A pre-treatment dispersant for particle size distribution test of carbon surface powder material and its use method
By pretreating the carbon surface powder material with polyether modified polyorganosiloxane, ethanol and water, the problem of difficulty in dispersion and easy agglomeration is solved, and the accuracy and efficiency of particle size distribution testing is achieved. Improved, eliminated the ultrasonic dispersion step and simplified the testing process.
Patent Information
- Application Number
- CN202211007476.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-22
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-08-22
AI Technical Summary
The existing carbon surface powder materials are difficult to disperse and easily agglomerate during particle size distribution testing, resulting in unsatisfactory test data. In addition, ultrasonic dispersion has difficulty in controlling and crushing risks, which affects the accuracy of the test results.
The proportional dispersant of polyether modified polyorganosiloxane, ethanol and water was pretreated to completely wet and disperse the carbon surface powder material, cancel the ultrasonic dispersion step, and a laser particle size meter was used for particle size distribution testing.
The stable dispersion of carbon surface powder materials is achieved, the accuracy and testing efficiency of particle size distribution testing is improved, the testing process is simplified, and secondary agglomeration and material breakage are avoided.
Smart Images

Figure CN115372117B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of dispersion of carbon surface powder materials, and in particular to a pre-treatment dispersant for a particle size distribution test of a carbon surface powder material and a use method thereof. Background Art
[0002] The main raw materials used in lithium-ion batteries are lithium iron phosphate, lithium nickel cobalt manganese oxide, lithium cobalt oxide, and graphite. Particle size distribution is one of the important physical indicators for detecting lithium-ion battery powder materials. In the case of graphite, the diffusion of lithium ions between graphite negative electrode materials is directly related to the particle size of the graphite material. The larger the particle size of the graphite, the longer the diffusion path of the lithium ions; at the same time, the particle size distribution will directly affect the battery pulping process and volume energy density. Under the same volume filling ratio, the larger the particle size of the material, the wider the particle size distribution, and the lower the viscosity of the slurry, which is beneficial for increasing the solid content and reducing the difficulty of coating.
[0003] Common particle size testing methods include laser diffraction, ultrasonic method, dynamic light diffraction, sedimentation method, screening method, etc. Among them, laser diffraction method is widely used due to its advantages such as simple operation and wide test range. Carbon surface powder materials such as lithium iron phosphate, conductive carbon, and graphite are difficult to disperse and easy to agglomerate due to their small particle size and surface hydrophobicity. At present, the industry uses external ultrasonic dispersion for such materials and then uses laser diffraction method to test the particle size distribution. External ultrasonic dispersion has problems such as difficult to control ultrasonic intensity, inability to determine ultrasonic time, and ultrasonic over-crushing, which makes large particles of the material easier to be crushed secondary or agglomerated particles are not effectively dispersed, making the particle size distribution test data unsatisfactory and unable to achieve the purpose of monitoring the properties of the material. Summary of the invention
[0004] The purpose of the present invention is to provide a pre-treatment dispersant for the particle size distribution test of a carbon surface powder material and a method for using the same. 1. Provide a pre-treatment dispersant for the particle size distribution test of a carbon surface powder material, so that the agglomerated carbon surface powder material particles are completely wetted and dispersed, and remain unchanged at all times, and no secondary agglomeration occurs, thereby improving the accuracy of the test data;
[0005] 2. Make the particle size distribution test process of carbon surface powder material simple, and eliminate the ultrasonic dispersion step in the powder material test process, thus improving the test efficiency;
[0006] To solve the above problems, the present invention provides the following technical solutions:
[0007] A method for pre-treatment of a particle size distribution test of a carbon surface powder material, the specific steps are as follows:
[0008] S1. Add a dispersant and water into a container, wherein the volume ratio of the dispersant to water is 1:9; the dispersant is prepared according to the following volume fractions: 1-2% polyether-modified polyorganosiloxane + 10-14% ethanol + 85-88% water;
[0009] S2. In the powder particle size test pretreatment device, the powder to be tested is dispersed in the mixed liquid of S1 at 0.1-1 g / 20 mL. The powder and mixed liquid are automatically circulated and the dispersed suspension is collected at the discharge port as the sample to be tested.
[0010] S3. Pour all the dispersed suspension samples into the dispersion tank of the laser particle size analyzer to perform particle size distribution test.
[0011] Preferably, the powder particle size test pretreatment device includes a liquid storage tank, a mounting plate is vertically provided on the rear wall of the liquid storage tank, the central rotation connection of the mounting plate is provided with a rotating shaft, the front side of the mounting plate is provided with an annular groove, the annular groove is coaxially arranged with the rotating shaft, the central rotation connection of the rotating shaft is provided with an air pumping tube, the air pumping tube is fixed on the liquid storage tank, the rear end of the rotating shaft is provided with a driving assembly, a plurality of floating and suction liquid assemblies are evenly provided on the rotating shaft along the circumferential direction, the rear sides of the floating and suction liquid assemblies are provided with sliders, the sliders are sealed and slidably connected in the annular groove, and the distal end of the slider is provided with an outlet A liquid hole is provided at the proximal end of the slider, an air outlet hole is provided at the proximal end of the slider, a through hole 1 and a through hole 2 are provided at the mounting plate, an exhaust pipe is provided at the rear side of the mounting plate, the air outlet hole is periodically connected to the exhaust pipe through the through hole 2, the bottom of the floating liquid suction component is connected to an air inlet pipe, the air inlet pipe is arranged along the radial direction of the rotating shaft, a through hole 3 is provided on the air pumping pipe, the air inlet pipe is periodically connected to the air pumping pipe through the through hole 3, a mixing box and a round box are also provided at the rear side of the mounting plate, the mixing box is connected to the side wall of the round box, a liquid inlet is provided on the shell of the mixing box, and the liquid outlet hole is periodically connected to the The mixing box is connected with the liquid inlet through a through hole 1, a cylinder is provided on the top of the mixing box, a push plate is slidably connected in the mixing box, a sampling tube is connected to the bottom of the shell of the mixing box, a rotating rod is rotatably connected to the center of the round box, a rotating plate is rotatably connected to the rotating rod, a baffle and an arc-shaped insert are provided at one end of the rotating plate, the baffle and the arc-shaped insert are respectively arranged on both sides of the rotating plate, an iron block is provided at the other end of the rotating plate, a magnetic sheet is provided on the inner wall of the round box, the magnetic sheet is magnetically adsorbed to the iron block, an arc-shaped groove is provided on the inner side of the shell of the round box, the arc-shaped groove is arranged at the connecting part of the round box and the mixing box, the The upper parts of the rotating plate and the baffle are both slidably connected in the arc groove, and the arc plug is rotatably connected to the arc groove. An arc slot is also provided in the shell of the round box, and the arc plug is slidably inserted in the arc slot. A pressure sensor is provided at the sealed end of the arc slot, and the pressure sensor and the drive assembly are electrically connected to the PLC. An hourglass is plugged into the top of the round box, and the hourglass is arranged above the angle area between the baffle and the rotating plate. A waste liquid pipe is connected to the side wall of the round box, and the waste liquid pipe is arranged at the angle between the baffle and the rotating plate. A vibration motor is provided on the outer wall of the round box and the mixing box.
[0012] Preferably, the driving assembly includes a gear ring arranged at the rear end of the rotating shaft, and a motor 1 is also provided on the rear side of the mounting plate. A gear is provided on the output shaft of the motor, and the gear is meshed with the gear ring. The motor 1 is electrically connected to the PLC.
[0013] Preferably, the floating liquid suction assembly includes a suction tube arranged on a rotating shaft, the slider is arranged between the suction tube and the annular groove, the air outlet hole and the liquid outlet hole are both connected to the internal cavity of the suction tube, the air inlet pipe is connected to the bottom of the suction tube, the outer end of the suction tube is connected to the liquid inlet pipe, the suction tube is sealingly and slidingly connected with a piston, the piston is provided with a push rod, the push rod extends from the liquid inlet pipe, a float is provided on the outer end of the push rod, and an annular plug is provided at the connection between the push rod and the float.
[0014] The advantages of the present invention are:
[0015] 1. The particle size distribution pretreatment dispersant provided by the present invention can effectively disperse the carbon surface powder material without ultrasonic dispersion, and will not destroy the particle size of the material itself. At the same time, the dispersed powder material is not easy to re-agglomerate, which improves the accuracy of the test data; the test method provided by the present invention simplifies the particle size distribution test process of the carbon surface powder material, eliminates internal and external ultrasound during dispersion, and improves the test efficiency;
[0016] 2. The present invention adopts a powder particle size test pretreatment device that can automatically weigh and mix solid powders and automatically extract and add an aqueous solution containing a dispersant, which can effectively prevent the powder from being lifted and overflowed. At the same time, it does not require manual multiple weighing, which can greatly reduce the workload. In combination with a dispersant with excellent dispersing performance, it can quickly prepare particle size samples to be tested, thereby improving detection efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 Particle size distribution pre-treatment dispersion diagram.
[0018] Figure 2 Comparison of lithium iron phosphate particle size distribution curves.
[0019] Figure 3 and Figure 4 Schematic diagram of the overall structure of the powder particle size test pretreatment device at different viewing angles.
[0020] Figure 5 This is a top view of the powder particle size test pre-treatment device.
[0021] Figure 6 for Figure 5 AA section view.
[0022] Figure 7 for Figure 5 Middle BB section view.
[0023] Figure 8 for Figure 5 Middle CC section view.
[0024] Among them, 1-liquid storage tank, 11-mounting plate, 111-ring groove, 112-exhaust pipe, 113-through hole 1, 114-through hole 2, 2-rotating shaft, 21-inflating pipe, 211-through hole 3, 22-gear ring, 3-suction pipe, 31-liquid inlet pipe, 32-push rod, 321-ring plug, 322-piston, 33-floating ball, 34-sliding block, 341-air outlet, 342-liquid outlet, 35 -intake pipe, 4-mixing box, 41-cylinder, 42-sampling tube, 43-push plate, 44-liquid inlet, 5-round box, 51-hourglass, 511-waste liquid pipe, 52-rotating rod, 53-rotating plate, 531-baffle, 54-iron block, 55-magnetic sheet, 56-arc slot, 561-pressure sensor, 57-arc plug, 58-arc slot, 6-motor 1, 61-gear, 7-vibration motor. DETAILED DESCRIPTION
[0025] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.
[0026] Example 1: A method for pre-treatment of a carbon surface powder material for particle size distribution test and test sample preparation:
[0027] In this embodiment, based on the agglomeration and difficult dispersion problems of carbon surface powder materials in the background technology, the present invention provides a pre-treatment dispersant for particle size distribution test of carbon surface powder materials and a method of use. The purpose is to provide a pre-treatment dispersant for particle size distribution, which can make the agglomerated carbon surface powder material particles in a stable dispersed state; the dispersed material remains unchanged, greatly improving the accuracy of the test data.
[0028] The pretreatment dispersant for the particle size distribution test of the carbon surface powder material described in the present invention is an effective ratio verified by continuous experiments, and the dispersant includes the following raw materials in mass ratio: 1% polyether modified polyorganosiloxane (FY-3102H wetting agent), 14% ethanol, and 85% water.
[0029] The polyether-modified polyorganosiloxane in the dispersant raw material is easily soluble in water and has extremely low surface tension. It provides excellent wettability, bond extension and penetration ability during the dispersion process, thereby improving the dispersion ability of carbon powder materials. Ethanol, as a buffering agent, can not only increase the dispersion ability of the entire system for carbon materials, but also make the dispersed material particles evenly distributed to avoid secondary agglomeration.
[0030] The proportion of polyether-modified polyorganosiloxane in the dispersant raw material can be adjusted to 0.5-2%. The raw material should not be added in too much amount. If the amount is too much, a large number of bubbles will be generated during the dispersion process, affecting the test results of the particle size distribution; the ethanol ratio can be adjusted to 10-20%, and organic solvents such as ethyl acetate can also be used.
[0031] The present invention also provides a method for using the particle size distribution pretreatment dispersant. Prepare the dispersant solvent according to the relevant ratio, use a pipette to draw 2 mL of the dispersant into a 50 mL beaker, add an appropriate amount of lithium iron phosphate powder to be tested, and shake well; then add 18 mL of water to the beaker and shake well; pour all the dispersed solution in the beaker into the dispersion tank of the laser particle size analyzer to perform a particle size distribution test.
[0032] In this embodiment, the dispersant is prepared according to the following volume fractions: 1% polyether-modified polyorganosiloxane + 14% ethanol + 85% water.
[0033] 1. Add 2 mL of dispersant to a 50 mL beaker;
[0034] 2. Add 1g of lithium iron phosphate powder to be tested into the beaker and shake well;
[0035] 3. Then add 18mL of water into the beaker and shake well; water can also be mixed with the dispersant first and then with the powder.
[0036] 4. Pour all the dispersed solution in the beaker into the dispersion tank of the laser particle size analyzer without ultrasound to perform particle size distribution test.
[0037] Comparative Example 1: Preparation of lithium iron phosphate particle size test sample:
[0038] 1. Add 20 mL of dispersant into a 50 mL beaker; the dispersant is 100% water.
[0039] 2. Add 1g of lithium iron phosphate powder to be tested into the beaker and shake well;
[0040] 3. Place the beaker in an ultrasonic cleaner and perform external ultrasound at 50% intensity for 3 minutes;
[0041] 4. Pour all the dispersed solution after ultrasound into the dispersion tank of the laser particle size analyzer for particle size distribution test;
[0042] Comparative Example 2: Preparation of lithium iron phosphate particle size test samples:
[0043] 1. Add 20 mL of dispersant into a 50 mL beaker; the dispersant is 100% ethanol.
[0044] 2. Add 1g of lithium iron phosphate powder to be tested into the beaker and shake well;
[0045] 3. Place the beaker in an ultrasonic cleaner and perform external ultrasound at 50% intensity for 3 minutes;
[0046] 4. Pour all the dispersed solution after ultrasound into the dispersion tank of the laser particle size analyzer for particle size distribution test;
[0047] Comparative Example 3: Preparation of lithium iron phosphate particle size test samples:
[0048] 1. Add 2 mL of dispersant to a 50 mL beaker; the dispersant is prepared according to the following volume fractions: 1% polyether-modified polyorganosiloxane + 99% water;
[0049] 2. Add 1g of lithium iron phosphate powder to be tested into the beaker and shake well;
[0050] 3. Then add 18mL of water to the beaker and shake well;
[0051] 4. Pour all the dispersed solution in the beaker into the dispersion tank of the laser particle size analyzer without ultrasound to perform particle size distribution test.
[0052] Example 2: Preparation of lithium iron phosphate particle size test sample:
[0053] 1. Add 2 mL of dispersant to a 50 mL beaker; the dispersant is prepared according to the following volume fractions: 2% polyether-modified polyorganosiloxane + 10% ethanol + 88% water;
[0054] 2. Add 0.5g of lithium iron phosphate powder to be tested into the beaker and shake well;
[0055] 3. Then add 18mL of water to the beaker and shake well;
[0056] 4. Pour all the dispersed solution in the beaker into the dispersion tank of the laser particle size analyzer without ultrasound to perform particle size distribution test.
[0057] Example 3: Preparation of lithium iron phosphate particle size test sample:
[0058] 1. Add 2 mL of dispersant to a 50 mL beaker; the dispersant is prepared according to the following volume fraction ratio: 1% polyether-modified polyorganosiloxane + 14% ethyl acetate + 85% water;
[0059] 2. Add 0.1g of lithium iron phosphate powder to be tested into the beaker and shake well;
[0060] 3. Then add 18mL of water to the beaker and shake well;
[0061] 4. Pour all the dispersed solution in the beaker into the dispersion tank of the laser particle size analyzer without ultrasound to perform particle size distribution test.
[0062] Example 4: Preparation of graphite particle size test sample:
[0063] 1. Add 2 mL of dispersant to a 50 mL beaker; the dispersant is prepared according to the following volume fraction ratio: 1% polyether-modified polyorganosiloxane + 14% ethanol + 85% water;
[0064] 2. Add 0.5g of graphite powder to be tested into the beaker and shake well;
[0065] 3. Then add 18mL of water to the beaker and shake well;
[0066] 4. Pour all the dispersed solution in the beaker into the dispersion tank of the laser particle size analyzer without ultrasound to perform particle size distribution test.
[0067] Example 5: Preparation of Conductive Carbon Black Particle Size Test Sample:
[0068] 1. Add 2 mL of dispersant to a 50 mL beaker; the dispersant is prepared according to the following volume fraction ratio: 1% polyether-modified polyorganosiloxane + 14% ethanol + 85% water;
[0069] 2. Add 0.5g of the conductive carbon black powder to be tested into the beaker and shake well;
[0070] 3. Then add 18mL of water to the beaker and shake well;
[0071] 4. Pour all the dispersed solution in the beaker into the dispersion tank of the laser particle size analyzer without ultrasound to perform particle size distribution test.
[0072] Example 6: The use of the dispersant disclosed in the present invention can quickly disperse the powder to be tested without the need for auxiliary dispersion methods such as ultrasound. However, in actual application, we found that a batch of powder often requires multiple sampling and preparation of samples for testing, and the results of multiple tests must be combined to obtain accurate particle size test data. When there are many types or batches of powders, the number of times weighing and preparation will increase significantly, which not only increases the workload, but also the particle size of powders such as lithium iron phosphate is generally small. When weighing, it is inevitable that they will be lifted up and inhaled by the operator, causing potential health hazards. In addition, the open preparation method can easily cause particles with smaller particle sizes to fly and adhere, resulting in the measured particle size results being larger and inaccurate.
[0073] Therefore, in this embodiment, a powder particle size test pre-treatment device is used to prepare the particle size test sample, and its structure is as follows: Figures 3 to 8As shown, it includes a liquid storage tank 1, a mounting plate 11 is vertically provided on the rear wall of the liquid storage tank 1, the central rotation connection of the mounting plate 11 is connected to the rotating shaft 2, the front side of the mounting plate 11 is provided with an annular groove 111, the annular groove 111 is coaxially arranged with the rotating shaft 2, the central rotation connection of the rotating shaft 2 is connected to the air pumping pipe 21, the air pumping pipe 21 is fixed on the liquid storage tank 1, a driving component is provided at the rear end of the rotating shaft 2, a plurality of floating liquid suction components are evenly provided on the rotating shaft 2 along the circumferential direction, the rear sides of the floating liquid suction components are provided with sliders 34, the sliders 34 are sealed and slidably connected in the annular groove 111, the distal end of the slider 34 is provided with a liquid outlet 342, the proximal end of the slider 34 is provided with an air outlet 341, the mounting plate 11 is provided with a liquid outlet 342, and the proximal end of the slider 34 is provided with an air outlet 341. The mounting plate 11 is provided with a through hole 113 and a through hole 214, the rear side of the mounting plate 11 is provided with an exhaust pipe 112, the air outlet hole 341 is periodically connected to the exhaust pipe 112 through the through hole 214, the bottom of the floating liquid suction assembly is connected to an air inlet pipe 35, the air inlet pipe 35 is arranged along the radial direction of the rotating shaft 2, the air pumping pipe 21 is provided with a through hole 311, the air inlet pipe 35 is periodically connected to the air pumping pipe 21 through the through hole 311, the rear side of the mounting plate 11 is also provided with a mixing box 4 and a round box 5, the side walls of the mixing box 4 and the round box 5 are connected, the shell of the mixing box 4 is provided with a liquid inlet 44, the liquid outlet hole 342 is periodically connected to the liquid inlet 44 through the through hole 113 The mixing box 4 is connected, a cylinder 41 is provided on the top, a push plate 43 is slidably connected in the mixing box 4, a sampling tube 42 is connected to the bottom of the shell of the mixing box 4, a rotating rod 52 is rotatably connected to the center of the round box 5, a rotating plate 53 is rotatably connected to the rotating rod 52, a baffle 531 and an arc-shaped insert 57 are provided at one end of the rotating plate 53, the baffle 531 and the arc-shaped insert 57 are respectively arranged on both sides of the rotating plate 53, an iron block 54 is provided at the other end of the rotating plate 53, a magnetic sheet 55 is provided on the inner wall of the round box 5, the magnetic sheet 55 and the iron block 54 are magnetically adsorbed, an arc-shaped groove 58 is provided on the inner side of the shell of the round box 5, the arc-shaped groove 58 is arranged at the connecting part of the round box 5 and the mixing box 4, the rotating plate 53 and the baffle 531 are arranged at the connecting part of the round box 5 and the mixing box 4, The upper part of the plate 531 is slidably connected to the arc groove 58, and the arc plug 57 is rotatably connected to the arc groove 58. The shell of the round box 5 is also provided with an arc slot 56, and the arc plug 57 is slidably inserted in the arc slot 56. The sealed end of the arc slot 56 is provided with a pressure sensor 561, and the pressure sensor 561 and the driving component are electrically connected to the PLC. The top of the round box 5 is plugged with an hourglass 51, and the hourglass 51 is arranged above the angle area between the baffle 531 and the rotating plate 53. The side wall of the round box 5 is connected with a waste liquid pipe 511, and the waste liquid pipe 511 is arranged at the angle between the baffle 531 and the rotating plate 53. The outer walls of the round box 5 and the mixing box 4 are provided with a vibration motor 7.
[0074] In this embodiment, the floating liquid suction component includes a suction tube 3 arranged on the rotating shaft 2, the slider 34 is arranged between the suction tube 3 and the annular groove 111, the air outlet hole 341 and the liquid outlet hole 342 are both connected to the internal cavity of the suction tube 3, the air inlet pipe 35 is connected to the bottom of the suction tube 3, the outer end of the suction tube 3 is connected to the liquid inlet pipe 31, the suction tube 3 is sealed and slidably connected with a piston 322, the piston 322 is provided with a push rod 32, the push rod 32 extends from the liquid inlet pipe 31, the outer end of the push rod 32 is provided with a float 33, and the connection between the push rod 32 and the float 33 is provided with an annular plug 321.
[0075] In this embodiment, the driving assembly includes a ring gear 22 arranged at the rear end of the rotating shaft 2, and a motor 6 is also provided on the rear side of the mounting plate 11. A gear 61 is provided on the output shaft of the motor, and the gear 61 is meshed with the ring gear 22. The motor 6 is electrically connected to the PLC.
[0076] The process of preparing the particle size test sample by the above-mentioned powder particle size test pretreatment device is as follows:
[0077] First, fill the liquid storage tank 1 with dispersion liquid, which is an aqueous solution containing 10% (V / V) dispersant, and the liquid level can be slightly lower than the air pumping tube 21. At this time, the float 33 at the 6 o'clock position moves upward due to the buoyancy, and the float 33 pushes the push rod 32 and the piston 322 to move upward. At this time, the dispersion liquid is sucked into the suction tube 3 through the liquid inlet tube 31, and the air above the piston 322 in the suction tube 3 is discharged through the air outlet 341, the second through hole 114 and the exhaust pipe 112, until the annular plug 321 moves up with the float 33 to block the liquid inlet tube 31, and the liquid suction process is completed. Turn on the motor 6, rotate the shaft 2 90° through the gear 61 and the ring gear 22, and the slider 34 also rotates 90° in the annular groove 111. At this time, the air outlet 341 is blocked by the annular groove 111 and no longer ventilates. The air outlet 341 is connected with the air outlet two and the exhaust pipe 112 only at the 6 o'clock position, and the air inlet pipe 35 is connected with the pumping pipe 21 through the through hole three 211 only at the 12 o'clock position. In addition, the liquid outlet 342 is connected with the liquid inlet 44 through the through hole one 113 only at the 12 o'clock position. The lithium iron phosphate powder is loaded into the hourglass 51 and inserted into the round box 5. The lithium iron phosphate powder gradually leaks into the space between the rotating plate 53 and the baffle 531. When the lithium iron phosphate powder between the rotating plate 53 and the baffle 531 accumulates to a certain amount, due to the principle of leverage, the rotating plate 53 will rotate around the rotating rod 52. At this time, the iron block 54 and the magnetic sheet 55 are separated, and the arc-shaped insert 57 is inserted into the arc-shaped groove 58. When the arc-shaped insert 57 is completely inserted into the arc-shaped groove 58, the angle area between the rotating plate 53 and the baffle 531 is just open to the mixing box 4. The vibration motor 7 is turned on to vibrate the powder between the rotating plate 53 and the baffle 531 and slide it into the mixing box 4. When the powder is emptied, the gravity of the iron block 54 drives the rotating plate 54 to rotate. The plate 53 is reversed and reset until the iron block 54 is adsorbed on the magnetic sheet 55. When the front end of the arc-shaped insert 57 touches the pressure sensor 561, the pressure sensor 561 sends an electrical signal to the PLC, and the PLC controls the motor to rotate the shaft 2 by 690 degrees. At this time, the suction pipe 3 and the slider 34 rotate to the 12 o'clock position, and air is pumped into the suction pipe 3 through the air inlet pipe 35 through the air pumping pipe 21. The air pushes the piston 322 upward, and the dispersion in the suction pipe 3 is pressed out into the mixing box 4 through the liquid outlet hole 342, the through hole 113 and the liquid inlet 44. The sampling tube 42 of the mixing box 4 is closed. At this time, the dispersion in the mixing box 4 and the lithium iron phosphate powder are fully mixed under the vibration motor 7. After the mixing and dispersing operation is completed, the cylinder 41 is opened, the sampling tube 42 is opened, and the dispersed mixture is completely pressed out to obtain a particle size detection sample. When the liquid in the suction tube 3 is completely pressed out, the piston 322, the push rod 32 and the float 33 are reset, and when the powder between the baffle 531 and the rotating plate 53 is accumulated to a certain amount again, the rotating plate 53 rotates again, and the arc-shaped insert 57 is used to trigger the rotating shaft 2 to rotate 90 degrees, and the liquid is repeatedly injected into the mixing box 4. By repeating the above operation, the preparation of multiple samples can be completed quickly.
[0078] When the powder samples are different, the hourglass 51 can be replaced and new powder can be loaded for preparation. When the rotating plate 53 is reset, the arc-shaped insert 57 will completely separate the round box 5 and the mixing box 4, but the arc-shaped insert 57 is tangent to the side wall of the mixing box 4 and will not affect the up and down sliding of the push plate 43. The space between the rotating plate 53 and the baffle 531 can be flushed with a dispersion liquid, and the dispersion liquid flows out from the waste liquid pipe 511 to dry the space between the rotating plate 53 and the baffle 531. In addition, if you want to clean the mixing box 4, you can leave some dispersion liquid in the suction tube 3. After the mixing is completed, continue to pump in air to squeeze all the remaining liquid in the suction tube 3 into the mixing box 4, flush the mixing box 4, and use the push plate 43 to empty the mixing box 4.
[0079] The particle size test results are as follows:
[0080] Table 1 Particle size distribution test data
[0081]
[0082] Result analysis:
[0083] Comparative Example 1 is a method of pre-dispersing lithium iron phosphate powder using a dispersant [water 100%]; there are obvious large agglomerated particles at the bottom of the pre-dispersed beaker that are not effectively dispersed, and the D0-D99 in the particle size distribution test data is obviously too large, with D99 reaching 80.5 μm; the agglomerated particles cannot be effectively dispersed by external ultrasound, indicating that the dispersion method using the dispersant [water 100%] is ineffective;
[0084] Comparative Example 2 is a method of pre-dispersing lithium iron phosphate powder using a dispersant [ethanol 100%]; there are many aggregated particles at the bottom of the pre-dispersed beaker that are not effectively dispersed, and the D50 in the particle size distribution test data is larger than that of the embodiment group; although the dispersion effect is improved by ethanol and external ultrasonic dispersion, the dispersion effect does not reach the expected goal;
[0085] Comparative Example 3 is a method of pre-dispersing lithium iron phosphate powder using a dispersant [polyether-modified polyorganosiloxane 1% + water 99%]; since there is no ethanol in the dispersant, the dispersed particles are secondary agglomerated and gathered at the bottom of the beaker, and the D50 in the particle size distribution test data is larger than that of the embodiment group; the dispersion effect is further improved by reducing the ethanol ratio of the dispersant, but the dispersion effect still does not reach the expected goal;
[0086] In Example 1, lithium iron phosphate powder was pre-dispersed using a dispersant [1% polyether-modified polyorganosiloxane + 14% ethanol + 85% water]; this is the optimal dispersant formula. It can be clearly seen in the beaker that the dispersed solution is evenly distributed without secondary agglomeration, and the D0-D99 data in the particle size distribution test data are relatively low; the sample was directly tested after being dispersed by the dispersant, and the ultrasonic method was eliminated. The dispersant with this ratio was used to achieve effective dispersion;
[0087] In Example 2, a dispersant [2% polyether-modified polyorganosiloxane + 10% ethanol + 88% water] is used to pre-disperse lithium iron phosphate powder; this dispersant changes the ratio of polyether-modified polyorganosiloxane to ethanol, and it can be clearly seen in the beaker that the dispersed solution is evenly distributed without secondary agglomeration, and the D0-D99 data in the particle size distribution test data are relatively low; the sample is directly tested after being dispersed by this dispersant, and the ultrasonic method is cancelled. The use of this ratio of dispersant achieves effective dispersion;
[0088] In Example 3, a dispersant [2% polyether-modified polyorganosiloxane + 10% ethanol + 88% water] is used to pre-disperse lithium iron phosphate powder; this dispersant changes the ratio of polyether-modified polyorganosiloxane to ethanol, and it can be clearly seen in the beaker that the dispersed solution is evenly distributed without secondary agglomeration, and the D0-D99 data in the particle size distribution test data are relatively low; the sample is directly tested after being dispersed by this dispersant, and the ultrasonic method is cancelled. The use of this ratio of dispersant achieves effective dispersion;
[0089] In Example 4, the graphite powder was pre-dispersed using a dispersant [1% polyether-modified polyorganosiloxane + 14% ethanol + 85% water]. It can be clearly seen in the beaker that the dispersed solution is evenly distributed without secondary agglomeration. The particle size distribution test data does not show a high D99 value, and the particle size volume distribution is reasonable. The sample was directly tested after being dispersed by the dispersant, and the ultrasonic method was cancelled. The dispersant with this ratio was used to achieve effective dispersion.
[0090] In Example 5, a dispersant [1% polyether-modified polyorganosiloxane + 14% ethanol + 85% water] is used to pre-disperse the conductive carbon black powder. It can be clearly seen in the beaker that the dispersed solution is evenly distributed without secondary agglomeration. The particle size distribution test data does not show a high D99 value, and the particle size volume distribution is reasonable. The sample is directly tested after being dispersed by the dispersant, and the ultrasonic method is eliminated. The dispersant with this ratio is used to achieve effective dispersion.
[0091] The particle size data of Example 6 is further reduced compared with Examples 1 to 3, which indicates that the preparation device and preparation method of Example 6 effectively reduce the dispersion of small-particle powders and further improve the accuracy of measurement. The use of a powder particle size test pre-treatment device can automatically weigh and mix solid powders and automatically extract and add a dispersant-containing aqueous solution, which can effectively prevent the powder from being lifted and overflowed. At the same time, it does not require manual multiple weighing, which can greatly reduce the workload. The use of a dispersant with excellent dispersibility can quickly prepare a particle size test sample, thereby improving the detection efficiency.
[0092] It is known from common technical knowledge that the present invention can be implemented by other embodiments that do not deviate from its spirit or essential features. Therefore, the above disclosed embodiments are only illustrative in all respects and are not exclusive. All changes within the scope of the present invention or within the scope equivalent to the present invention are included in the present invention.
Claims
1. A method for pre-treatment of a carbon surface powder material for particle size distribution testing, characterized in that: The specific steps are as follows: S1. Add dispersant and water into a container, wherein the volume ratio of the dispersant to water is 1:9; the dispersant is prepared according to the following volume fractions: 1-2% polyether-modified polyorganosiloxane + 10-14% ethanol + 85-88% water; S2. In the powder particle size test pretreatment device, the powder to be tested is dispersed in the mixed liquid of S1 at 0.1-1 g / 20 mL. The powder and mixed liquid are automatically circulated and the dispersed suspension is collected at the discharge port as the sample to be tested. S3, pour all the dispersed suspension samples into the dispersion tank of the laser particle size analyzer to perform a particle size distribution test; The powder particle size test pretreatment device comprises a liquid storage tank (1), a mounting plate (11) is vertically provided on the rear wall of the liquid storage tank (1), the center of the mounting plate (11) is rotatably connected to a rotating shaft (2), a front side of the mounting plate (11) is provided with an annular groove (111), the annular groove (111) is coaxially arranged with the rotating shaft (2), the center of the rotating shaft (2) is rotatably connected to an air pumping pipe (21), the air pumping pipe (21) is fixedly arranged on the liquid storage tank (1), a driving component is provided at the rear end of the rotating shaft (2), a plurality of floating and absorbing liquid components are evenly arranged on the rotating shaft (2) along the circumferential direction, a slider (34) is provided on the rear side of each of the floating and absorbing liquid components, the sliders (34) are sealed and slidably connected in the annular groove (111), and the sliders (34) are sealed and slidably connected in the annular groove (111). 4) is provided with a liquid outlet hole (342) at the distal end, and an air outlet hole (341) is provided at the proximal end of the slider (34). The mounting plate (11) is provided with a through hole 1 (113) and a through hole 2 (114). The rear side of the mounting plate (11) is provided with an exhaust pipe (112). The air outlet hole (341) is periodically connected to the exhaust pipe (112) through the through hole 2 (114). The bottom of the floating and sucking liquid assembly is connected with an air inlet pipe (35). The air inlet pipe (35) is arranged along the radial direction of the rotating shaft (2). The pumping pipe (21) is provided with a through hole 3 (211). The air inlet pipe (35) is periodically connected to the pumping pipe (21) through the through hole 3 (211). The rear side of the mounting plate (11) is also provided with a mixing box (4). and a round box (5), the mixing box (4) being connected to the side wall of the round box (5), a liquid inlet (44) being provided on the shell of the mixing box (4), the liquid outlet (342) being periodically connected to the liquid inlet (44) through a through hole (113), a cylinder (41) being provided on the top of the mixing box (4), a push plate (43) being slidably connected inside the mixing box (4), a sampling tube (42) being connected to the bottom of the shell of the mixing box (4), a rotating rod (52) being rotatably connected to the center of the round box (5), a rotating plate (53) being rotatably connected to the rotating rod (52), a baffle (531) and an arc-shaped insert (57) being provided at one end of the rotating plate (53), the baffle (531) and the arc-shaped insert (57) being respectively arranged on the rotating plate ( 53), an iron block (54) is provided at the other end of the rotating plate (53), a magnetic sheet (55) is provided on the inner wall of the round box (5), the magnetic sheet (55) and the iron block (54) are magnetically attracted, an arc groove (58) is provided on the inner side of the shell of the round box (5), the arc groove (58) is provided at the connection part of the round box (5) and the mixing box (4), the upper parts of the rotating plate (53) and the baffle (531) are both slidably connected in the arc groove (58), the arc plug (57) is rotatably connected with the arc groove (58), an arc slot (56) is further provided in the shell of the round box (5), the arc plug (57) is slidably plugged in the arc slot (56), and a pressure sensor (561) is provided at the sealing end of the arc slot (56),The pressure sensor (561) and the driving assembly are both electrically connected to the PLC; an hourglass (51) is plugged into the top of the round box (5); the hourglass (51) is arranged above the angle area between the baffle plate (531) and the rotating plate (53); a waste liquid pipe (511) is connected to the side wall of the round box (5); the waste liquid pipe (511) is arranged at the angle between the baffle plate (531) and the rotating plate (53); and a vibration motor (7) is arranged on the outer walls of the round box (5) and the mixing box (4); The floating liquid suction component comprises a suction tube (3) arranged on the rotating shaft (2), the slider (34) is arranged between the suction tube (3) and the annular groove (111), the air outlet hole (341) and the liquid outlet hole (342) are both connected to the internal cavity of the suction tube (3), the air inlet pipe (35) is connected to the bottom of the suction tube (3), the outer end of the suction tube (3) is connected to the liquid inlet pipe (31), the suction tube (3) is sealed and slidably connected with a piston (322), the piston (322) is provided with a push rod (32), the push rod (32) extends from the liquid inlet pipe (31), the outer end of the push rod (32) is provided with a float (33), and the connection between the push rod (32) and the float (33) is provided with an annular plug (321).
2. A method for pre-treatment of a particle size distribution test of a carbon surface powder material according to claim 1, characterized in that: The driving assembly comprises a gear ring (22) arranged at the rear end of the rotating shaft (2); a motor 1 (6) is also arranged on the rear side of the mounting plate (11); a gear (61) is arranged on the output shaft of the motor 1; the gear (61) is meshed with the gear ring (22); and the motor 1 (6) is electrically connected to the PLC.