A kind of wear-resistant cleaning paper tape

By using water glass, adhesives of phosphate base materials and modified starch in paper tape, combined with the wear-resistant layer of glass fiber cloth, the problem of insufficient stickiness of paper tape is solved, and efficient wear resistance and clean environmental protection performance is achieved.

CN115353823BActive Publication Date: 2024-11-15GUANGZHOU YINGYUAN STATIONERY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211082681.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-06
Publication Date
2024-11-15
Estimated Expiration
2042-09-06

AI Technical Summary

Technical Problem

The existing paper tape is not sticky enough, making it difficult to meet the needs of wear resistance and cleanliness and environmental protection.

Method used

Using adhesives made of water glass and phosphate as base materials, modified starch, modified calcium sulfate whiskers, fly ash, boric acid, D-sorbitol, iron tetraoxide, kaolin, silane coupling agent KH550 and gas phase Components such as silica form wear-resistant cleaning paper tape with a wear-resistant layer of fiberglass cloth to ensure adhesion and stickiness.

Benefits of technology

It realizes wear-resistant cleaning paper tape without volatile substances, has good adhesion and stickiness, significantly improves wear-resistant effect and meets the requirements of cleaning and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115353823B_ABST
    Figure CN115353823B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of paper tapes, and the present invention specifically discloses a wear-resistant cleaning paper tape, wherein the wear-resistant cleaning paper tape comprises a first adhesive layer, a kraft paper layer, a second adhesive layer, and a wear-resistant layer from bottom to top, wherein the first adhesive layer is formed by coating an adhesive below the kraft paper layer, and the second adhesive layer is formed by coating an adhesive above the kraft paper layer, and the second adhesive layer is used to connect the kraft paper layer and the wear-resistant layer. The adhesive is prepared from the following raw materials: water glass, phosphate, modified starch, modified calcium sulfate whisker, fly ash, boric acid, D-sorbitol, ferric oxide, kaolin, silane coupling agent KH550, fumed silica, and methyl hydroxypropyl cellulose. The wear-resistant cleaning paper tape does not contain volatile substances, has good cleaning and environmental protection, and has good bonding force and stickiness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of paper tapes, and in particular to a wear-resistant cleaning paper tape. Background Art

[0002] Paper tapes can be divided into kraft paper tapes, sealing paper tapes, stationery tapes, masking tapes, etc. according to different materials. Compared with general tapes, paper tapes are usually not as sticky. Paper tapes are generally made in various colors and patterns, so they are widely used in paper pasting, beautification, layout, DIY and other purposes. How to improve the stickiness of paper tapes has become a technical problem that needs to be solved urgently by technicians in this field.

[0003] Patent CN104371586A discloses a highly wear-resistant insulating paper tape, which can be considered as the closest prior art to the present invention, and specifically discloses a composite adhesive layer, a rubber layer, a paper layer and a wear-resistant layer stacked in sequence from top to bottom, wherein the rubber layer is a mixed adhesive layer of nitrile rubber and silicone rubber; the wear-resistant layer is a glass fiber cloth layer, and the glass fiber cloth layer and the paper layer are bonded together by an adhesive. It uses a mixed adhesive layer of nitrile rubber and silicone rubber to make the tape have good heat resistance and cold resistance, and adheres a layer of glass fiber cloth to the outside of the paper layer, which effectively improves the wear resistance of the tape. First, it uses nitrile rubber and silicone rubber, which have certain volatility, and secondly, its viscosity still needs to be improved. Summary of the invention

[0004] The invention provides a wear-resistant cleaning paper tape. The wear-resistant cleaning paper tape does not contain volatile substances, has good cleaning and environmental protection properties, and has good bonding force and lasting adhesiveness.

[0005] The present invention solves the technical problem by adopting the following technical solutions:

[0006] A wear-resistant cleaning paper tape comprises, from bottom to top, a first adhesive layer, a kraft paper layer, a second adhesive layer, and a wear-resistant layer. The first adhesive layer is formed by coating an adhesive below the kraft paper layer, the second adhesive layer is formed by coating an adhesive above the kraft paper layer, and the second adhesive layer is used to connect the kraft paper layer and the wear-resistant layer.

[0007] As a preferred solution, the wear-resistant layer is glass fiber cloth.

[0008] The wear-resistant layer material is glass fiber cloth, which can significantly improve the wear-resistant effect, so that the paper tape has good wear-resistant effect.

[0009] As a preferred embodiment, the adhesive is prepared from the following raw materials in parts by weight: 45 to 60 parts of water glass, 10 to 16 parts of phosphate, 6 to 12 parts of modified starch, 3 to 7 parts of modified calcium sulfate whiskers, 1 to 5 parts of fly ash, 1 to 2.5 parts of boric acid, 1.5 to 2.5 parts of D-sorbitol, 0.6 to 1.5 parts of ferrosoferric oxide, 0.5 to 1 part of kaolin, 0.4 to 0.8 parts of silane coupling agent KH550, 0.2 to 0.8 parts of fumed silica, and 0.1 to 0.4 parts of methyl hydroxypropyl cellulose.

[0010] The inventors of the present invention have found through extensive research that an adhesive having good bonding strength and long-lasting adhesion is prepared by taking the above-mentioned adhesive with water glass and phosphate as the base materials, using ferrosinone and kaolin as the curing agent, adding fumed silica as the thixotropic agent, and combining with silane coupling agent KH550, fly ash, boric acid, D-sorbitol, methyl hydroxypropyl cellulose, and adding modified starch and modified calcium sulfate whiskers for reinforcement and viscosity enhancement.

[0011] Furthermore, the adhesive does not contain volatile substances and has good cleaning and environmental protection properties.

[0012] As a preferred embodiment, the adhesive is prepared from the following raw materials in parts by weight: 50 to 60 parts of water glass, 12 to 16 parts of phosphate, 8 to 12 parts of modified starch, 4 to 7 parts of modified calcium sulfate whiskers, 2 to 5 parts of fly ash, 1.5 to 2.5 parts of boric acid, 1.6 to 2.5 parts of D-sorbitol, 0.8 to 1.5 parts of ferrosoferric oxide, 0.6 to 1 part of kaolin, 0.5 to 0.8 parts of silane coupling agent KH550, 0.2 to 0.6 parts of fumed silica, and 0.1 to 0.3 parts of methyl hydroxypropyl cellulose.

[0013] As a preferred embodiment, the adhesive is prepared from the following raw materials in parts by weight: 58 parts of water glass, 15 parts of phosphate, 10 parts of modified starch, 6 parts of modified calcium sulfate whiskers, 4 parts of fly ash, 2 parts of boric acid, 1.9 parts of D-sorbitol, 1 part of ferrosoferric oxide, 0.8 parts of kaolin, 0.6 parts of silane coupling agent KH550, 0.5 parts of fumed silica, and 0.2 parts of methyl hydroxypropyl cellulose.

[0014] As a preferred embodiment, the phosphate is aluminum dihydrogen phosphate.

[0015] As a preferred embodiment, the preparation method of the modified starch is:

[0016] S1, adding 10 to 20 parts by weight of corn starch and 10 to 20 parts by weight of potato starch to 60 to 90 parts by weight of deionized water, and dispersing them evenly to obtain a starch mixture;

[0017] S2, adding 1 to 4 parts by weight of 3,4-dihydroxybenzoic acid, 2 to 6 parts by weight of sodium hexametaphosphate, 5 to 10 parts by weight of sodium lauryl sulfate, and 6 to 12 parts by weight of urea to 50 to 90 parts by weight of deionized water, stirring at 70 to 90° C. and 200 to 600 rpm for 20 to 60 min to obtain a modified solution;

[0018] S3, dropping 10 to 20 parts by weight of the modified liquid into 20 to 50 parts by weight of the starch mixture, stirring at a speed of 200 to 1000 rpm for 60 to 150 min, filtering, and drying to obtain modified starch.

[0019] The invention modifies starch with a modifier prepared from 3,4-dihydroxybenzoic acid, sodium hexametaphosphate, sodium dodecyl sulfate and urea, and adds the modified starch into an adhesive with water glass and phosphate as base materials, thereby significantly improving the bonding force and the stickiness.

[0020] Moreover, the modified starch prepared by different modified starch preparation methods has different effects on adhesion and sustained viscosity. The modified starch prepared by the modified starch preparation method of the present invention can significantly improve adhesion and sustained viscosity compared with modified starch prepared by other methods.

[0021] As a preferred embodiment, the preparation method of the modified calcium sulfate whisker is:

[0022] S11, adding 6 to 15 parts by weight of calcium sulfate whiskers and 2 to 5 parts by weight of citric acid to 30 to 60 parts by weight of anhydrous ethanol, dispersing them evenly, adding 0.5 to 2 parts by weight of stearic acid, heating to 65 to 80° C., stirring at a speed of 100 to 400 rpm for 10 to 30 minutes, and obtaining a mixed solution;

[0023] S12, adding 4 to 10 parts by weight of heptadecafluorodecyltriethoxysilane and 4 to 10 parts by weight of tridecafluorooctyltriethoxysilane to 50 to 80 parts by weight of deionized water, mixing well, and preparing a modified liquid;

[0024] S13, dropping 5 to 12 parts by weight of the modified liquid into 15 to 25 parts by weight of the mixed liquid, and then adding 0.5 to 2 parts by weight of glycerol, dispersing evenly, ultrasonically treating in a water bath at 65 to 80° C., filtering, and drying to obtain modified calcium sulfate whiskers.

[0025] As described in patent CN101608104A, the T-peel strength of the anionic polymerized SBS block copolymer adhesive modified by inorganic whiskers is 41.51% higher than that of the anionic polymerized SBS block copolymer adhesive not modified by inorganic whiskers. The adhesive strength is significantly improved after modification, the modification process is simple, the cost is low, and the application prospect is very broad.

[0026] However, due to the large specific surface area, strong surface polarity and different interface properties with the matrix, if inorganic whiskers are directly added to the matrix, problems such as uneven agglomeration and dispersion, low bonding strength with the matrix and poor compatibility will occur, which will ultimately affect the performance. Therefore, they need to be modified.

[0027] The inventors of the present invention have found through extensive research that by pre-treating calcium sulfate whiskers with citric acid and stearic acid and then modifying them with fluorinated silanes (heptadecafluorodecyltriethoxysilane and tridecafluorooctyltriethoxysilane), they can be evenly dispersed in the adhesive system without agglomeration, which can significantly improve the bonding strength and adhesion retention.

[0028] The inventors found that modifying calcium sulfate whiskers with fluorine-containing silanes (heptadecafluorodecyltriethoxysilane, tridecafluorooctyltriethoxysilane) can significantly improve adhesion and persistence. If other coupling agents are used to replace the fluorine-containing silanes, the adhesion and persistence will be significantly reduced.

[0029] As a preferred embodiment, the ultrasonic treatment power is 200-800W, and the ultrasonic treatment time is 25-40min.

[0030] As a preferred embodiment, the preparation method of the adhesive is:

[0031] S21, adding water glass, phosphate, modified starch, modified calcium sulfate whisker, fly ash, boric acid, D-sorbitol, fumed silica, and methyl hydroxypropyl cellulose into a reaction kettle, and stirring at 60-80° C. and 400-1200 rpm for 2-6 hours;

[0032] S22, adding ferrosoferric oxide, kaolin, and silane coupling agent KH550, stirring at a speed of 400 to 1200 rpm for 40 to 100 min, discharging the material, and obtaining an adhesive.

[0033] Beneficial effects of the present invention: the wear-resistant cleaning paper tape described in the present invention does not contain volatile substances, has good cleaning and environmental protection, and has good bonding strength and persistent adhesion. The wear-resistant layer material is glass fiber cloth, which can significantly improve the wear resistance, so that the paper tape has good wear resistance. An adhesive with water glass and phosphate as the base material is adopted, ferrous oxide and kaolin are used as curing agents, and fumed silica is added as a thixotropic agent. Silane coupling agent KH550, fly ash, boric acid, D-sorbitol, methyl hydroxypropyl cellulose are matched, and modified starch and modified calcium sulfate whiskers are added for reinforcement and viscosity enhancement to prepare an adhesive with good bonding strength and persistent adhesion. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1It is a schematic diagram of the structure of the present invention;

[0035] Markings in the figure: 1. first adhesive layer; 2. kraft paper layer; 3. second adhesive layer; 4. wear-resistant layer. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] In the present invention, all parts are parts by weight.

[0038] Example 1

[0039] A wear-resistant cleaning paper tape comprises, from bottom to top, a first adhesive layer 1, a kraft paper layer 2, a second adhesive layer 3, and a wear-resistant layer 4, wherein the first adhesive layer 1 is formed by coating an adhesive below the kraft paper layer 2, the second adhesive layer 3 is formed by coating an adhesive above the kraft paper layer 2, and the second adhesive layer 3 is used to connect the kraft paper layer 2 and the wear-resistant layer 4.

[0040] The thickness of the first adhesive layer 1 and the second adhesive layer 3 are both 40 μm, the thickness of the wear-resistant layer 4 is 50 μm, and the thickness of the kraft paper layer 2 is 0.12 mm.

[0041] The wear-resistant layer 4 is glass fiber cloth.

[0042] The adhesive is prepared from the following raw materials in parts by weight: 58 parts of water glass, 15 parts of aluminum dihydrogen phosphate, 10 parts of modified starch, 6 parts of modified calcium sulfate whiskers, 4 parts of fly ash, 2 parts of boric acid, 1.9 parts of D-sorbitol, 1 part of ferrosoferric oxide, 0.8 parts of kaolin, 0.6 parts of silane coupling agent KH550, 0.5 parts of fumed silica, and 0.2 parts of methyl hydroxypropyl cellulose.

[0043] The above-mentioned adhesive with water glass and phosphate as the base materials is adopted, ferroferric oxide and kaolin are used as curing agents, fumed silica is added as a thixotropic agent, and silane coupling agent KH550, fly ash, boric acid, D-sorbitol, methyl hydroxypropyl cellulose are matched, and modified starch and modified calcium sulfate whiskers are added for reinforcement and viscosity enhancement to prepare an adhesive with good bonding strength and sustained viscosity.

[0044] Furthermore, the adhesive does not contain volatile substances and has good cleaning and environmental protection properties.

[0045] The preparation method of the modified starch is:

[0046] S1, adding 15 parts by weight of corn starch and 12 parts by weight of potato starch to 73 parts by weight of deionized water, and dispersing them evenly to obtain a starch mixture;

[0047] S2, adding 3 parts by weight of 3,4-dihydroxybenzoic acid, 5 parts by weight of sodium hexametaphosphate, 8 parts by weight of sodium lauryl sulfate, and 10 parts by weight of urea to 74 parts by weight of deionized water, stirring at 80° C. and 400 rpm for 50 min to obtain a modified solution;

[0048] S3, dropping 15 parts by weight of the modified liquid into 30 parts by weight of the starch mixture, stirring at 800 rpm for 100 min, filtering, and drying to obtain modified starch.

[0049] The starch is modified with a modifier prepared from 3,4-dihydroxybenzoic acid, sodium hexametaphosphate, sodium dodecyl sulfate and urea, and then added into an adhesive based on water glass and phosphate, thereby significantly improving the bonding strength and the stickiness.

[0050] The preparation method of the modified calcium sulfate whisker is:

[0051] S11, adding 10 parts by weight of calcium sulfate whiskers and 4 parts by weight of citric acid to 35 parts by weight of anhydrous ethanol, dispersing them evenly, adding 1 part by weight of stearic acid, heating to 70° C., stirring at 300 rpm for 20 min, to obtain a mixed solution;

[0052] S12, adding 8 parts by weight of heptadecafluorodecyltriethoxysilane and 6 parts by weight of tridecafluorooctyltriethoxysilane to 66 parts by weight of deionized water, mixing well, and preparing a modified liquid;

[0053] S13, dropping 8 parts by weight of the modified liquid into 20 parts by weight of the mixed liquid, and then adding 1 part by weight of glycerol, dispersing evenly, ultrasonically treating at 500W for 30 minutes in a 70°C water bath, filtering, and drying to obtain modified calcium sulfate whiskers.

[0054] The calcium sulfate whiskers are pretreated with citric acid and stearic acid and then modified with fluorine-containing silane (heptadecafluorodecyltriethoxysilane and tridecafluorooctyltriethoxysilane) so that they can be evenly dispersed in the adhesive system without agglomeration, thereby significantly improving the bonding strength and the stickiness.

[0055] The preparation method of the adhesive is:

[0056] S21, adding water glass, phosphate, modified starch, modified calcium sulfate whisker, fly ash, boric acid, D-sorbitol, fumed silica, and methyl hydroxypropyl cellulose into a reaction kettle, and stirring at 70° C. and 600 rpm for 4 h;

[0057] S22, adding ferrosoferric oxide, kaolin, and silane coupling agent KH550, stirring at a speed of 800 rpm for 60 min, discharging the material, and obtaining an adhesive.

[0058] Example 2

[0059] A wear-resistant cleaning paper tape comprises, from bottom to top, a first adhesive layer 1, a kraft paper layer 2, a second adhesive layer 3, and a wear-resistant layer 4, wherein the first adhesive layer 1 is formed by coating an adhesive below the kraft paper layer 2, the second adhesive layer 3 is formed by coating an adhesive above the kraft paper layer 2, and the second adhesive layer 3 is used to connect the kraft paper layer 2 and the wear-resistant layer 4.

[0060] The thickness of the first adhesive layer 1 and the second adhesive layer 3 are both 40 μm, the thickness of the wear-resistant layer 4 is 50 μm, and the thickness of the kraft paper layer 2 is 0.12 mm.

[0061] The wear-resistant layer 4 is glass fiber cloth.

[0062] The adhesive is prepared from the following raw materials in parts by weight: 58 parts of water glass, 16 parts of aluminum dihydrogen phosphate, 10 parts of modified starch, 4 parts of modified calcium sulfate whiskers, 5 parts of fly ash, 1.5 parts of boric acid, 2.5 parts of D-sorbitol, 0.8 parts of ferrosoferric oxide, 1 part of kaolin, 0.5 parts of silane coupling agent KH550, 0.6 parts of fumed silica, and 0.1 parts of methyl hydroxypropyl cellulose.

[0063] The preparation method of the modified starch is:

[0064] S1, adding 10 parts by weight of corn starch and 20 parts by weight of potato starch to 70 parts by weight of deionized water, dispersing them evenly to obtain a starch mixture;

[0065] S2, adding 2 parts by weight of 3,4-dihydroxybenzoic acid, 6 parts by weight of sodium hexametaphosphate, 8 parts by weight of sodium lauryl sulfate, and 12 parts by weight of urea to 72 parts by weight of deionized water, stirring at 80° C. and 300 rpm for 60 min to obtain a modified solution;

[0066] S3, dropping 15 parts by weight of the modified liquid into 40 parts by weight of the starch mixture, stirring at 800 rpm for 100 min, filtering, and drying to obtain modified starch.

[0067] The preparation method of the modified calcium sulfate whisker is:

[0068] S11, adding 12 parts by weight of calcium sulfate whiskers and 3 parts by weight of citric acid to 34 parts by weight of anhydrous ethanol, dispersing them evenly, adding 1 part by weight of stearic acid, heating to 70° C., stirring at 300 rpm for 20 min, to obtain a mixed solution;

[0069] S12, adding 6 parts by weight of heptadecafluorodecyltriethoxysilane and 8 parts by weight of tridecafluorooctyltriethoxysilane to 66 parts by weight of deionized water, mixing well, and preparing a modified liquid;

[0070] S13, dropping 10 parts by weight of the modified liquid into 20 parts by weight of the mixed liquid, then adding 1 part by weight of glycerol, dispersing evenly, ultrasonically treating at 500W for 30 minutes in a 70°C water bath, filtering, and drying to obtain modified calcium sulfate whiskers.

[0071] The preparation method of the adhesive is:

[0072] S21, adding water glass, phosphate, modified starch, modified calcium sulfate whisker, fly ash, boric acid, D-sorbitol, fumed silica, and methyl hydroxypropyl cellulose into a reaction kettle, and stirring at 70° C. and 600 rpm for 4 h;

[0073] S22, adding ferrosoferric oxide, kaolin, and silane coupling agent KH550, stirring at a speed of 800 rpm for 60 min, discharging the material, and obtaining an adhesive.

[0074] Example 3

[0075] A wear-resistant cleaning paper tape comprises, from bottom to top, a first adhesive layer 1, a kraft paper layer 2, a second adhesive layer 3, and a wear-resistant layer 4, wherein the first adhesive layer 1 is formed by coating an adhesive below the kraft paper layer 2, the second adhesive layer 3 is formed by coating an adhesive above the kraft paper layer 2, and the second adhesive layer 3 is used to connect the kraft paper layer 2 and the wear-resistant layer 4.

[0076] The thickness of the first adhesive layer 1 and the second adhesive layer 3 are both 40 μm, the thickness of the wear-resistant layer 4 is 50 μm, and the thickness of the kraft paper layer 2 is 0.12 mm.

[0077] The wear-resistant layer 4 is glass fiber cloth.

[0078] The adhesive is prepared from the following raw materials in parts by weight: 59.6 parts of water glass, 16 parts of aluminum dihydrogen phosphate, 6 parts of modified starch, 7 parts of modified calcium sulfate whiskers, 4 parts of fly ash, 2.5 parts of boric acid, 1.5 parts of D-sorbitol, 1.5 parts of ferrosoferric oxide, 0.5 parts of kaolin, 0.8 parts of silane coupling agent KH550, 0.2 parts of fumed silica, and 0.4 parts of methyl hydroxypropyl cellulose.

[0079] The preparation method of the modified starch is:

[0080] S1, adding 20 parts by weight of corn starch and 10 parts by weight of potato starch to 70 parts by weight of deionized water, and dispersing them evenly to obtain a starch mixture;

[0081] S2, adding 1 part by weight of 3,4-dihydroxybenzoic acid, 6 parts by weight of sodium hexametaphosphate, 5 parts by weight of sodium lauryl sulfate, and 10 parts by weight of urea to 78 parts by weight of deionized water, stirring at 80° C. and 500 rpm for 40 min to obtain a modified solution;

[0082] S3, dropping 12 parts by weight of the modified liquid into 30 parts by weight of the starch mixture, stirring at 600 rpm for 150 min, filtering, and drying to obtain modified starch.

[0083] The preparation method of the modified calcium sulfate whisker is:

[0084] S11, adding 10 parts by weight of calcium sulfate whiskers and 2 parts by weight of citric acid to 60 parts by weight of anhydrous ethanol, dispersing them evenly, adding 0.5 parts by weight of stearic acid, heating to 65° C., stirring at 400 rpm for 10 min, and obtaining a mixed solution;

[0085] S12, adding 10 parts by weight of heptadecafluorodecyltriethoxysilane and 4 parts by weight of tridecafluorooctyltriethoxysilane to 50 parts by weight of deionized water, mixing well, and preparing a modified liquid;

[0086] S13, drop 5 parts by weight of the modified liquid into 15 parts by weight of the mixed liquid, then add 0.5 parts by weight of glycerol, disperse evenly, treat with ultrasound at 500W for 30 minutes in a 65°C water bath, filter, and dry to obtain modified calcium sulfate whiskers.

[0087] The preparation method of the adhesive is:

[0088] S21, adding water glass, phosphate, modified starch, modified calcium sulfate whisker, fly ash, boric acid, D-sorbitol, fumed silica, and methyl hydroxypropyl cellulose into a reaction kettle, and stirring at 70° C. and 600 rpm for 4 h;

[0089] S22, adding ferrosoferric oxide, kaolin, and silane coupling agent KH550, stirring at a speed of 800 rpm for 60 min, discharging the material, and obtaining an adhesive.

[0090] Comparative Example 1

[0091] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 does not contain the modified starch, and the other aspects are the same.

[0092] Comparative Example 2

[0093] The difference between Comparative Example 2 and Example 1 is that Comparative Example 2 uses starch to replace modified starch, and the other parts are the same.

[0094] The starch in Comparative Example 2 is composed of corn starch and potato starch in a weight ratio of 5:4.

[0095] Comparative Example 3

[0096] The difference between Comparative Example 3 and Example 1 is that the preparation method of the modified starch described in Comparative Example 3 is different from that in Example 1, and the others are the same.

[0097] In this comparative example, the starch was oxidized and modified by potassium permanganate.

[0098] The preparation method of the modified starch is:

[0099] S1, adding 15 parts by weight of corn starch and 12 parts by weight of potato starch to 73 parts by weight of deionized water, and dispersing them evenly to obtain a starch mixture;

[0100] S2, adding 10 parts by weight of potassium permanganate to 90 parts by weight of deionized water, stirring at 80° C. and 400 rpm for 50 min to obtain a modified solution;

[0101] S3, dropping 15 parts by weight of the modified liquid into 30 parts by weight of the starch mixture, stirring at 800 rpm for 100 min, filtering, and drying to obtain modified starch.

[0102] Comparative Example 4

[0103] The difference between Comparative Example 4 and Example 1 is that Comparative Example 4 does not contain the modified calcium sulfate whiskers, and the other aspects are the same.

[0104] Comparative Example 5

[0105] The difference between Comparative Example 5 and Example 1 is that Comparative Example 5 uses calcium sulfate whiskers to replace the modified calcium sulfate whiskers, and the other contents are the same.

[0106] Comparative Example 6

[0107] The difference between Comparative Example 6 and Example 1 is that the preparation method of the modified calcium sulfate whisker described in Comparative Example 6 is different from that in Example 1, and the others are the same.

[0108] In this comparative example, an equal amount of silane coupling agent KH570 is used to replace the heptadecafluorodecyltriethoxysilane and tridecafluorooctyltriethoxysilane.

[0109] The preparation method of the modified calcium sulfate whisker is:

[0110] S11, adding 10 parts by weight of calcium sulfate whiskers and 4 parts by weight of citric acid to 35 parts by weight of anhydrous ethanol, dispersing them evenly, adding 1 part by weight of stearic acid, heating to 70° C., stirring at 300 rpm for 20 min, to obtain a mixed solution;

[0111] S12, adding 14 parts by weight of silane coupling agent KH570 to 66 parts by weight of deionized water, mixing well, and preparing a modified liquid;

[0112] S13, drop 8 parts by weight of the modified liquid into 20 parts by weight of the mixed liquid, add 1 part by weight of glycerol, disperse evenly, treat with ultrasound at 500W for 30 minutes in a 70°C water bath, filter, and dry to obtain modified calcium sulfate whiskers

[0113] The adhesive tapes prepared in the above embodiments were tested, wherein the adhesiveness was tested using GB4851-1998 and the peeling force was tested using a computer servo tensile machine.

[0114] The test results are shown in Table 1.

[0115] Table 1 Test results

[0116]

[0117]

[0118] It can be seen from Table 1 that the paper tape of the present invention has good adhesion and long-lasting adhesion.

[0119] Comparative Examples 1 to 3 show that the ratio of different adhesives and the preparation parameters of modified calcium sulfate whiskers and modified starch can affect the bonding force and the lasting adhesion.

[0120] By comparing Example 1 with Comparative Examples 1 to 3, it can be seen that the modified starch described in the present invention can significantly improve the adhesion and sustained adhesion, and the modified starch prepared by different modified starch preparation methods has different effects on the adhesion and sustained adhesion. The modified starch prepared by the modified starch preparation method described in the present invention can more significantly improve the adhesion and sustained adhesion than the modified starch prepared by other methods.

[0121] By comparing Example 1 with Comparative Examples 4 to 6, it can be seen that the modified calcium sulfate whisker of the present invention can significantly improve the bonding force and the persistent adhesion. In the preparation method of the modified calcium sulfate whisker, the modification of the calcium sulfate whisker by the fluorine-containing silane (heptadecafluorodecyltriethoxysilane, tridecafluorooctyltriethoxysilane) can significantly improve the bonding force and the persistent adhesion. If other coupling agents are used to replace the fluorine-containing silane, the bonding force and the persistent adhesion will be significantly reduced.

[0122] With the above-mentioned ideal embodiments of the present invention as inspiration, through the above-mentioned description, relevant personnel can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A wear-resistant cleaning paper tape, characterized in that: From bottom to top, it includes a first adhesive layer, a kraft paper layer, a second adhesive layer, and a wear-resistant layer, wherein the first adhesive layer is formed by coating an adhesive below the kraft paper layer, and the second adhesive layer is formed by coating an adhesive above the kraft paper layer, and the second adhesive layer is used to connect the kraft paper layer and the wear-resistant layer; The adhesive is prepared from the following raw materials in parts by weight: 45-60 parts of water glass, 10-16 parts of phosphate, 6-12 parts of modified starch, 3-7 parts of modified calcium sulfate whiskers, 1-5 parts of fly ash, 1-2.5 parts of boric acid, 1.5-2.5 parts of D-sorbitol, 0.6-1.5 parts of ferrosoferric oxide, 0.5-1 part of kaolin, 0.4-0.8 parts of silane coupling agent KH550, 0.2-0.8 parts of fumed silica, and 0.1-0.4 parts of methyl hydroxypropyl cellulose; The preparation method of the modified starch is: S1, adding 10 to 20 parts by weight of corn starch and 10 to 20 parts by weight of potato starch to 60 to 90 parts by weight of deionized water, and dispersing them evenly to obtain a starch mixture; S2, adding 1 to 4 parts by weight of 3,4-dihydroxybenzoic acid, 2 to 6 parts by weight of sodium hexametaphosphate, 5 to 10 parts by weight of sodium lauryl sulfate, and 6 to 12 parts by weight of urea to 50 to 90 parts by weight of deionized water, stirring at 70 to 90° C. and 200 to 600 rpm for 20 to 60 min to obtain a modified solution; S3, dropping 10 to 20 parts by weight of the modified liquid into 20 to 50 parts by weight of the starch mixture, stirring at a speed of 200 to 1000 rpm for 60 to 150 min, filtering, and drying to obtain modified starch; The preparation method of the modified calcium sulfate whisker is: S11, adding 6 to 15 parts by weight of calcium sulfate whiskers and 2 to 5 parts by weight of citric acid to 30 to 60 parts by weight of anhydrous ethanol, dispersing them evenly, adding 0.5 to 2 parts by weight of stearic acid, heating to 65 to 80° C., stirring at a speed of 100 to 400 rpm for 10 to 30 minutes, and obtaining a mixed solution; S12, adding 4 to 10 parts by weight of heptadecafluorodecyltriethoxysilane and 4 to 10 parts by weight of tridecafluorooctyltriethoxysilane to 50 to 80 parts by weight of deionized water, mixing well, and preparing a modified liquid; S13, dropping 5 to 12 parts by weight of the modified liquid into 15 to 25 parts by weight of the mixed liquid, and then adding 0.5 to 2 parts by weight of glycerol, dispersing evenly, ultrasonically treating in a water bath at 65 to 80° C., filtering, and drying to obtain modified calcium sulfate whiskers.

2. The wear-resistant cleaning paper tape according to claim 1, characterized in that: The wear-resistant layer is glass fiber cloth.

3. The wear-resistant cleaning paper tape according to claim 1, characterized in that: The adhesive is prepared from the following raw materials in parts by weight: 50-60 parts of water glass, 12-16 parts of phosphate, 8-12 parts of modified starch, 4-7 parts of modified calcium sulfate whiskers, 2-5 parts of fly ash, 1.5-2.5 parts of boric acid, 1.6-2.5 parts of D-sorbitol, 0.8-1.5 parts of ferrosoferric oxide, 0.6-1 part of kaolin, 0.5-0.8 parts of silane coupling agent KH550, 0.2-0.6 parts of fumed silica, and 0.1-0.3 parts of methyl hydroxypropyl cellulose.

4. The wear-resistant cleaning paper tape according to claim 1, characterized in that: The adhesive is prepared from the following raw materials in parts by weight: 58 parts of water glass, 15 parts of phosphate, 10 parts of modified starch, 6 parts of modified calcium sulfate whiskers, 4 parts of fly ash, 2 parts of boric acid, 1.9 parts of D-sorbitol, 1 part of ferrosoferric oxide, 0.8 parts of kaolin, 0.6 parts of silane coupling agent KH550, 0.5 parts of fumed silica, and 0.2 parts of methyl hydroxypropyl cellulose.

5. The wear-resistant cleaning paper tape according to claim 3, characterized in that: The phosphate is aluminum dihydrogen phosphate.

6. The wear-resistant cleaning paper tape according to claim 1, characterized in that: The ultrasonic treatment power is 200-800W, and the ultrasonic treatment time is 25-40min.

7. The wear-resistant cleaning paper tape according to any one of claims 1 to 6, characterized in that: The preparation method of the adhesive is: S21, adding water glass, phosphate, modified starch, modified calcium sulfate whisker, fly ash, boric acid, D-sorbitol, fumed silica, and methyl hydroxypropyl cellulose into a reaction kettle, and stirring at 60-80° C. and 400-1200 rpm for 2-6 hours; S22, adding ferrosoferric oxide, kaolin, and silane coupling agent KH550, stirring at a speed of 400 to 1200 rpm for 40 to 100 min, discharging the material, and obtaining an adhesive.