Method for producing molybdenum concentrate from molybdenum-bismuth sulfide ore
By performing acid leaching and flotation processes in molybdenum bismuth sulfide ore, the problems of molybdenum bismuth mutual content and reagent dosage in molybdenum bismuth separation process were successfully solved, achieving efficient molybdenum bismuth separation and high recovery rate of molybdenum concentrate.
Patent Information
- Application Number
- CN202211022835.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-25
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-08-25
AI Technical Summary
The existing molybdenum bismuth sulfide separation process has problems such as high molybdenum bismuth mutual content, large reagent usage, and high cost, making it difficult to effectively separate molybdenum and bismuth.
The molybdenum bismuth sulfide ore is first acid leaching, and then molybdenum is separated through the flotation process, kerosene is used as a collector and terpineol is used as a foaming agent to adjust the pH and temperature of the ore slurry to achieve effective flotation of molybdenum.
Effective separation of molybdenum bismuth was achieved, and the molybdenum content in the obtained molybdenum concentrate was >46 wt%, and the molybdenum recovery rate reached more than 98.5%, reducing the process cost.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nonferrous metal beneficiation, and more specifically, to a method for producing molybdenum concentrate from molybdenum-bismuth sulfide ore and the molybdenum concentrate obtained by the method. Background Art
[0002] my country is rich in molybdenum-bismuth sulfide resources, with a close symbiotic relationship between nitrogen, molybdenum and bismuth, and very similar flotation properties. Therefore, the separation of molybdenum and bismuth has become a major problem faced in the development and utilization of molybdenum-bismuth sulfide ores. In the early days, the mineral processing technology of "molybdenum-bismuth-sulfur full flotation-molybdenum-bismuth and sulfur separation-molybdenum-bismuth separation" was mostly used for processing, and gradually developed "molybdenum-bismuth equal flotation-molybdenum-bismuth separation" and "bismuth-sulfur equal flotation-bismuth-sulfur separation" and other processing methods, and the indicators of molybdenum-bismuth separation have been greatly improved. Even so, due to the constraints of the mineralization characteristics of molybdenum-bismuth sulfide ores and the physical separation methods of mineral processing, the current molybdenum-bismuth separation process has problems such as high mutual content of molybdenum and bismuth, large amount of reagents, and high cost. Some researchers carried out "molybdenum-bismuth co-floatation-molybdenum-bismuth separation" treatment on molybdenum-bismuth sulfide ore with Mo0.64% and Bi1.12%, and finally produced bismuth concentrate with Bi content of 21.12%, of which Mo content was 1.54%; at the same time, they produced molybdenum concentrate with Mo content of 20.12%, of which Bi content reached 4.47%, and the separation of molybdenum and bismuth was not complete. Summary of the invention
[0003] Based on the above technical problems existing in the prior art, the present invention provides a method for producing molybdenum concentrate from molybdenum-bismuth sulfide ore, which can effectively separate molybdenum and bismuth and obtain a molybdenum-containing concentrate with a molybdenum content greater than 46wt%, and the recovery rate of molybdenum in the molybdenum-bismuth sulfide ore is more than 98.5%.
[0004] In order to achieve the above object, the technical solution of the present invention is as follows:
[0005] The method for producing molybdenum concentrate from molybdenum-bismuth sulfide ore comprises the following steps:
[0006] S1. Grind the molybdenum-bismuth sulfide ore to 95%≤200 mesh, add acid and leaching aid, leach at 50-95°C, separate, and obtain leaching residue and leachate;
[0007] S2, adding water to the leached residue obtained in step S1 to prepare slurry, adjusting the slurry pH to 1-7, using kerosene as a collector and pinene alcohol as a frother to flotation molybdenum to obtain a molybdenum concentrate, wherein the molybdenum content in the molybdenum concentrate is greater than 46wt%.
[0008] In some embodiments, in step S1, the molybdenum content in the molybdenum-bismuth sulfide ore is 5-15 wt%.
[0009] In some embodiments, in step S1, the acid is sulfuric acid with a concentration of 4 to 10 mol / L.
[0010] In some embodiments, in step S1, the soaking aid is a sodium chloride solution with a concentration of 0.5 to 5 mol / L.
[0011] In some embodiments, in step S1, during leaching, the liquid-to-solid ratio is 2 to 10 L: 1 kg.
[0012] In some embodiments, the leaching efficiency can be accelerated by stirring the leaching, and the leaching time is 2 to 10 hours.
[0013] In some embodiments, the total amount of kerosene is 160-200 g / t, and the amount of terpineol is 50-80 g / t.
[0014] In some embodiments, the pulp temperature is controlled at 10-30° C. during flotation.
[0015] The present invention also provides a molybdenum concentrate, which is obtained by the method of any of the above embodiments, and the molybdenum content in the molybdenum concentrate is greater than 46wt% and the bismuth content is less than 1wt%.
[0016] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0017] The present invention strictly follows the steps of acid leaching the molybdenum-bismuth sulfide ore and then flotation to realize the production of molybdenum concentrate from the molybdenum-bismuth sulfide ore, not only realizing the separation of molybdenum and bismuth, but also making the molybdenum content in the obtained molybdenum concentrate greater than 46wt%, and the recovery rate of molybdenum in the molybdenum-bismuth sulfide ore is as high as more than 98.5%. Among them, in this method, the molybdenum-bismuth sulfide ore is first acid-leached under specific conditions, which can effectively leach the bismuth element, and realize the separation of molybdenum and bismuth by solid-liquid separation; then, kerosene is used as a collector and pine alcohol is used as a frother to flotation molybdenum, so as to improve the grade of the molybdenum ore, so that the molybdenum content in the obtained molybdenum concentrate is greater than 46wt%, and the recovery rate of molybdenum in the molybdenum-bismuth sulfide ore is ≥98.5%.
[0018] The method of the present invention can not only effectively separate molybdenum and bismuth in molybdenum-bismuth sulfide ore, but also has a high recovery rate for molybdenum, and is suitable for industrialization. DETAILED DESCRIPTION
[0019] Many specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar modifications without violating the connotation of the present invention, so the present invention is not limited to the specific implementation disclosed below.
[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0021] The molybdenum-bismuth sulfide ore raw material used in all the following embodiments is a molybdenum-bismuth sulfide ore mined from a certain mine. After testing, its elemental composition is shown in Table 1 below:
[0022] Table 1 Main metal element contents of molybdenum-bismuth sulfide ore
[0023] Components Bi Mo Cu Fe Pb Ca S Content (wt%) 23.23 10.16 1.25 3.85 1.95 3.86 6.38
[0024] Example 1
[0025] The method for producing molybdenum concentrate from molybdenum-bismuth sulfide ore comprises the following steps:
[0026] S1. Grind the molybdenum-bismuth sulfide ore raw material to 95%≤200 mesh, add 4 mol / L sulfuric acid and 2 mol / L sodium chloride solution at a liquid-solid ratio of 5L:1kg, stir and leach at 60°C for 3h, separate the solid and liquid, and obtain leaching residue and leachate;
[0027] S2. Add water to the leached residue obtained in step S1 to make a pulp, adjust the pulp pH to 4, control the pulp temperature to 25°C, use kerosene as a collector and pinene alcohol as a frother to flotate molybdenum, and obtain molybdenum sulphite concentrate. After testing, the elemental composition of the obtained molybdenum sulphite concentrate is shown in Table 2 below; wherein the amount of kerosene is 160g / t and the amount of pinene alcohol is 55g / t.
[0028] Table 2 Main metal content of molybdenum concentrate
[0029] Components Mo S Cu Fe Bi Ca Content (wt%) 48.12 33.64 1.89 4.64 0.52 3.01
[0030] Example 2
[0031] The method for producing molybdenum concentrate from molybdenum-bismuth sulfide ore comprises the following steps:
[0032] S1. Grind the molybdenum-bismuth sulfide ore raw material to 95%≤200 mesh, add 6 mol / L sulfuric acid and 2 mol / L sodium chloride solution at a liquid-solid ratio of 5L:1kg, stir and leach at 60°C for 3h, separate the solid and liquid, and obtain leaching residue and leachate;
[0033] S2. Add water to the leached residue obtained in step S1 to make a pulp, adjust the pulp pH to 4, control the pulp temperature to 25°C, use kerosene as a collector and pinene alcohol as a frother to flotate molybdenum, and obtain molybdenum sulphite concentrate. After testing, the elemental composition of the obtained molybdenum sulphite concentrate is shown in Table 3 below; wherein the amount of kerosene is 180g / t and the amount of pinene alcohol is 70g / t.
[0034] Table 3 Main metal content of molybdenum concentrate
[0035] Components Mo S Cu Fe Bi Ca Content (wt%) 50.04 34.77 2.08 4.47 0.61 3.14
[0036] Example 3
[0037] The method for producing molybdenum concentrate from molybdenum-bismuth sulfide ore comprises the following steps:
[0038] S1. Grind the molybdenum-bismuth sulfide ore raw material to 95%≤200 mesh, add 4 mol / L sulfuric acid and 2 mol / L sodium chloride solution at a liquid-solid ratio of 5L:1kg, stir and leach at 60°C for 3h, separate the solid and liquid, and obtain leaching residue and leachate;
[0039] S2. Add water to the leached residue obtained in step S1 to make a pulp, adjust the pulp pH to 4, control the pulp temperature to 25°C, use kerosene as a collector and pinene alcohol as a frother to flotate molybdenum, and obtain molybdenum sulphite concentrate. After testing, the elemental composition of the obtained molybdenum sulphite concentrate is shown in Table 4 below; wherein the amount of kerosene is 200g / t and the amount of pinene alcohol is 80g / t.
[0040] Table 4 Main metal content of molybdenum concentrate
[0041] Components Mo S Cu Fe Bi Ca Content (wt%) 46.31 32.89 1.77 4.32 0.98 4.15
[0042] Example 4
[0043] The method for producing molybdenum concentrate from molybdenum-bismuth sulfide ore comprises the following steps:
[0044] S1. Grind the molybdenum-bismuth sulfide ore raw material to 95%≤200 mesh, add 4 mol / L sulfuric acid and 2 mol / L sodium chloride solution at a liquid-solid ratio of 5L:1kg, stir and leach at 80°C for 3h, separate the solid and liquid, and obtain leaching residue and leachate;
[0045] S2. Add water to the leached residue obtained in step S1 to make a pulp, adjust the pulp pH to 4, control the pulp temperature to 25°C, use kerosene as a collector and pinene alcohol as a frother to flotate molybdenum, and obtain molybdenum sulphite concentrate. After testing, the elemental composition of the obtained molybdenum sulphite concentrate is shown in Table 5 below; wherein the amount of kerosene is 180g / t and the amount of pinene alcohol is 70g / t.
[0046] Table 5 Main metal content of molybdenum concentrate
[0047] Components Mo S Cu Fe Bi Ca Content (wt%) 47.59 33.01 2.21 3.98 0.73 3.62
[0048] Example 5
[0049] The method for producing molybdenum concentrate from molybdenum-bismuth sulfide ore comprises the following steps:
[0050] S1. Grind the molybdenum-bismuth sulfide ore raw material to 95%≤200 mesh, add 4 mol / L sulfuric acid and 2 mol / L sodium chloride solution at a liquid-solid ratio of 5L:1kg, stir and leach at 50°C for 3h, separate the solid and liquid, and obtain leaching residue and leachate;
[0051] S2. Add water to the leached residue obtained in step S1 to make a pulp, adjust the pulp pH to 4, control the pulp temperature to 25°C, use kerosene as a collector and pinene alcohol as a frother to flotate molybdenum, and obtain molybdenum sulphite concentrate. After testing, the elemental composition of the obtained molybdenum sulphite concentrate is shown in Table 6 below; wherein the amount of kerosene is 180g / t and the amount of pinene alcohol is 70g / t.
[0052] Table 6 Main metal content of molybdenum concentrate
[0053] Components Mo S Cu Fe Bi Ca Content (wt%) 47.13 33.27 2.28 4.05 0.64 3.77
[0054] Example 6
[0055] The method for producing molybdenum concentrate from molybdenum-bismuth sulfide ore comprises the following steps:
[0056] S1. Grind the molybdenum-bismuth sulfide ore raw material to 95%≤200 mesh, add 4 mol / L sulfuric acid and 2 mol / L sodium chloride solution at a liquid-solid ratio of 5L:1kg, stir and leach at 100°C for 3h, separate the solid and liquid, and obtain leaching residue and leachate;
[0057] S2. Add water to the leached residue obtained in step S1 to make a pulp, adjust the pulp pH to 4, control the pulp temperature to 25°C, use kerosene as a collector and pinene alcohol as a frother to flotate molybdenum, and obtain molybdenum sulphite concentrate. After testing, the elemental composition of the obtained molybdenum sulphite concentrate is shown in Table 7 below; wherein the amount of kerosene is 180g / t and the amount of pinene alcohol is 70g / t.
[0058] Table 7 Main metal content of molybdenum concentrate
[0059] Components Mo S Cu Fe Bi Ca Content (wt%) 51.04 35.98 2.87 4.08 0.86 3.24
[0060] Example 7
[0061] The method for producing molybdenum concentrate from molybdenum-bismuth sulfide ore comprises the following steps:
[0062] S1. Grind the molybdenum-bismuth sulfide ore raw material to 95%≤200 mesh, add 4 mol / L sulfuric acid and 2 mol / L sodium chloride solution at a liquid-solid ratio of 5L:1kg, stir and leach at 60°C for 3h, separate the solid and liquid, and obtain leaching residue and leachate;
[0063] S2. Add water to the leached residue obtained in step S1 to make a pulp, adjust the pulp pH to 1, control the pulp temperature to 25°C, use kerosene as a collector and pinene alcohol as a frother to flotate molybdenum, and obtain molybdenum sulphite concentrate. After testing, the elemental composition of the obtained molybdenum sulphite concentrate is shown in Table 8 below; wherein, the amount of kerosene is 180g / t, and the amount of pinene alcohol is 70g / t.
[0064] Table 8 Main metal content of molybdenum concentrate
[0065] Components Mo S Cu Fe Bi Ca Content (wt%) 46.87 33.24 1.89 4.64 0.52 3.01
[0066] Example 8
[0067] The method for producing molybdenum concentrate from molybdenum-bismuth sulfide ore comprises the following steps:
[0068] S1. Grind the molybdenum-bismuth sulfide ore raw material to 95%≤200 mesh, add 4 mol / L sulfuric acid and 2 mol / L sodium chloride solution at a liquid-solid ratio of 5L:1kg, stir and leach at 60°C for 3h, separate the solid and liquid, and obtain leaching residue and leachate;
[0069] S2. Add water to the leached residue obtained in step S1 to make a pulp, adjust the pulp pH to 7, control the pulp temperature to 25°C, use kerosene as a collector and pinene alcohol as a frother to flotate molybdenum, and obtain molybdenum sulphite concentrate. After testing, the elemental composition of the obtained molybdenum sulphite concentrate is shown in Table 9 below; wherein, the amount of kerosene is 180g / t, and the amount of pinene alcohol is 70g / t.
[0070] Table 9 Main metal content of molybdenum concentrate
[0071] Components Mo S Cu Fe Bi Ca Content (wt%) 48.54 33.73 2.05 4.41 0.77 3.73
[0072] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0073] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for producing molybdenum concentrate from molybdenum-bismuth sulfide ore, characterized in that: The following steps are involved: S1. Grind the molybdenum-bismuth sulfide ore to 95%≤200 mesh, add acid and leaching aid, leach at 50-95°C, separate, and obtain leaching residue and leaching liquid; S2, adding water to the leached residue obtained in step S1 to prepare a pulp, adjusting the pulp pH to 1-7, using kerosene as a collector and pinene alcohol as a frother to flotate molybdenum to obtain a molybdenum concentrate, wherein the molybdenum content of the molybdenum concentrate is greater than 46wt% and the bismuth content is less than 1wt%; In step S1, the acid is sulfuric acid with a concentration of 4-10 mol / L; the leaching aid is sodium chloride solution with a concentration of 0.5-5 mol / L; during leaching, the liquid-to-solid ratio is 2-10 L:1 kg; In step S2, the pulp temperature is controlled to be 10-30°C during flotation.
2. The method for producing molybdenum concentrate from molybdenum-bismuth sulfide ore according to claim 1, characterized in that: In step S1, the molybdenum content in the molybdenum-bismuth sulfide ore is 5-15wt%.
3. The method for producing molybdenum concentrate from molybdenum-bismuth sulfide ore according to claim 1, characterized in that: The total amount of kerosene is 160-200 g / t, and the amount of terpineol is 50-80 g / t.