the substrate when the speed is increased. Finally, the speed is increased in the third and fourth stages, which can achieve the required set speed without causing a large change in the warping of the substrate. In this way, the problem of warping of the substrate and the flying of the epitaxial wafer caused by the flying of the epitaxial wafer in the process of growing the epitaxial layer can be greatly improved, the integrity and appearance quality of the epitaxial wafer can be improved, the situation of the epitaxial wafer flying and damaging the graphite disk can be avoided, and the optoelectronic performance of the epitaxial wafer can be guaranteed.
[0036] Figure 2 FIG. 1 is a flow chart of another epitaxial wafer preparation method provided by an embodiment of the present disclosure. Figure 2 As shown, the epitaxial wafer preparation method comprises:
[0037] Step 201: Place the substrate into a graphite plate in a reaction chamber.
[0038] Optionally, the substrate is a sapphire substrate, a silicon substrate or a silicon carbide substrate. The substrate can be a flat substrate or a patterned substrate.
[0039] As an example, in the embodiment of the present disclosure, the substrate is a sapphire substrate. The sapphire substrate is a commonly used substrate with mature technology and low cost. Specifically, it can be a patterned sapphire substrate or a sapphire flat sheet substrate.
[0040] In the disclosed embodiment, the reaction chamber may be a reaction chamber of a MOCVD (Metal organic Chemical Vapor Depositio) device.
[0041] Step 202: Adjust the pressure in the reaction chamber to 600 torr to 800 torr.
[0042] Before introducing ammonia into the reaction chamber, the pressure in the reaction chamber is quickly increased. This can fix the substrate in the groove of the graphite disk as much as possible through the effect of high pressure, thereby enhancing the stability of the substrate.
[0043] By controlling the pressure in the reaction chamber within the above range, it is possible to avoid the situation where the pressure is too low, resulting in a poor stabilization effect of the pressure on the substrate, and it is also possible to avoid the situation where the pressure in the reaction chamber is too high, resulting in a long time required to increase the pressure in the reaction chamber.
[0044] Exemplarily, step 201 may include controlling the pressure in the reaction chamber to 650 torr. Controlling the pressure in the reaction chamber to this temperature can ensure that the substrate can be stabilized after the pressure is increased, and the time spent on increasing the pressure will not increase.
[0045] As an example, in the embodiment of the present disclosure, the pressure in the reaction chamber can also be adjusted to 650 torr to 800 torr.
[0046] Step 203: introducing ammonia gas into the reaction chamber.
[0047] The flow rate of ammonia gas introduced into the reaction chamber is 100 sccm to 500 sccm.
[0048] Compared with the related art, replacing hydrogen with ammonia and introducing ammonia into the reaction chamber can stabilize the substrate; and can also effectively avoid the etching effect of hydrogen, thereby preventing the substrate from warping significantly.
[0049] In the above implementation, by controlling the flow rate of the ammonia gas to be within the above range, it is possible to avoid a flow rate that is too small, resulting in less ammonia gas being introduced and affecting the function of stabilizing the substrate; and it is also possible to avoid a flow rate that is too large, resulting in more ammonia gas being introduced and affecting the time of subsequent processing.
[0050] As an example, in the embodiment of the present disclosure, the flow rate of ammonia gas introduced into the reaction chamber may be 200 sccm to 400 sccm, which can maximize the stabilizing effect of ammonia gas on the substrate and avoid increasing the subsequent treatment time of removing ammonia gas due to excessive amount of ammonia gas introduced.
[0051] Exemplarily, the flow rate of ammonia gas introduced into the reaction chamber may be 300 sccm.
[0052] Step 204: adjusting the rotation speed of the graphite disk by at least one step-wise speed regulation until the rotation speed of the graphite disk meets the set rotation speed.
[0053] Among them, the step speed regulation includes the first stage, the second stage, the third stage and the fourth stage which are executed in sequence. In the first stage, the rotation speed of the graphite disk is controlled to increase, in the second stage, the rotation speed of the graphite disk is controlled to decrease, in the third stage, the rotation speed of the graphite disk is controlled to increase, and in the fourth stage, the rotation speed of the graphite disk is controlled to remain unchanged. In the same step speed regulation, the maximum rotation speed of the graphite disk in the first stage is less than the maximum rotation speed of the graphite disk in the third stage.
[0054] Since the step-type speed regulation includes four stages, the speed of the graphite disk is increased in the first stage, the speed of the graphite disk is reduced in the second stage, and the speed of the graphite disk is increased again in the third stage, and the maximum speed of the graphite disk in the third stage is ensured to be greater than the maximum speed in the first stage, and finally the speed of the graphite disk is stabilized.
[0055] In this way, the centrifugal force on the substrate warping is reduced by slightly increasing the speed. In the second stage, the speed is reduced again to release the substrate warping change when the speed is increased. Finally, the speed is increased in the third and fourth stages to achieve the required set speed without causing a large change in the substrate warping. This can greatly improve the problem of epitaxial wafer flying caused by the substrate warping during the growth of the epitaxial layer, and improve the integrity and appearance quality of the epitaxial wafer.
[0056] Optionally, in the same step-wise speed regulation, the maximum rotational speed of the graphite disk in the first stage is 0 to 30 rpm higher than the minimum rotational speed of the graphite disk in the second stage.
[0057] This can prevent the rotation speed of the graphite disk from decreasing too much in the second stage, which will slow down the overall speed of the graphite disk and increase the processing time of the substrate; it can also prevent the rotation speed of the graphite disk from decreasing too little, which will fail to release the warping change of the substrate when the rotation speed is increased.
[0058] Optionally, in the same step-wise speed regulation, the maximum rotational speed of the graphite disk in the first stage is 0 to 70 rpm lower than the maximum rotational speed of the graphite disk in the third stage.
[0059] This can prevent the rotation speed of the graphite disk from increasing too much in the third stage, which may cause the substrate to warp easily; it can also prevent the rotation speed of the graphite disk from increasing too little, which may cause the overall speed of the graphite disk to increase slowly and increase the processing time of the substrate.
[0060] And the maximum speed of the third stage is higher than the maximum speed of the first stage, so as to ensure that after one step speed regulation, the speed of the graphite disk can be increased to a certain extent, so that the speed of the graphite disk can be gradually increased to the set speed through multiple step speed regulation.
[0061] In the disclosed embodiment, the set rotation speed may be 120 rpm to 150 rpm.
[0062] In the process of controlling the rotation speed of the graphite disk, if the rotation speed of the graphite disk is directly adjusted to the set rotation speed at one time, the substrate may be easily warped due to the centrifugal force.
[0063] To this end, in the embodiment disclosed herein, two consecutive step-by-step speed adjustments are used to gradually adjust the rotation speed of the graphite disk to 120 rpm to 150 rpm.
[0064] Step 204 may specifically include the following two steps:
[0065] The first step is to perform the first step speed adjustment on the graphite disk.
[0066] Among them, in the first step speed regulation, the speed of the graphite disk is controlled to increase to V1 in the first stage, the speed of the graphite disk is controlled to decrease to V2 in the second stage, the speed of the graphite disk is controlled to increase to V3 in the third stage, and the speed of the graphite disk is controlled to be maintained at V3 in the fourth stage, V3>V1>V2, 40rpm≤V1≤60rpm, 30rpm≤V2≤40rpm, 60rpm≤V3≤80rpm.
[0067] In the second step, the graphite disk is adjusted in a second step.
[0068] Among them, in the second step speed regulation, the speed of the graphite disk is controlled to increase to V4 in the first stage, the speed of the graphite disk is controlled to decrease to V5 in the second stage, the speed of the graphite disk is controlled to increase to V6 in the third stage, and the speed of the graphite disk is controlled to be maintained at V6 in the fourth stage, V6>V4>V5, 80rpm≤V4≤100rpm, 80rpm≤V5≤90rpm, 120rpm≤V6≤150rpm.
[0069] In the disclosed embodiment, two step-by-step speed regulation is adopted. In the first step-by-step speed regulation, the duration of the first stage is 1min to 2min, so that the rotation speed of the graphite disk is first controlled to slowly rise to 40rpm to 60rpm. The rotation speed range of this section changes less, and the effect on the warping effect of the substrate is small. The duration of the second stage is 1.5min to 3min, so the rotation speed of the graphite disk is controlled to decrease to 30rpm to 40rpm, mainly to slightly reduce the rotation speed and release the stress changes caused by the warping generated in the previous part. The duration of the third stage is 2min to 4min, so the rotation speed of the graphite disk is controlled to slowly rise to 60rpm to 80rpm, and the rotation speed is slightly increased again to prepare for the next increase in the rotation speed. The duration of the fourth stage is 2min to 4min, that is, the rotation speed of the graphite disk is finally stabilized at 60rpm to 80rpm, which lasts for 2min to 4min.
[0070] During the second step-by-step speed regulation, the duration of the first stage is 2 to 3 minutes. In this way, the speed of the graphite disk is slowly increased to 80 rpm to 100 rpm. The speed increased in this section is based on the first step-by-step speed regulation, which reduces the production time. The duration of the second stage is 2.5 to 4 minutes. In this way, the speed of the graphite disk is controlled to be reduced to 80 rpm to 90 rpm. Since the speed has been increased twice in a row, the stress caused by the change in warping will be superimposed, so it is released again by reducing the speed. The duration of the third stage is 3 to 4 minutes. In this way, the speed of the graphite disk is slowly increased to 120 rpm to 150 rpm. The duration of the fourth stage is 2.5 to 4 minutes. Finally, the speed of the graphite disk is controlled to be stable at 120 rpm to 150 rpm and lasts for 2.5 to 4 minutes. Because the stress change of warping has been released back and forth several times, in order to improve efficiency, it can be increased to the set speed and stabilized at this time.
[0071] Step 205: Adjust the temperature in the reaction chamber to 800° C. to 1200° C. and maintain it for a set time to remove ammonia in the reaction chamber.
[0072] After the substrate is pretreated with ammonia, the ammonia in the reaction chamber needs to be removed to prevent the ammonia from affecting the growth of the thick epitaxial layer. In the embodiment of the present disclosure, the ammonia in the reaction chamber is decomposed by increasing the temperature in the reaction chamber.
[0073] By setting the temperature in the reaction chamber within the above range, it is possible to avoid the temperature being too low, which would affect the decomposition effect of ammonia, and it is also possible to avoid the temperature being too high, which would increase the heating time required to increase the temperature and increase the substrate processing time.
[0074] Optionally, the duration is set to 3 minutes to 6 minutes. Setting the duration within the above range can prevent the ammonia high temperature treatment from being too short, resulting in incomplete decomposition of the ammonia; and can also prevent the ammonia high temperature treatment from being too long, thereby increasing the substrate treatment time.
[0075] Exemplarily, the set duration may be 5 minutes.
[0076] Step 206: sequentially growing a buffer layer, a GaN layer, an n-type layer, an active layer, an electron blocking layer and a p-type layer on the substrate.
[0077] In the embodiment of the present disclosure, when growing the epitaxial layer, high-purity hydrogen or high-purity nitrogen or a mixture of high-purity hydrogen and high-purity nitrogen is used as a carrier gas, high-purity ammonia is used as an N source, trimethyl gallium (TMGa) and triethyl gallium (TEGa) are used as gallium sources, trimethyl indium (TMIn) is used as an indium source, silane is used as an N-type dopant, trimethyl aluminum (TMAl) is used as an aluminum source, and bis(cyclopentadienyl) magnesium (CP2Mg) is used as a P-type dopant. The pressure of the reaction chamber is 100 torr to 600 torr.
[0078] Figure 3 Schematic diagram of the structure of an epitaxial wafer provided by an embodiment of the present disclosure. Figure 3 As shown, when growing the buffer layer 11 , the growth temperature is controlled to be 530° C. to 560° C., and the growth pressure is controlled to be 200 torr to 500 torr, so that a buffer layer 11 is formed on the substrate 10 .
[0079] The thickness of the buffer layer may be 10 nm to 30 nm. For example, the thickness of the buffer layer is 20 nm.
[0080] Exemplarily, the buffer layer may be an AlN layer.
[0081] like Figure 3 As shown, when growing the GaN layer 12 , the growth temperature is controlled to be 1000° C. to 1100° C., and the growth pressure is controlled to be 200 torr to 600 torr, so that a GaN layer 12 is formed on the buffer layer 11 .
[0082] In the implementation of the present disclosure, the GaN layer is a high-temperature buffer layer, and the GaN layer may be undoped.
[0083] The thickness of the GaN layer is 2 μm to 3.5 μm. For example, the thickness of the GaN layer is 3 μm.
[0084] like Figure 3 As shown, when growing the n-type layer 13 , the growth temperature is controlled to be 1000° C. to 1100° C., and the growth pressure is controlled to be 150 torr to 300 torr, so that an n-type layer 13 is formed on the GaN layer 12 .
[0085] The thickness of the n-type layer is 2 μm to 3 μm, for example, the thickness of the n-type layer is 2.5 μm.
[0086] Illustratively, the n-type layer may be a Si-doped GaN layer.
[0087] like Figure 3 As shown, when growing the active layer 14 , the growth temperature is controlled to be 700° C. to 900° C., and the growth pressure is controlled to be 150 torr to 300 torr, and the active layer 14 is formed on the n-type layer 13 .
[0088] The active layer may include alternately grown InGaN well layers and GaN barrier layers. When growing the InGaN well layers, the reaction chamber temperature is 760°C to 780°C and the reaction chamber pressure is 200 torr; when growing the GaN barrier layers, the reaction chamber temperature is 860°C to 890°C and the reaction chamber pressure is 200 torr.
[0089] Exemplarily, the thickness of the active layer is 150 nm to 200 nm, for example, the thickness of the active layer is 150 nm.
[0090] like Figure 3 As shown, when growing the electron blocking layer 15 , the growth temperature is controlled to be 930° C. to 970° C., and the growth pressure is controlled to be 150 torr to 200 torr, so that the electron blocking layer 15 is formed on the active layer 14 .
[0091] The thickness of the electron blocking layer is 30 nm to 50 nm. For example, the thickness of the electron blocking layer is 40 nm.
[0092] For example, the electron blocking layer is Al-doped or Mg-doped Al y Ga 1-y N, y = 0.15-0.25.
[0093] like Figure 3 As shown, when the p-type layer 16 is grown, the growth temperature is controlled to be 940° C. to 980° C., and the growth pressure is controlled to be 200 torr to 600 torr, so that the p-type layer 16 is formed on the electron blocking layer 15 .
[0094] The thickness of the p-type layer is 50 nm to 80 nm. For example, the thickness of the p-type layer is 60 nm.
[0095] Exemplarily, the p-type layer may be a high-temperature, highly Mg-doped GaN layer.
[0096] Finally, the epitaxial wafer is annealed.
[0097] Optionally, annealing can be performed in a nitrogen atmosphere for 30 minutes to terminate the growth of the epitaxial wafer, and then the heating system and the gas supply system are turned off until the temperature of the reaction chamber drops to room temperature.
[0098] The above description is only an optional embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure shall be included in the protection scope of the present disclosure.
Claims
1. A method for preparing an epitaxial wafer for improving the flying of light-emitting diode epitaxial wafers, characterized in that: The epitaxial wafer preparation method comprises: placing the substrate into a graphite tray in a reaction chamber; introducing ammonia gas into the reaction chamber; The rotation speed of the graphite disk is adjusted by at least one step-by-step speed regulation until the rotation speed of the graphite disk meets the set rotation speed, the step-by-step speed regulation includes a first stage, a second stage, a third stage and a fourth stage which are sequentially executed, in which the rotation speed of the graphite disk is controlled to increase in the first stage, the rotation speed of the graphite disk is controlled to decrease in the second stage, the rotation speed of the graphite disk is controlled to increase in the third stage, and the rotation speed of the graphite disk is controlled to remain unchanged in the fourth stage, and in the same step-by-step speed regulation, the maximum rotation speed of the graphite disk in the first stage is less than the maximum rotation speed of the graphite disk in the third stage; An epitaxial layer is grown on the substrate.
2. The method for preparing an epitaxial wafer according to claim 1, characterized in that: In the same step-by-step speed regulation, the maximum speed of the graphite disk in the first stage is 0 to 30 rpm higher than the minimum speed of the graphite disk in the second stage; The maximum rotation speed of the graphite disk in the first stage is 0 to 70 rpm lower than the maximum rotation speed of the graphite disk in the third stage.
3. The method for preparing an epitaxial wafer according to claim 2, characterized in that: The set speed is 120 rpm to 150 rpm; the step of adjusting the speed of the graphite disk by at least one step-wise speed regulation until the speed of the graphite disk meets the set speed includes: The graphite disk is subjected to the first step-wise speed regulation, wherein in the first step-wise speed regulation, the rotation speed of the graphite disk is controlled to increase to V1 in the first stage, the rotation speed of the graphite disk is controlled to decrease to V2 in the second stage, the rotation speed of the graphite disk is controlled to increase to V3 in the third stage, and the rotation speed of the graphite disk is controlled to be maintained at V3 in the fourth stage, V3>V1>V2, 40rpm≤V1≤60rpm, 30rpm≤V2≤40rpm, 60rpm≤V3≤80rpm; The graphite disk is subjected to the second step-wise speed regulation. In the second step-wise speed regulation, the rotational speed of the graphite disk is controlled to increase to V4 in the first stage, the rotational speed of the graphite disk is controlled to decrease to V5 in the second stage, the rotational speed of the graphite disk is controlled to increase to V6 in the third stage, and the rotational speed of the graphite disk is controlled to be maintained at V6 in the fourth stage, V6>V4>V5, 80rpm≤V4≤100rpm, 80rpm≤V5≤90rpm, 120rpm≤V6≤150rpm.
4. The method for preparing an epitaxial wafer according to claim 3, characterized in that: In the first step-by-step speed regulation, the duration of the first stage is 1 min to 2 min, the duration of the second stage is 1.5 min to 3 min, the duration of the third stage is 2 min to 4 min, and the duration of the fourth stage is 1.5 min to 3 min.
5. The method for preparing an epitaxial wafer according to claim 3, characterized in that: In the second step speed regulation, the duration of the first stage is 2 minutes to 3 minutes, the duration of the second stage is 2.5 minutes to 4 minutes, the duration of the third stage is 3 minutes to 4 minutes, and the duration of the fourth stage is 2.5 minutes to 4 minutes.
6. The method for preparing an epitaxial wafer according to any one of claims 1 to 5, characterized in that: The flow rate of ammonia gas introduced into the reaction chamber is 100 sccm to 500 sccm.
7. The method for preparing an epitaxial wafer according to any one of claims 1 to 5, characterized in that: Before introducing ammonia gas into the reaction chamber, the method includes: adjusting the pressure in the reaction chamber to 600 torr to 800 torr.
8. The method for preparing an epitaxial wafer according to any one of claims 1 to 5, characterized in that: Before growing the epitaxial layer on the substrate, the method includes: adjusting the temperature in the reaction chamber to 800° C. to 1200° C. and maintaining it for a set time to remove ammonia in the reaction chamber.
9. The method for preparing an epitaxial wafer according to claim 8, characterized in that: The set time length is 3 minutes to 6 minutes.
10. The method for preparing an epitaxial wafer according to any one of claims 1 to 5, characterized in that: The step of growing an epitaxial layer on the substrate comprises: A buffer layer, a GaN layer, an n-type layer, an active layer, an electron blocking layer and a p-type layer are sequentially grown on the substrate.