A method for preparing 2000MPa hot-formed steel without coating and oxidation

Through converter smelting, LF refining and double-roll casting and rolling, Fe-Cr-Al-Si-Ce protective film is formed, which solves the problems of surface oxidation and decarbonization of hot-formed steels, simplifies the process flow, reduces costs and energy consumption, and realizes the Efficient and environmentally friendly 2000MPa thermoformed steel production.

CN115365317BActive Publication Date: 2024-11-19JIUQUAN IRON & STEEL (GRP) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210982582.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-16
Publication Date
2024-11-19
Estimated Expiration
2042-08-16

AI Technical Summary

Technical Problem

In the existing thermal steel manufacturing process, the surface of bare sheets is prone to oxidation and decarbonization, resulting in reduced parts accuracy and short mold life. The traditional plating process is high in cost, high energy consumption and serious pollution, and lacks simplification, high efficiency and low Cost production method.

Method used

Through converter smelting, LF refining, double-roll casting, controlled rolling, controlled cooling and grinding processing, a dense Fe-Cr-Al-Si-Ce protective film is formed to avoid oxidation, decarbonization and cracking of steel sheets during the thermoforming process. Simplify the process flow and reduce production costs.

Benefits of technology

The production of high-strength thermoformed steel without coating is achieved, the process flow is simplified, energy consumption is reduced, zinc pollution is avoided, the product surface quality is good, the mechanical properties are in compliance with the standards, and it is directly suitable for painting, making the production more environmentally friendly.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the technical field of steel production and manufacturing, and more specifically discloses a method for preparing 2000MPa hot-formed steel that is free of coating and oxidation. The production process is as follows: after molten steel is smelted in a converter and refined in an LF furnace, it is injected into a crystallizer through a large ladle, a tundish, and a molten steel distributor in sequence, and a 0.8-2.0mm thin-gauge steel strip is directly produced by double-roll casting, controlled rolling, and controlled cooling. The oxide scale formed during hot rolling is used to remove the loose oxide scale structure on the surface of the hot-rolled plate by grinding, and a dense inner oxide film that is closely combined with the matrix is ​​retained. The good high-temperature performance is used to prevent the sheet from generating oxidation, peeling, and cracking defects during hot forming heating and quenching, and the parts can be directly painted without treatment. The new process saves the cold rolling and galvanizing processes, simplifies the production process, reduces the process energy consumption, and avoids the environmental pollution problem of zinc in galvanizing and later scrap steel recycling, providing an advanced production process for hot-formed steel manufacturing and processing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of steel manufacturing, and in particular to a method for preparing a coating-free and oxidation-resistant 2000MPa hot-formed steel. Background Art

[0002] Hot forming technology is a new technology that has emerged in recent years and is specifically used for forming ultra-high-strength steel stamping parts. Hot forming is a new process that divides forming and strengthening into two steps to produce ultra-high-strength automotive parts. Its advantages are ultra-high strength, precise forming, and avoiding the problem of cold forming rebound of high-strength steel. It is widely used in the production of safety parts such as door anti-collision beams, front and rear bumpers, and body structural parts such as A-pillars, B-pillars, C-pillars, and center channels. One of the key steps in the hot forming process is to heat the steel sheet to the austenite temperature and keep it warm, and then cool and quench it in the mold. During the processing, the surface of the bare sheet is prone to oxidation and decarburization, resulting in reduced component accuracy and mold life. Plating the bare sheet can effectively avoid defects such as surface oxidation and decarburization in the hot forming process, so that the workpiece has a certain degree of corrosion resistance after forming, prevent surface oxidation and decarburization during the forming process, and improve the corrosion resistance after painting. There are two types of coatings for hot-formed steel: Zn or Zn alloy coating and Al-Si coating. Galvanizing is the most mature and widely used coating technology. However, in the hot forming process, due to the high austenitizing heating temperature, the surface zinc will oxidize, and the coating is prone to cracking, which limits its practical application. Al-Si coating is mainly composed of metal compounds such as aluminum iron and aluminum silicon iron. The protective layer formed can prevent the diffusion of iron into the coating. Al-Si coating technology is widely used in hot forming steel. However, the Al-Si coating process is protected by foreign patents, and production requires a large amount of patent fees, resulting in increased production costs. At the same time, the traditional coating process has a long production process, high energy consumption, and high pollution. For this reason, there is an urgent need for a green and low-cost hot forming steel production method that is free of coating, short process, high efficiency and energy saving to overcome the shortcomings of the original technology. Summary of the invention

[0003] Based on the deficiencies in the prior art, the present invention provides a coating-free, oxidation-resistant 2000MPa hot-forming steel manufacturing method, which is characterized in that through converter smelting, LF refining, twin-roller casting and rolling, controlled rolling and controlled cooling, and grinding of the oxide scale on the surface of the steel, a dense protective film containing elements such as Fe-Cr-Al-Si-Ce is formed on the surface of the substrate by utilizing its own characteristics, thereby preventing the sheet from generating oxidation, decarburization, peeling and cracking defects during hot forming heating and quenching, simplifying the manufacturing process, saving energy and reducing consumption, reducing production costs, and realizing green production.

[0004] The present invention adopts the following technical solution:

[0005] A method for preparing 2000MPa hot-formed steel that is free of coating and oxidation, comprising the following process steps:

[0006] (1) Converter smelting: Bottom blowing of argon throughout the process, the final temperature is controlled at 1650-1690℃, the final molten steel contains C: 0.06%-0.13%, P ≤ 0.012%; slag blocking steel tapping, the slag volume is controlled to be ≤ 30mm; medium carbon ferromanganese, ferrosilicon, ferrochrome and ferroniobium are added during the steel tapping process for deoxidation and alloying.

[0007] (2) LF refining: white slag is made for incoming molten steel, desulfurization is carried out, and composition is adjusted; refining slag, active lime and aluminum balls are added to the ladle to make white slag for refining and desulfurization, the basicity of the ladle top slag is controlled at 4~7, the white slag retention time is ≥16min, the FeO+MnO content of the outgoing slag sample is ≤1.0%, and the outgoing S content is ≤0.012%; titanium wire, boron wire, calcium wire and cerium wire are fed in sequence in the later stage of refining to improve the composition of the molten steel; soft argon is blown for stirring during the wire feeding process, and the outgoing molten steel temperature is 1630~1645℃.

[0008] The main components of the refined slag are CaO: 50-55%, Al2O3: 30-35%, SiO2: 1-6%, MgO: 4-8%, and the amount of refined slag added is 4-5kg / ton of steel; the activity of the active lime is ≥350ml, the particle size is 5-50mm, and the main components are: CaO ≥92%, S ≤0.045%, K2O+Na2O <0.35%; the amount of active lime added is 1.6-2.5kg / ton of steel; the amount of aluminum shot added is 0.6-1.5kg / ton of steel.

[0009] The mass percentage of each component in the molten steel after LF refining treatment is: C: 0.24~0.32%, Si: 0.40~0.60%, Mn: 1.0~1.5%, S≤0.010%, P≤0.012%, Als: 0.025~0.045%, Cr: 0.25~0.55%, Ce: 0.020~0.060%, Ti: 0.025~0.040%, V: 0.020~0.050%, Nb: 0.020~0.040%, B: 0.0010~0.0030%.

[0010] (3) Intermediate transfer: The molten steel with qualified composition is hoisted to the ladle turret, and poured into the tundish after being cooled for 10 minutes. The superheat is controlled at 20~50℃ and the heat is kept.

[0011] (4) Twin-roll casting: Molten steel is injected into the twin-roll casting machine through an immersed nozzle, the roll gap is controlled between 1.5 and 4.5 mm, the solidification rate of the molten steel is controlled between 200 and 600 °C / s, the billet drawing speed is controlled between 60 and 120 m / min, and argon or nitrogen is used for protection during the casting process.

[0012] (5) Billet rolling: hot rolling is carried out under argon or nitrogen protection; micro-tension rolling is adopted, the rolling speed is 80~200m / min, the rolling temperature is 950~1200℃, the reduction is 50~80%, and the strip thickness after hot rolling is controlled at 0.8~2.0mm;

[0013] In the above steps (4) and (5), the pressure of the protective gas is 0.2-0.5 MPa, and the purity of the protective gas is 99.99%.

[0014] (6) Controlled cooling of steel strip: After rolling, the steel strip is promptly cooled by water curtain using laminar cooling method. The cooling water pressure is 0.3~1.0Mpa, the cooling rate of the steel strip is controlled to be 10~60℃ / min, and the final cooling temperature is 500~750℃. By controlling the rolling temperature and the final cooling temperature, the thickness of the iron oxide scale of the steel strip is between 15~30µm.

[0015] (7) Steel strip coiling: After the head and tail are cut off, the steel strip is sent to the coiler through the pinch roller for coiling to obtain the finished thin strip steel coil.

[0016] (8) Leveling treatment: Strong roller leveling to ensure the flatness of the steel strip surface and control the flatness of the plate surface ≤5I.

[0017] (9) Grinding treatment: In a closed grinding box, the gap between the grinding rollers is automatically adjusted according to the thickness of the steel strip. The steel strip is ground under slight tension and the easily detached iron oxide scale on the surface of the steel slab is washed off, leaving only the 5µm~10µm thick wustite oxide film that is tightly bonded to the bottom layer and the substrate. The steel strip is dried after leaving the grinding box. The diameter of the grinding roller is 350mm, the rotation speed is 120~600r / min, and the steel strip tension is 30~150KN.

[0018] (10) Hot forming treatment: According to the size of the automobile parts, the thin strip is processed into the corresponding size, and the sheet is heated to 820~930℃ by electromagnetic induction heating device, and kept at this temperature for 3~5 minutes for austenitization treatment, and then stamped and quenched in a mold with a cooling device to obtain ultra-high strength parts with good surface quality. The quenching coolant is hot water at 92~100℃ (containing ≤1% salt).

[0019] The present invention has the following beneficial effects:

[0020] 1. The thin strip casting and rolling process is used to directly produce ultra-high strength hot-formed steel. The high alloy content and the oxide scale formed by hot rolling are used. After grinding, the iron oxide scale on the surface of the hot-rolled steel plate is removed, and the film containing Fe-Cr-Al-Si-Ce elements that is closely combined with the bottom layer and the matrix is ​​retained. Its high temperature resistance is used to prevent the sheet from producing oxidation, decarburization, peeling and cracking defects during hot forming heating and quenching. The parts can be directly painted without treatment. It is a simple and efficient production process.

[0021] 2. The new process eliminates the cold rolling and galvanizing steps, simplifies the manufacturing process, greatly shortens the product production cycle, and reduces manufacturing costs.

[0022] 3. The new process simplifies the production process, significantly reduces production energy consumption, overcomes the environmental pollution problem of zinc in galvanizing and subsequent scrap steel recycling, and realizes green production. DETAILED DESCRIPTION

[0023] The present invention will be further explained below in conjunction with specific embodiments.

[0024] The production process of 1.5mm thick, coating-free, oxidation-resistant 2000MPa hot-formed steel is as follows:

[0025] Converter smelting: argon is blown from the bottom throughout the whole process, the final temperature is 1672℃, C in the final molten steel is 0.07%, P is 0.010%; slag blocking is used for tapping, and the slag volume under tapping is controlled to be 22mm. During the tapping process, medium carbon ferromanganese, ferrosilicon, ferrochrome and ferroniobium are added for deoxidation and alloying according to the requirements of the finished product composition.

[0026] LF furnace refining: add 4.5kg / ton steel of refining slag, 3.0kg / ton steel of active lime and 1.2kg / ton steel of aluminum shot into the ladle to make white slag desulfurization; slag basicity is 5-6, outgoing slag sample TFe+MnO≤1.0%, white slag retention time is 20min; after refining for 30 minutes, titanium wire, boron wire, calcium wire and cerium wire are fed in turn, the cerium wire feeding amount is 360m, the wire feeding speed is 3.2m / min, and the outgoing temperature is 1642℃.

[0027] The composition of molten steel after LF refining is: C: 0.30%, Si: 0.51%, Mn: 1.46%, S: 0.008%, P: 0.012%, Als: 0.032%, Cr: 0.45%, Ce: 0.046%, Ti: 0.027%, V: 0.045%, Nb: 0.021%, B: 0.0012%.

[0028] The qualified ones after treatment are transferred to the tundish. The superheat of the molten steel is 42℃. 5 to 8 bags of ladle covering agent are added to keep the molten steel warm to ensure that there is no exposed molten steel.

[0029] Twin-roll casting: Molten steel is injected into the twin-roll casting machine through an immersed nozzle. The preset roll gap of the casting rolls is 3.5mm. Argon is used for protection during the flow of molten steel, and the protective gas pressure is 0.40MPa. The cooling rate of the solidified molten steel in the casting rolls is 240℃ / s, and the billet casting speed is 65m / min. The thickness of the strip obtained after casting is 3.5mm.

[0030] Rolling: Hot rolling is carried out under argon protection, with a protective gas pressure of 0.4 MPa; the strip passes through the pinch rolls and is then rolled under constant tension, with a rolling speed of 120 m / min, a rolling temperature of 1050°C, a reduction rate of 57%, and a strip thickness of 1.5 mm after hot rolling.

[0031] Controlled cooling: After hot rolling, the strip at 950°C is cooled to 620°C by a laminar flow cooling device. The water pressure of the laminar flow device is 0.8MPa and the cooling rate of the steel strip is 24°C / min.

[0032] Coiling: After the head and tail of the steel strip are cut off, it is sent to the coiler through the pinch roller for coiling to obtain the hot-rolled finished thin strip steel coil.

[0033] Leveling treatment: Use strong roller to level the steel strip, the plate surface straightness is 4I.

[0034] Grinding treatment: The oxide scale on the surface of the hot-rolled plate is ground in the grinding box. The tension applied to the steel strip is 75 kN, the diameter of the grinding roller is 350 mm, the speed of the grinding roller is 550 rpm, and 3 pairs of grinding rollers are turned on; the ground iron oxide scale is washed away by circulating filtered water. After grinding, the thickness of the remaining oxide scale on the steel strip is 8 µm. The steel strip is dried after leaving the grinding box.

[0035] Hot forming treatment: The sheet is heated to 880℃ and kept warm for 3.5min. After being stamped in the mold, it is quickly placed in 95℃ hot water containing 0.5% salt for quenching.

[0036] Product surface quality and mechanical properties: After stamping, the surface of the parts is free of oxidation, peeling and cracking, and the surface quality is good; the mechanical properties are tested according to national standards, and the yield strength R el =1205MPa, tensile strength R m =2040MPa, elongation A 80 =7.2%, which meets the standard requirements; after the parts are directly painted, there is no peeling or cracking on the surface paint layer, and the quality is excellent.

Claims

1. A method for preparing 2000MPa hot-formed steel without coating and oxidation, characterized in that: The process steps include: (1) Converter smelting: Bottom blowing argon throughout the process, the final temperature is controlled at 1650-1690℃, the final molten steel contains C: 0.06%-0.13%, P≤0.012%; slag blocking steel tapping, the slag volume is controlled to be ≤30mm, and medium carbon ferromanganese, ferrosilicon, ferrochrome, ferrovanadium, and ferroniobium are added in sequence during steel tapping for deoxidation and alloying; (2) LF refining: white slag is made for incoming molten steel, desulfurization is carried out, and composition is adjusted; refining slag, active lime and aluminum shot are added to the ladle to make white slag for refining and desulfurization, the basicity of the ladle top slag is controlled at 4-7, the white slag retention time is ≥16min, the FeO+MnO content of the outgoing slag sample is ≤1.0%, and the outgoing S content is ≤0.012%; titanium wire, boron wire, calcium wire and cerium wire are fed in turn in the later stage of refining, and soft argon is blown for stirring during the wire feeding process, and the outgoing molten steel temperature is 1630-1645℃; The main components of the refined slag are CaO: 50-55%, Al2O3: 30-35%, SiO2: 1-6%, MgO: 4-8%, and the amount of refined slag added is 4-5kg / ton of steel; the activity of the active lime is ≥350ml, the particle size is 5-50mm, and the main components are: CaO ≥92%, S ≤0.045%, K2O+Na2O <0.35%; the amount of active lime added is 1.6-2.5kg / ton of steel; the amount of aluminum shot added is 0.6-1.5kg / ton of steel; (3) Intermediate transfer: The molten steel with qualified composition is hoisted to the ladle turret, and poured into the tundish after being calmed for 10 minutes. The superheat is controlled at 20~50℃ and heat-insulated; The mass percentage of each component in the molten steel after LF refining is: C: 0.24-0.32%, Si: 0.40-0.60%, Mn: 1.0-1.5%, S≤0.010%, P≤0.012%, Als: 0.025-0.045%, Cr: 0.25-0.55%, Ce: 0.020-0.060%, Ti: 0.025-0.040%, V: 0.020-0.050%, Nb: 0.020-0.040%, B: 0.0010-0.0030%; (4) Twin-roll casting: Molten steel is injected into the twin-roll casting machine through an immersed nozzle, the roll gap is controlled between 1.5 and 4.5 mm, the solidification rate of the molten steel is controlled between 200 and 600 °C / s, the billet drawing speed is controlled between 60 and 120 m / min, and argon or nitrogen is used for protection during the casting process; (5) Billet rolling: hot rolling is carried out under argon or nitrogen protection; micro-tension rolling is adopted, the rolling speed is 80~200m / min, the rolling temperature is 950~1200℃, the reduction is 50~80%, and the thickness of the steel strip after hot rolling is controlled at 0.8~2.0mm; (6) Controlled cooling of steel strip: After rolling, the steel strip is cooled by water curtain using laminar cooling method. The cooling water pressure is 0.3~1.0Mpa. The cooling rate of the steel strip is controlled at 10~60℃ / min, and the final cooling temperature is 500~750℃; (7) Steel strip coiling: After the head and tail of the steel strip are cut off, it is sent to the coiler through the pinch roller for coiling to obtain the finished thin steel strip coil; (8) Leveling treatment: Strong roller leveling to ensure the flatness of the steel strip surface and control the flatness of the plate surface ≤5I; (9) Grinding treatment: In a closed grinding box, the gap between the grinding rollers is automatically adjusted according to the thickness of the steel strip. The steel strip is ground under slight tension and the easily detached iron oxide scale on the surface of the steel strip is washed off, leaving only the oxide film with a thickness of 5µm to 10µm that is tightly bonded to the bottom layer and the substrate. The steel strip is dried after leaving the grinding box. (10) Hot forming treatment: According to the size of the automobile parts, the thin strip is processed into the corresponding size, and the sheet is heated to 820~930℃ using an electromagnetic induction heating device and kept warm for 3~5 minutes for austenitization treatment. Then, it is stamped and quenched in a mold with a cooling device to obtain an ultra-high strength component with good surface quality.

2. The method for preparing a coating-free, oxidation-resistant 2000MPa hot-formed steel according to claim 1, characterized in that: In the steps (4) and (5), the protective gas pressure is 0.2-0.5 MPa, and the protective gas purity is 99.99%.

3. The method for preparing a coating-free, oxidation-resistant 2000MPa hot-formed steel according to claim 1, characterized in that: In step (9), the diameter of the grinding roller is 350 mm, the rotation speed is 120-600 r / min, and the tension of the steel belt is 30-150 KN.

4. The method for preparing a coating-free, oxidation-resistant 2000MPa hot-formed steel according to claim 1, characterized in that: In step (10), the quenching coolant is hot water at 90-100° C., which contains ≤1% salt.

5. The 2000MPa hot-formed steel prepared by the method for preparing a coating-free, oxidation-resistant 2000MPa hot-formed steel according to any one of claims 1 to 4, wherein the mass percentages of the main components are: C: 0.24-0.32%, Si: 0.40-0.60%, Mn: 1.0-1.5%, S≤0.010%, P≤0.012%, Als: 0.025-0.045%, Cr: 0.25-0.55%, Ce: 0.020-0.060%, Ti: 0.025-0.040%, V: 0.020-0.050%, Nb: 0.020-0.040%, B: 0.0010-0.0030%; the remainder is iron and unavoidable impurities.