Laminated nonwoven fabrics and sanitary materials
By controlling the fiber diameter and the gap size between the fibers in the laminated nonwoven fabric, the problem that nonwoven fabrics in the prior art is difficult to achieve water absorption and quick drying at the same time, and efficient moisture transfer and surface drying of sanitary materials are achieved.
Patent Information
- Application Number
- CN202180028338.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-06-11
- Filing Date
- 2021-06-08
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-06-08
AI Technical Summary
Non-woven fabrics with existing sanitary materials are difficult to achieve rapid water absorption and sufficient quick drying at the same time, resulting in moisture residue on components that directly contact the skin, affecting comfort.
The capillary is enhanced by controlling the fiber diameter and interfiber gap size in the laminated nonwoven fabric, especially the interfiber gap size of the smallest nonwoven fabric layer, Ra ≤ 200 μm, and optimizing the fiber diameter and interlayer structure in the laminated nonwoven fabric, thereby enhancing the capillary tube. to promote water transfer.
It realizes the full quick-drying and excellent water absorption of non-woven fabrics for sanitary materials, ensures dry surfaces and improves the comfort of use.
Smart Images

Figure BDA0003888503290000221
Abstract
Description
Technical Field
[0001] The present invention relates to a laminated nonwoven fabric particularly suitable for use in sanitary materials and a sanitary material using the laminated nonwoven fabric. Background Art
[0002] Generally speaking, for sanitary materials such as diapers, sanitary napkins, and masks, the key to comfort is to quickly remove moisture such as urine and sweat and keep the surface of the parts dry.
[0003] Therefore, in the parts that come into direct contact with the skin, it is required to achieve both "water absorption" to quickly absorb water and "quick drying" to transfer the absorbed water from the outermost layer to make the surface dry.
[0004] In the past, various nonwoven fabrics subjected to hydrophilization treatment were widely used as the surface member. Although the above structure can guide moisture from the outermost layer to the inner nonwoven fabric and absorbent, moisture easily remains in the outermost layer, and the "quick-drying property" is poor.
[0005] In response to this problem, Patent Document 1 proposes a nonwoven fabric in which a fiber layer (skin-facing side) containing fine-fine fibers and a fiber layer containing coarse-fine fibers are laminated and partially interwoven at the boundary surface. In addition, Patent Document 2 proposes a sheet material in which sheets having different average fiber non-occupied voids due to differences in the mixing ratio and fiber diameter of a plurality of fibers are laminated, and the average fiber non-occupied voids of the first layer in contact with the skin are larger than those of the layers other than the first layer.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 7-042057
[0009] Patent document 2: Japanese Patent Application Laid-Open No. 7-178133. Summary of the invention
[0010] Problems to be solved by the invention
[0011] However, in the technology of Patent Document 1, it is difficult to simultaneously achieve "quick-drying property" and "water absorbency".
[0012] On the other hand, the technology of Patent Document 2 states that by providing a difference in the void volume other than the fibers between the layers, the difference in the capillary effect can be utilized to guide the moisture absorbed by the first layer to the second layer (the layer opposite to the skin surface). However, the technology of Patent Document 2 does not have sufficient "quick-drying property".
[0013] Therefore, an object of the present invention is to provide a laminated nonwoven fabric having sufficient quick-drying properties and excellent water absorption properties for maintaining comfort in a member using a nonwoven fabric for sanitary materials.
[0014] Means for solving problems
[0015] The inventors of the present application have discovered that in the technology of Patent Document 1, since the fiber layer containing fine-fine fibers on the skin side has a dense structure relative to other layers, moisture is easily retained in the fiber layer on the skin side, making it difficult to obtain "quick-drying properties". In addition, since the dense fiber layer on the skin side has reduced liquid permeability, it is unable to quickly absorb moisture, making it difficult to obtain "water absorption properties".
[0016] In addition, the inventors of the present application discovered that since the average fiber non-occupied voids disclosed in Patent Document 2 represent the total volume of the space other than the fibers, it is not an indicator of the void size between the fibers that is important for the capillary force. Although there are differences between the layers, there will be no difference in the capillary force. In particular, in Patent Document 2, since the size of the voids between the fibers of the non-skin surface layer is large, the capillary force cannot be fully exerted, the effect of transferring moisture from the skin surface is limited, and the "quick-drying property" is not sufficient.
[0017] Furthermore, the inventors of the present application have repeatedly conducted in-depth studies to achieve the above-mentioned purpose, and as a result, they have found that in a laminated nonwoven fabric, by controlling the inter-fiber space size taking into account the fiber diameter in addition to the unit area weight and thickness within a specific range in a specific nonwoven fabric layer, a laminated nonwoven fabric having sufficient water absorption and quick-drying properties for use as a nonwoven fabric for sanitary materials can be obtained.
[0018] The present invention has been accomplished based on the above findings, and according to the present invention, the following inventions are provided.
[0019] The present invention is a laminated nonwoven fabric, which is a laminated nonwoven fabric formed by laminating nonwoven fabric layers containing thermoplastic resin fibers, wherein in the nonwoven fabric layer (A) having the smallest average single fiber diameter among the nonwoven fabric layers, the inter-fiber void size Ra (μm) calculated by the following formula (1) is less than 200 μm.
[0020] Ra=(100×Ta×da) / (Wa×Da)-Da···Formula (1)
[0021] in,
[0022] Ta: Thickness of nonwoven fabric layer (A) (μm)
[0023] da: Density (dtex) of the thermoplastic resin fiber constituting the nonwoven fabric layer (A)
[0024] Wa: Weight per unit area of the nonwoven fabric layer (A) (g / m2 )
[0025] Da: average single fiber diameter (μm) of the thermoplastic resin fibers constituting the nonwoven fabric layer (A).
[0026] The present invention is also directed to a sanitary material, at least a portion of which is composed of the laminated nonwoven fabric of the present invention.
[0027] Effects of the Invention
[0028] According to the present invention, it is possible to obtain a laminated nonwoven fabric which has quick-drying properties sufficient for use as a nonwoven fabric for sanitary materials and has an excellent water absorption rate. DETAILED DESCRIPTION
[0029] Hereinafter, the present invention will be described in detail. However, the present invention is not limited to the scope of the following description within the scope of the gist thereof.
[0030] [Thermoplastic resin fiber]
[0031] First, the laminated nonwoven fabric of the present invention is formed by laminating nonwoven fabric layers containing thermoplastic resin fibers.
[0032] The "thermoplastic resin fiber" in the present invention refers to a fiber containing a thermoplastic resin. Such thermoplastic resin fiber may be one kind or may contain a plurality of kinds of thermoplastic resin fibers.
[0033] Examples of the thermoplastic resin used for the thermoplastic resin fiber of the present invention include the following resins:
[0034] Aromatic polyester polymers such as polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, polyhexylene terephthalate, and copolymers thereof,
[0035] Aliphatic polyester polymers and copolymers thereof such as polylactic acid, polyethylene succinate, polybutylene succinate, polybutylene succinate adipate, polyhydroxybutyrate-polyhydroxyvalerate copolymer, polycaprolactone, etc.,
[0036] Aliphatic polyamide polymers such as polyamide 6, polyamide 66, polyamide 610, polyamide 10, polyamide 12, polyamide 6-12 and copolymers thereof,
[0037] Polyolefin polymers such as polypropylene, polyethylene, polybutene, polymethylpentene and their copolymers,
[0038] A water-insoluble ethylene-vinyl alcohol copolymer-based polymer containing 25 mol % to 70 mol % of ethylene units,
[0039] Polystyrene-based, polydiene-based, chlorine-based, polyolefin-based, polyester-based, polyurethane-based, polyamide-based, fluorine-based elastic polymers, etc.
[0040] The thermoplastic resin may also contain various additives such as inorganic substances such as titanium dioxide, silicon dioxide, and barium oxide, colorants such as carbon black, dyes, and pigments, flame retardants, fluorescent whitening agents, antioxidants, and ultraviolet absorbers.
[0041] It should be noted that the thermoplastic resin constituting the thermoplastic resin fibers between the nonwoven fabric layers may be the same or different.
[0042] The thermoplastic resin fiber in the present invention may be a single-component fiber or a composite fiber formed by a composite of two or more resins. When the thermoplastic resin fiber is a composite fiber, it is not particularly limited as long as the effect of the present invention is not impaired, and it can be appropriately selected from core-sheath type, island-in-the-sea type, parallel type, eccentric core-sheath type, etc. In addition, it may be a split fiber composite fiber in which a part or all of the fiber is split from one fiber into a plurality of fibers.
[0043] The cross-sectional shape of the thermoplastic resin fiber of the present invention is not particularly limited as long as it does not impair the effects of the present invention, and may be a circular cross-sectional shape or a triangular, flat, hexagonal, hollow or other shaped cross-sectional shape. When the laminated nonwoven fabric of the present invention is used for sanitary materials, a circular cross-sectional shape is preferred due to its high productivity and excellent softness.
[0044] [Laminated interface of laminated nonwoven fabric]
[0045] The following describes the process for determining the lamination interface of the nonwoven fabric layers in the laminated nonwoven fabric of the present invention. The lamination interface in the laminated nonwoven fabric of the present invention is determined by the following procedure.
[0046] (Steps for determining the stacking interface)
[0047] Step 1: Collect a 5 cm x 5 cm sample piece from the laminated nonwoven fabric. Avoid portions with poor uniformity or reduced thickness.
[0048] Step 2: Take a three-dimensional image of the sample obtained in step 1 using a high-resolution three-dimensional X-ray microscope. The resolution of the measurement can be any range that allows the fiber diameter of each nonwoven fabric layer to be determined, preferably 1.0 μm / voxel or less. Here, when the laminated nonwoven fabric is embossed, the image is taken in such a way that the center point between the embossed points, i.e., the center of the convex portion remaining due to the embossing process, is included in the imaging range of the X-ray CT image.
[0049] Step 3: Extract a 0.5 mm x 0.5 mm region as the analysis target region from the three-dimensional image captured in step 2. Here, when the laminated nonwoven fabric is embossed, the analysis target region is extracted so as to include the center point between the embossed points.
[0050] Step 4: For the analysis target region extracted in Step 3, slice (cross-sectional) images perpendicular to the thickness direction of the laminated nonwoven fabric and parallel to each other are created at intervals of 1 voxel.
[0051] Step 5: The fiber diameters of all fibers contained in each slice image obtained in step 4 are analyzed, and the average value thereof is calculated as a provisional average fiber diameter.
[0052] Step 6: Plot the position of each slice image produced in step 4 in the thickness direction of the laminated nonwoven fabric on the x-axis (in μm), and plot the provisional average fiber diameter of each slice image obtained in step 5 on the y-axis (in μm) to obtain a graph.
[0053] Step 7: In the graph obtained in step 6, the rate of change of the y-axis value relative to the x-axis Δy / Δx is calculated based on the data of 15 consecutive voxels by the least squares method, and the interval on the x-axis where its absolute value is greater than 0.30 is determined as the position of the interface where the non-woven fabric layers are stacked on each other.
[0054] [Non-woven fabric layer (A)]
[0055] The nonwoven fabric layer (A) in the laminated nonwoven fabric of the present invention is defined as a layer having the smallest average single fiber diameter among the nonwoven fabric layers constituting the laminated nonwoven fabric.
[0056] The average single fiber diameter of each nonwoven fabric layer was determined as follows.
[0057] (Measurement procedure of average single fiber diameter of nonwoven fabric layer)
[0058] Step 1: A cross section in the thickness direction of the laminated nonwoven fabric is photographed using a scanning electron microscope (SEM) at a magnification such that the entire thickness direction of the laminated nonwoven fabric is within the photographing range.
[0059] Step 2: Apply the position information of the stacking interface obtained in the "stacking interface determination step" to the cross-sectional photograph obtained in step 1. The interval on the x-axis where the absolute value of Δy / Δx is greater than 0.30 in step 7 of the "stacking interface detection step" is used as the stacking interface interval, and the intervals divided by the stacking interface interval are used as the analysis intervals for each nonwoven fabric layer.
[0060] Step 3: Using the image analysis software, analyze the area Af (μm) formed by the cross-sectional profile of the single fiber in the analysis area of each nonwoven fabric layer determined in step 2. 2 ) is measured and the diameter of a perfect circle having the same area as the area Af is calculated. For this operation, 20 single fibers randomly selected from the same analysis interval are measured and the arithmetic mean is calculated in μm, with the second decimal place rounded off to the nearest integer, as the average single fiber diameter.
[0061] The average single fiber diameter Da of the thermoplastic resin fibers constituting the nonwoven fabric layer (A) is preferably 20.0 μm or less. By making Da 20.0 μm or less, more preferably 15.0 μm or less, the inter-fiber void size Ra of the nonwoven fabric layer (A) described later can be effectively reduced, and a suitable capillary force can be obtained. In addition, Da is preferably 2.0 μm or more. By making Da 2.0 μm or more, the inter-fiber void size Ra of the nonwoven fabric layer (A) can be suppressed from being extremely reduced, and the reduction of liquid permeability can be suppressed.
[0062] In the laminated nonwoven fabric of the present invention, in the nonwoven fabric layer (A), the inter-fiber void size Ra calculated by the following formula (1) is 200 μm or less.
[0063] Ra=(100×Ta×da) / (Wa×Da)-Da···Formula (1)
[0064] in,
[0065] Ta: Thickness of nonwoven fabric layer (A) (μm)
[0066] da: Density (dtex) of the thermoplastic resin fiber constituting the nonwoven fabric layer (A)
[0067] Wa: Weight per unit area of the nonwoven fabric layer (A) (g / m 2 )
[0068] Da: average single fiber diameter (μm) of the thermoplastic resin fibers constituting the nonwoven fabric layer (A).
[0069] The thickness of each nonwoven fabric layer was determined as follows.
[0070] (Measurement procedure of thickness of nonwoven fabric layer)
[0071] Step 1: The average single fiber diameters of the nonwoven fabric layer to be measured and the other nonwoven fabric layer stacked therewith obtained in the "step of measuring the average single fiber diameter of the nonwoven fabric layer" are added together and divided by 2 to calculate the average fiber diameters of the two layers. When another nonwoven fabric layer is stacked on the other side of the nonwoven fabric layer to be measured, the average single fiber diameters between the other nonwoven fabric layer are similarly added together and divided by 2 to calculate the average fiber diameters of the two layers.
[0072] Step 2: In the diagram obtained in step 6 of "Specific step of stacking interface", in the interval of the stacking interface between the nonwoven fabric layer to be measured for thickness and the other nonwoven fabric layers stacked therewith, determine the x coordinate when y is the average value of the fiber diameters of the two layers calculated in step 1.
[0073] Step 3: When other nonwoven fabric layers are stacked on both sides of the nonwoven fabric layer to be measured for thickness, the distance between the x coordinates when the average value of the fiber diameters of the two stacked layers is taken in the interval of the stacking interface on both sides is calculated as the thickness of the nonwoven fabric layer to be measured. When other nonwoven fabric layers are stacked on only one side of the nonwoven fabric layer to be measured for thickness, the distance between the x coordinate when the average value of the fiber diameters of the two layers is taken and the x coordinate of the surface exposed on the other side of the nonwoven fabric layer to be measured is calculated in the interval of the stacking interface as the thickness of the nonwoven fabric layer to be measured.
[0074] The thickness Tt of the laminated nonwoven fabric can be determined by calculating the distance between the x coordinates of both side surfaces of the laminated nonwoven fabric in step 3 of "step of measuring the thickness of the nonwoven fabric layer".
[0075] In addition, the fineness of the thermoplastic resin fibers constituting the nonwoven fabric layer is set to the value obtained by rounding off the second decimal place of the value calculated according to the following formula using the average single fiber diameter of the thermoplastic resin fibers and the density of the thermoplastic resin fibers measured in the "step for measuring the average single fiber diameter of the nonwoven fabric layer".
[0076] d=(π×ρ×D 2 ) / 400
[0077] in,
[0078] d: Density of thermoplastic resin fibers constituting the nonwoven fabric layer (dtex)
[0079] ρ: Density of thermoplastic resin fibers constituting the nonwoven fabric layer (g / cm 3 )
[0080] D: average single fiber diameter (μm) of the thermoplastic resin fibers constituting the nonwoven fabric layer.
[0081] The density ρ of thermoplastic resin fiber is the value measured based on "8.17.2 Density gradient tube method" of JIS L1013:2010 "Test methods for chemical filaments". A density gradient tube with an appropriately adjusted density range was prepared, and the fiber density (g / cm2) was measured for a fiber piece of about 0.1 g collected from the nonwoven fabric layer. 3 ) to the third decimal place. The same operation as above was performed on five different samples randomly collected from the nonwoven fabric layer, and the arithmetic average of the obtained results was calculated, and the value rounded off to the third decimal place was used as the density ρ (g / cm 3 ).
[0082] In addition, the certified unit area weight W (g / m 2 ) is calculated as follows.
[0083] First, the unit area weight Wt (g / m2) of the laminated nonwoven fabric was measured based on "6.2 Mass per unit area" of JIS L1913:2010 "General nonwoven fabric test methods". 2 Specifically, three test pieces of 20 cm × 25 cm in size cut from the laminated nonwoven fabric were collected for each 1 m sample width, and their respective masses (g) under the standard state were weighed. The average value of each piece was calculated as 2 The value obtained by rounding off the mass to the second decimal place is taken as the unit area weight Wt (g / m 2 ).
[0084] Next, using the thickness T of the nonwoven fabric layer and the thickness Tt of the laminated nonwoven fabric obtained in the above steps, the value calculated by the following formula is rounded off to the second decimal place as the nonwoven fabric layer identification unit area weight W (g / m 2 ).
[0085] W=W×T / Tt···formula.
[0086] The inter-fiber space size shown in formula (1) is a value indicating the length of one side of the space defined by the fibers when the fibers contained in the nonwoven fabric layer are arranged regularly in a lattice shape. The smaller the inter-fiber space size, the stronger the capillary force, and it is considered that the water suction force is improved.
[0087] In the laminated nonwoven fabric of the present invention, by making the inter-fiber void size Ra of the nonwoven fabric layer (A) with the smallest average single fiber diameter less than 200 μm, preferably less than 100 μm, and more preferably less than 80 μm, when liquid is dropped onto the outermost surface of the laminated nonwoven fabric, the capillary force of the nonwoven fabric layer (A) can be improved, more liquid is transferred to the nonwoven fabric layer (A), and good quick-drying properties are exhibited.
[0088] In addition, when the inter-fiber space size Ra is 30 μm or more, it is preferable in terms of ensuring a certain level of liquid permeability and water absorbency.
[0089] The inter-fiber void size Ra can be controlled by controlling the average single fiber diameter Da of the thermoplastic resin fibers constituting the nonwoven fabric layer.
[0090] The thickness of the nonwoven fabric layer (A) is preferably 100 μm or more. By making the thickness of the nonwoven fabric layer (A) 100 μm or more, more preferably 120 μm or more, more liquid absorbed by the laminated nonwoven fabric can be retained in the nonwoven fabric layer (A), and the water distribution ratio described later on the surface of the nonwoven fabric layer (A) can be increased.
[0091] On the other hand, the thickness of the nonwoven fabric layer (A) is preferably 1000 μm or less. When the thickness of the nonwoven fabric layer (A) is 1000 μm or less, it is possible to prevent liquid from accumulating inside the nonwoven fabric layer (A) and suppress liquid transfer between nonwoven fabric layers.
[0092] [Non-woven fabric layer (B)]
[0093] The nonwoven fabric layer (B) in the laminated stretch nonwoven fabric of the present invention is defined as a nonwoven fabric layer laminated in contact with the nonwoven fabric layer (A).
[0094] In the laminated nonwoven fabric of the present invention, for at least one of the nonwoven fabric layers (B) laminated in contact with the nonwoven fabric layer (A) (including the case where the nonwoven fabric layer (B) is laminated in contact with only one side of the nonwoven fabric layer (A), the ratio of the inter-fiber void size Rb (μm) calculated by the following formula (2) to the above-mentioned Ra (μm) is preferably 1.1 times or more.
[0095] Rb=(100×Tb×db) / (Wb×Db)-Db···Formula (2)
[0096] in,
[0097] Tb: Thickness of nonwoven fabric layer (B) (μm)
[0098] db: Density (dtex) of the thermoplastic resin fiber constituting the nonwoven fabric layer (B)
[0099] Wb: Weight per unit area of the nonwoven fabric layer (B) (g / m 2 )
[0100] Db: average single fiber diameter (μm) of the thermoplastic resin fibers constituting the nonwoven fabric layer (B).
[0101] In addition, Tb (μm), db (dtex), and Wb (g / m 2), Db (μm) is calculated as shown by the thickness T of the nonwoven fabric layer, the fineness d of the thermoplastic resin fibers constituting the nonwoven fabric layer, the recognized unit area weight W of the nonwoven fabric layer, and the average single fiber diameter D of the thermoplastic resin fibers constituting the nonwoven fabric layer.
[0102] By setting Rb / Ra to 1.1 times or more, more preferably 1.2 times or more, and even more preferably 1.5 times or more, moisture can be efficiently transferred to the nonwoven fabric layer (A) due to the large difference in capillary force between the nonwoven fabric layer (A) and the nonwoven fabric layer (B), thereby improving quick-drying properties.
[0103] On the other hand, if the ratio of Rb to Ra gradually increases, the proportion of inter-fiber voids in the nonwoven fabric layer (B) also increases. From the viewpoint of suppressing the uneven weight per unit area that occurs at this time and suppressing the reduction in strength starting from the uneven weight per unit area, Rb / Ra is preferably 10.0 times or less.
[0104] The inter-fiber void size Rb of the nonwoven fabric layer (B) is preferably 100 μm or more. When Rb is 100 μm or more, more preferably 120 μm or more, liquid permeability becomes good, so the amount of liquid remaining in the nonwoven fabric layer (B) is reduced, and quick-drying properties can be obtained.
[0105] The inter-fiber void size Rb of the nonwoven fabric layer (B) is preferably 500 μm or less. By setting Rb to 500 μm or less, it is possible to prevent the liquid transferred to the nonwoven fabric layer (A) from seeping out when a load is applied to the laminated nonwoven fabric, thereby maintaining a dry surface.
[0106] When the inter-fiber void size Rb (μm) in the nonwoven fabric layer (B) is controlled within the above range, the average single fiber diameter Db of the thermoplastic resin fibers constituting the nonwoven fabric layer (B) is preferably within a range of 15.0 μm to 30.0 μm.
[0107] The thickness of the nonwoven fabric layer (B) is preferably in the range of 100 to 1000 μm. By making the thickness of the nonwoven fabric layer (B) greater than 100 μm, it is possible to suppress the water distribution ratio described later from being increased due to the partial seepage of the water retained in the nonwoven fabric layer (A). In addition, by making the thickness of the nonwoven fabric layer (B) less than 1000 μm, the liquid absorbed from the nonwoven fabric layer (B) can be rapidly infiltrated into the nonwoven fabric layer (A).
[0108] [Laminated nonwoven fabric]
[0109] For the laminated nonwoven fabric of the present invention, when physiological saline is absorbed on both sides of the fabric by the following steps, it is preferred that the water distribution ratio defined by the following formula (3) is 40% or less on at least one of the four surfaces, namely, the surface absorbing the physiological saline, i.e., the absorption surface and the surface on the opposite side thereof.
[0110] (Measurement steps of water distribution ratio)
[0111] Step 1: Cut out a 5 cm x 5 cm sample from the laminated nonwoven fabric.
[0112] Step 2: Prepare two filter papers for each measurement. Cut two types of filter papers in accordance with JIS P3801 into 5 cm×5 cm pieces, and measure the mass of each piece.
[0113] Step 3: 0.250±0.005 mL of physiological saline solution was dripped onto the polypropylene film. At this time, the mass of the dripped physiological saline solution was measured in advance.
[0114] Step 4: The laminated nonwoven fabric is placed on the dripped physiological saline with the absorption surface absorbing the physiological saline facing downward, and kept for 1 minute.
[0115] Step 5: After the holding in step 4, remove the laminated nonwoven fabric from the polypropylene film, place it on the first sheet of filter paper with the absorbent surface facing upward, and quickly place the second sheet of filter paper on it.
[0116] Step 6: Apply pressure of 5 g / cm2 from above the second filter paper. 2 Place a 125g weight in the same way and keep it there for 1 minute.
[0117] Step 7: After the holding in step 6 above, remove the weight, measure the mass of each filter paper, and calculate the mass increase of each filter paper.
[0118] Step 8: Calculate the water distribution ratio of each surface in the laminated nonwoven fabric according to the following formula.
[0119] Water distribution ratio (%) = 100 × W1 / W0
[0120] in,
[0121] W0: The mass of the saline solution dripped in step 3 above (g)
[0122] W1: The increase in mass of the filter paper abutting against its surface in step 7 above (g).
[0123] The lower the water distribution ratio value obtained in the above steps, the less liquid is retained on the surface. That is, if the water distribution ratio is low at the surface that contacts the skin, even after absorbing liquid, a dry feeling can still be felt when touching.
[0124] In the laminated nonwoven fabric of the present invention, by setting the water distribution ratio of at least one of the four surfaces to 40% or less, more preferably 30% or less, and even more preferably 20% or less, the surface retains less moisture and can effectively maintain a dry surface.
[0125] In the laminated nonwoven fabric of the present invention, as a method for achieving the above-mentioned surface water distribution ratio, it is preferred to laminate the nonwoven fabric layer (B) on at least one outermost surface. That is, as described above, the nonwoven fabric layer (B) is defined as a nonwoven fabric layer laminated in contact with the nonwoven fabric layer (A), and therefore, in the laminated nonwoven fabric of the above-mentioned preferred embodiment, the laminated structure has the following from at least one side:
[0126] Non-woven fabric layer (B) / non-woven fabric layer (A)…
[0127] Moreover, as described above, since the nonwoven fabric layer (A) is defined as the layer with the smallest average single fiber diameter among the nonwoven fabric layers constituting the laminated nonwoven fabric, when liquid is absorbed from the outermost surface of the nonwoven fabric layer (B) having a larger average single fiber diameter, the liquid is quickly transferred to the nonwoven fabric layer (A) whose inter-fiber void size is controlled to be very small as described above, and therefore the water distribution ratio of the outermost surface of the nonwoven fabric layer (B) becomes smaller, thereby achieving quick-drying properties.
[0128] In addition, the laminated nonwoven fabric of the present invention preferably has a water distribution ratio of 50% or more on the opposite side of the surface having a water distribution ratio of 40% or less. By making the water distribution ratio 50% or more, more preferably 60% or more, the absorbed liquid will not be retained inside the laminated nonwoven fabric, and the liquid can be smoothly transferred from the surface absorbing the liquid to the other surface.
[0129] In the laminated nonwoven fabric of the present invention, in order to control the water distribution ratio of the surface opposite to the surface absorbing the liquid within the above range, it is preferred that the nonwoven fabric layer (A) having high capillary force is disposed on one surface.
[0130] It is preferred that the water absorption rate of the laminated nonwoven fabric of the present invention measured from at least one surface is 20 seconds or less.
[0131] The water absorption rate referred to herein is a value measured based on "7.1.1 Dropping method" of JIS L1907:2010 "Test method for water absorption of fiber products". One drop of water is dropped onto the laminated nonwoven fabric, and the time from absorption to disappearance of the mirror reflection on the surface is measured. The simple average of the values measured at 10 different locations is calculated in seconds, and the value obtained by rounding off the first decimal place is used as the water absorption rate referred to in the present invention.
[0132] The water absorption rate is 20 seconds or less, more preferably 10 seconds or less, which indicates that the performance of removing water adhering to the surface is good.
[0133] The weight per unit area of the laminated nonwoven fabric of the present invention is preferably 10 to 100 g / m 2 .
[0134] By setting the unit area weight to preferably 10 g / m 2 More preferably 13 g / m 2 More preferably, 15 g / m 2 On the other hand, by making the weight per unit area preferably 100 g / m 2 Below, more preferably 50g / m 2 As described below, it is possible to produce a laminated nonwoven fabric having moderate softness suitable for use as a nonwoven fabric for sanitary materials.
[0135] The laminated nonwoven fabric of the present invention is preferably formed by integrating the nonwoven fabric layers. Integration here means that the nonwoven fabric layers are joined by interweaving of fibers, fixation with components such as adhesives, or fusion of thermoplastic resins constituting the layers.
[0136] The laminated nonwoven fabric of the present invention may be provided with a hydrophilic agent for the purpose of further improving water absorption.
[0137] [Sanitary materials]
[0138] The sanitary material of the present invention has excellent water absorption and quick-drying properties because at least a part of the sanitary material is composed of the laminated nonwoven fabric of the present invention.
[0139] The sanitary material of the present invention can be suitably used for health-related purposes such as medical treatment and nursing care. The sanitary material of the present invention can be suitably used mainly for disposable articles, for example, paper diapers, sanitary napkins, gauze, bandages, masks, gloves, and band-aids.
[0140] Among them, it can be used as a component of various parts such as the surface sheet, back sheet, and side gathers in disposable diapers.
[0141] For the diaper as the sanitary material of the present invention, it is preferred that the surface sheet is composed of the laminated nonwoven fabric of the present invention. When the laminated nonwoven fabric of the present invention is used as the surface sheet of the diaper, when the nonwoven fabric layer (B) is used in a manner that the nonwoven fabric layer (B) is arranged on the skin side of the surface sheet, the urine discharged can be quickly absorbed and quickly transferred to the nonwoven fabric layer (A), so that the surface of the surface sheet can be kept dry.
[0142] In addition, for the diaper as a sanitary material of the present invention, it is also preferred that at least a part of the waist portion is composed of the laminated nonwoven fabric of the present invention. When the laminated nonwoven fabric of the present invention is used as a part of the waist portion of the diaper, when the nonwoven fabric layer (B) is used in a manner that the nonwoven fabric layer (B) is disposed on the skin side of the waist portion of the diaper, sweat can be quickly absorbed and quickly transferred to the nonwoven fabric layer (A), so that the surface of the waist portion can be kept dry.
[0143] In addition, the sanitary material of the present invention is also suitable for use as a mask. In the mask as the sanitary material of the present invention, it is preferred that the inner surface layer is composed of the laminated nonwoven fabric of the present invention. The so-called inner surface layer in the present invention refers to the layer closest to the mouth side in the surface body covering the mouth. When the laminated nonwoven fabric of the present invention is used in a manner in which the nonwoven fabric layer (B) is set to the skin side, even if sweat and exhaled breath condense and moisture adheres to the skin side, it can be immediately absorbed into the laminated nonwoven fabric, and the skin surface can be kept dry, so it can be used in a manner without discomfort when worn.
[0144] [Method for producing laminated nonwoven fabric]
[0145] Next, a preferred embodiment for producing the laminated nonwoven fabric of the present invention will be described in detail.
[0146] The production method of the nonwoven fabric layer (A) and the nonwoven fabric layer (B) constituting the laminated nonwoven fabric of the present invention can be selected from known production methods such as a spunbond method, a meltblown method, and a staple carding method.
[0147] Among them, the spunbond method is excellent in productivity and can be cited as a preferred method.
[0148] Hereinafter, a preferred embodiment of producing the laminated nonwoven fabric of the present invention by a spunbond method will be described, but the present invention is not limited thereto.
[0149] The spunbond method refers to a method for producing nonwoven fabrics that requires the following steps: a thermoplastic resin as a raw material is melted, spun from a spinneret, and then cooled and solidified. The yarn obtained is pulled and stretched by an ejector and captured on a moving net to form a nonwoven fiber web, which is then thermally bonded.
[0150] The shapes of the spinneret and the ejector used may be various shapes such as circular and rectangular. Among them, the combination of a rectangular die and a rectangular ejector is preferred because the amount of compressed air used is small and the yarns are not easily welded or rubbed.
[0151] The spinning temperature in the present invention is preferably set to (melting temperature of the raw material thermoplastic resin + 10°C) or higher and (melting temperature of the raw material thermoplastic resin + 100°C) or lower. By setting the spinning temperature within the above range, a stable molten state can be formed, and excellent spinning stability can be obtained.
[0152] In addition, when manufacturing the nonwoven fabric layer (A), the average inter-fiber space can be reduced by reducing the fiber diameter. Therefore, in order to stably manufacture fine fibers, the melt viscosity of the polymer used in the nonwoven fabric layer (A) is preferably 100 Pa·s or less, more preferably 50 Pa·s or less.
[0153] The melt viscosity of the polymer referred to here is measured by using a vacuum dryer to reduce the moisture content to 200 ppm or less, and changing the strain rate in stages to measure the sheet polymer. The strain rate is 1216 s when the measurement temperature is set to the same as the spinning temperature. -1 The value at time.
[0154] The spun yarn is then cooled, and methods for cooling the spun yarn include, for example, a method of forcibly blowing cold air to the yarn, a method of naturally cooling the yarn using the ambient temperature around the yarn, and a method of adjusting the distance between the spinneret and the ejector, and a method combining these methods may also be used. In addition, the cooling conditions may be appropriately adjusted and adopted in consideration of the discharge amount per single hole of the spinneret, the spinning temperature, the ambient temperature, and the like.
[0155] Next, the cooled and solidified sliver is pulled and stretched by compressed air injected from an injector.
[0156] In the laminated nonwoven fabric of the present invention, the average inter-fiber space size of the nonwoven fabric layer (A) and the nonwoven fabric layer (B) can be controlled by the diameter of the constituent fibers.
[0157] The diameter of the fiber is determined by the discharge amount of each discharge hole of the spinneret and the pulling speed, that is, the spinning speed. Therefore, it is preferred to determine the discharge amount and the spinning speed in a manner that can control the diameter to obtain the desired inter-fiber space size.
[0158] The spinning speed is preferably 2000 m / min or more. By setting the spinning speed to 2000 m / min or more, more preferably 3000 m / min or more, high productivity is achieved, and the fiber orientation and crystallization proceed, thereby obtaining high-strength long fibers.
[0159] The long fiber sliver stretched by the pulling is collected on a moving net to form a sheet, and then supplied to a thermal bonding process.
[0160] The laminated nonwoven fabric of the present invention is laminated with a nonwoven fabric layer. As a method for laminating the nonwoven fabric layer, for example, the following method can be adopted: on the nonwoven fabric layer obtained by capturing the thermoplastic resin fiber on the capturing net by the spunbonding method as described above, the next nonwoven fabric layer obtained by the spunbonding method is continuously captured in an on-line manner, and the lamination is integrated; the two or more nonwoven fabric layers (A) obtained separately are superimposed on each other in an off-line manner, and the lamination is integrated by thermal compression bonding, etc. Among them, the method of continuously capturing the next nonwoven fabric layer in an on-line manner on the nonwoven fabric layer, and laminating and integrating by thermal bonding is a preferred method due to its excellent productivity.
[0161] As a method for integrating the nonwoven fabric layers with each other by thermal bonding to form the laminated nonwoven fabric of the present invention, a method of thermal bonding using various rollers such as a heat embossing roller with engravings (concavoconvex parts) applied on the surface of each of the upper and lower pairs of rollers, a heat embossing roller composed of a combination of a roller with a flat (smooth) surface and a roller with engravings (concavoconvex parts) applied on the surface of the other roller, and a heat calendering roller composed of a combination of an upper and lower pair of flat (smooth) rollers, or a method based on thermal pressure bonding such as ultrasonic bonding using ultrasonic vibration of a horn to perform heat fusion bonding. In addition, as a method of integrating the laminated nonwoven fabric layers of the present invention by thermal bonding, the so-called air-through method, which is a method of blowing hot air, can also be cited.
[0162] Among them, the method of thermal bonding using a pair of upper and lower heat rolls is preferred because the nonwoven fabric layer (A) can be made dense and the size of inter-fiber gaps can be reduced by bonding the laminated nonwoven fabrics while compressing them.
[0163] When the laminated nonwoven fabric of the present invention is produced by thermal compression bonding using heated rolls, it is preferred that the linear pressure applied to the laminated nonwoven fabric between the rolls be 100 N / cm or more because the nonwoven fabric layer (A) can be sufficiently dense.
[0164] In the laminated nonwoven fabric, it is preferred that the surface closer to the nonwoven fabric layer (A) than the nonwoven fabric layer (B) is processed by a flat roll and the surface on the opposite side is processed by a heat embossing roll on which engraving is performed. By adopting such a combination of rolls, the nonwoven fabric layer (B) is less likely to be compressed relative to the nonwoven fabric layer (A), so that the difference in the size of the inter-fiber gaps between the nonwoven fabric layer (A) and the nonwoven fabric layer (B) can be ensured to be large.
[0165] The laminated nonwoven fabric of the present invention may also be provided with a hydrophilic agent before winding. As a method for providing the laminated nonwoven fabric with a hydrophilic agent, coating with a kiss roller, spraying, or dipping can be cited. Coating with a kiss roller is preferred from the perspective of uniformity and ease of controlling the amount of adhesion.
[0166] Example
[0167] The present invention is described in detail below based on examples. However, the present invention is not limited to these examples. It should be noted that in the measurement of various physical properties, unless otherwise specified, the measurement is based on the above-mentioned method.
[0168] (1) Determination of stacking interface
[0169] The lamination interface of the laminated nonwoven fabric was determined by the aforementioned "lamination interface determination step." It should be noted that "nano3DX" manufactured by RIGAKU Co., Ltd. was used as a high-resolution three-dimensional X-ray microscope. The resolution was 0.6 μm / voxel.
[0170] (2) Average single fiber diameter
[0171] The average single fiber diameter of each nonwoven fabric layer was measured by the aforementioned "Measuring procedure of average single fiber diameter of nonwoven fabric layer." It should be noted that "S-5500" manufactured by Hitachi High-Technologies Corporation was used as a scanning electron microscope (SEM), and "WinROOF2015" manufactured by Mitani Shoji Co., Ltd. was used as image analysis software.
[0172] (3) Average single fiber diameter during the manufacturing process of laminated nonwoven fabric
[0173] For each thermoplastic resin fiber, a fiber sample was randomly collected from the nonwoven fiber web collected on the net, and an image of the cross section of the fiber was taken at a magnification that enables observation of a single fiber using a scanning electron microscope "S-5500" manufactured by Hitachi High-Technologies Corporation. Then, "WinROOF2015" manufactured by Mitani Shoji Co., Ltd. was used as image analysis software and the measurement was performed as described above.
[0174] The average single fiber diameter during the production of the laminated nonwoven fabric was measured, and it was confirmed that in the present embodiment and comparative example, an average single fiber diameter that was no different from that measured by the above-mentioned "step for measuring the average single fiber diameter of the nonwoven fabric layer" was obtained.
[0175] (4) Thickness
[0176] The thickness of the laminated nonwoven fabric and each nonwoven fabric layer is measured by the aforementioned "step of measuring the thickness of the nonwoven fabric layer".
[0177] The thickness obtained by a simple method
[0178] An image of a cross section perpendicular to the machine direction of the laminated nonwoven fabric was taken with a scanning electron microscope (S-5500 manufactured by Hitachi High-Technologies Corporation) at a magnification sufficient to observe the thickness. The thickness of the laminated nonwoven fabric and each nonwoven fabric layer was measured based on the taken image.
[0179] The thickness of the laminated nonwoven fabric and each nonwoven fabric layer obtained by the simple method was measured, and it was confirmed that in the present Example and Comparative Example, a thickness equal to that measured by the above-mentioned "nonwoven fabric layer thickness measurement procedure" was obtained.
[0180] (6) Size of inter-fiber gaps
[0181] The inter-fiber space size of the nonwoven fabric layer was calculated by the following formula.
[0182] R=(100×T×d) / (W×D)-D
[0183] in,
[0184] T: Thickness of nonwoven fabric layer (μm) Measured by the above (4).
[0185] d: Fineness (dtex) of the thermoplastic resin fibers constituting the nonwoven fabric layer. The fineness is measured according to the definition of d described above.
[0186] W: Weight per unit area of nonwoven fabric layer (g / m 2 ). The measurement was performed according to the above-mentioned definition of W. It should be noted that it was confirmed that there was no difference in the basis weight between the present embodiment and the comparative example and the nonwoven fiber web layer described later.
[0187] D: Average single fiber diameter (μm) of the thermoplastic resin fibers constituting the nonwoven fabric layer. Measured by the above (2).
[0188] (7) Water distribution ratio
[0189] The water distribution ratios of both sides of the laminated nonwoven fabrics were measured by the aforementioned "water distribution ratio measurement step". In the present embodiment and comparative example, the side after the nonwoven fabric layer (B) was arranged on the outermost surface was used as the "absorption side" in step 4 of the "water distribution ratio measurement step". In addition, the number of samples was set to 5, and the arithmetic average was calculated, and the first decimal place was rounded off.
[0190] (8) Water absorption speed
[0191] The water absorption rate is measured according to "7.1.1 Drop method" of JIS L1907:2010 "Test method for water absorption of textile products". One drop of water is dropped onto the laminated nonwoven fabric, and the time from absorption to disappearance of the mirror reflection on the surface is measured. The simple average of the values measured at 10 different locations is calculated in seconds, and the first decimal place is rounded off.
[0192] (9) Water absorption and quick drying
[0193] For the laminated nonwoven fabric after the water distribution ratio was measured in (7) above, healthy general adults (15 men and 15 women, a total of 30 people) touched the "absorption surface" with their hands and evaluated the dryness of the surface according to the following three levels. For each nonwoven fabric, the average score of the evaluation results was calculated as the skin touch of the laminated nonwoven fabric.
[0194] 5: The surface feels dry and no moisture is felt
[0195] 3: Although there is no water on the surface, it is moist
[0196] 1: The surface is moist and wet
[0197] [Example 1]
[0198] (Non-woven fiber web layer (A))
[0199] Polypropylene (PP, melt viscosity 30Pa·s) was melted by an extruder and spun out from a rectangular die at a single hole discharge rate of 0.30g / min. After the spun yarn was cooled and solidified, it was pulled and stretched in a rectangular ejector by compressed air at a pressure of 0.10MPa, and captured on a moving net to obtain a nonwoven fiber web layer (A) by a spunbond method. The average single fiber diameter of the fibers constituting the obtained nonwoven fiber web layer (A) was 10.6μm. In addition, the unit area weight was 35.0g / m 2 .
[0200] (Non-woven fiber mesh layer (B))
[0201] The polypropylene (PP) which is the same raw material as that used in the nonwoven fiber web layer (A) is melted by an extruder and spun out from a rectangular die at a single hole discharge rate of 0.85 g / min. After the spun yarn is cooled and solidified, it is pulled and stretched in a rectangular ejector by compressed air with an ejector pressure of 0.08 MPa, and captured on the nonwoven fiber web layer (A) on a moving net, and a nonwoven fiber web layer (B) is obtained by a spunbond method. The average single fiber diameter of the fibers constituting the obtained nonwoven fiber web layer (B) is 20.4 μm. In addition, the unit area weight is 30.0 g / m 2 .
[0202] The nonwoven web layer (B) is collected on the nonwoven web layer (A) and laminated in-line to obtain a laminated web having a two-layer structure of nonwoven web layer (A) / nonwoven web layer (B).
[0203] (Laminated non-woven fabric)
[0204] The obtained laminated fiber web was thermally bonded at a linear pressure of 300 N / cm and a thermal bonding temperature of 125°C using an embossing roll having a pair of upper and lower heating mechanisms, wherein a metal embossing roll having perfectly circular protrusions arranged alternately at the same pitch in both the MD and CD directions was used as the upper roll, and a metal flat roll was used as the lower roll. Subsequently, a hydrophilic treatment was performed to obtain a fiber web having a unit weight of 65.0 g / m 2 Laminated non-woven fabric.
[0205] The obtained laminated nonwoven fabric was evaluated for the thickness of each layer, the size of the inter-fiber gap, the water distribution ratio, the water absorption speed, and the water absorption quick-drying property. The thickness of the nonwoven fabric layer (A) was 300 μm, and the size of the inter-fiber gap was 54 μm. The thickness of the nonwoven fabric layer (B) was 420 μm, and the size of the inter-fiber gap was 181 μm. The results are shown in Table 1.
[0206] [Example 2]
[0207] A laminated nonwoven fabric was obtained in the same manner as in Example 1 except that the single hole discharge rate was 0.80 g / min in the step of obtaining the nonwoven fiber web layer (A) and that the single hole discharge rate was 1.20 g / min in the step of obtaining the nonwoven fiber web layer (B). The evaluation results of the obtained laminated nonwoven fabric are shown in Table 1.
[0208] [Example 3]
[0209] The evaluation results of the obtained laminated nonwoven fabric are shown in Table 1, except that the single hole discharge rate was 0.35 g / min in the step of obtaining the nonwoven fiber web layer (B).
[0210] [Example 4]
[0211] The nonwoven fiber web layer (A) had a unit area weight of 15.0 g / m 2 , the unit area weight of the nonwoven fiber web layer (B) is set to 13.0 g / m 2 , except for this, a laminated nonwoven fabric was obtained in the same manner as in Example 1. Table 1 shows the evaluation results of the obtained laminated nonwoven fabric.
[0212] [Example 5]
[0213] The nonwoven fiber web layer (A) had a unit area weight of 10.0 g / m 2 , except for this, a laminated nonwoven fabric was obtained in the same manner as in Example 1. Table 1 shows the evaluation results of the obtained laminated nonwoven fabric.
[0214] [Example 6]
[0215] (Non-woven fiber web layer (A))
[0216] In the same manner as in Example 1, a nonwoven fiber web layer (A) was obtained.
[0217] (Non-woven fiber mesh layer (B))
[0218] A nonwoven fiber web layer (B) was obtained in the same manner as in Example 1 except that the drawn and stretched yarn was directly captured on the moving net.
[0219] After the nonwoven web layer (A) and the nonwoven web layer (B) are obtained separately, they are laminated by an off-line operation to obtain a laminated web having a two-layer structure of nonwoven web layer (A) / nonwoven web layer (B).
[0220] (Laminated non-woven fabric)
[0221] The obtained laminated fiber web was thermally bonded and subjected to a hydrophilic treatment in the same manner as in Example 1 to obtain a laminated nonwoven fabric. Table 1 shows the evaluation results of the obtained laminated nonwoven fabric.
[0222] [Example 7]
[0223] The polymer used in the nonwoven fabric layer (A) and the nonwoven fabric layer (B) was polyethylene glycol copolymerized polyethylene terephthalate (copolymerized PET, the copolymerization ratio of polyethylene glycol was 8% by mass of the polymer).
[0224] (Non-woven fiber web layer (A))
[0225] As the raw material polymer of the fiber, 8% by mass of the polymer was copolymerized with polyethylene glycol (co-PET). The nonwoven fiber web layer (A) was obtained in the same manner as in Example 1 except that the copolymerized PET was used and the web travel speed was changed. The average single fiber diameter of the fibers constituting the obtained spunbonded nonwoven fabric layer (A) was 8.5 μm. In addition, the unit area weight was 30.0 g / m 2 .
[0226] (Non-woven fiber mesh layer (B))
[0227] The nonwoven fiber web layer (B) was obtained in the same manner as in Example 1 except that the same copolymer PET as the raw material used in the nonwoven fiber web layer (A) was used. The properties of the fibers constituting the obtained spunbonded nonwoven fabric layer (B) were as follows: the average single fiber diameter was 17.5 μm. The weight per unit area was 30.0 g / m 2 37.0g / m 2 .
[0228] (Laminated non-woven fabric)
[0229] The laminated nonwoven fabric was obtained by the same method as in Example 1 except that the thermal bonding temperature was set to 200°C. The thickness of the nonwoven fabric layer (A) was 270 μm, and the inter-fiber gap size was 73 μm. The thickness of the nonwoven fabric layer (B) was 350 μm, and the inter-fiber gap size was 158 μm. The evaluation results of the obtained laminated nonwoven fabric are shown in Table 1.
[0230] [Comparative Example 1]
[0231] In the process of obtaining the nonwoven fiber web layer (A), the unit discharge amount was set to 1.20 g / min, the ejector pressure was set to 0.08 MPa, and in the process of obtaining the nonwoven fiber web layer (B), the single hole discharge amount was set to 1.20 g / min. A laminated nonwoven fabric was obtained in the same manner as in Example 1. The average single fiber diameter of the fibers constituting the obtained nonwoven fiber web layer (A) was 22.0 μm. In addition, the thickness of the nonwoven fabric layer (A) was 430 μm, and the inter-fiber gap size was 245 μm. The evaluation results of the obtained laminated nonwoven fabric are shown in Table 1.
[0232] [Table 1]
[0233]
[0234] As shown in Table 1, Examples 1 to 7 are excellent in water absorption and quick drying. In particular, Examples 1 and 6 both achieve high levels of water absorption speed and water absorption and quick drying. On the other hand, Comparative Example 1 has low water absorption and quick drying.
Claims
1. A laminated nonwoven fabric, comprising a laminated nonwoven fabric comprising nonwoven fabric layers containing thermoplastic resin fibers, wherein in a nonwoven fabric layer A having the smallest average single fiber diameter among the nonwoven fabric layers, a fiber interspace size Ra calculated by the following formula (1) is 200 μm or less, wherein the unit of Ra is μm, Ra=(100×Ta×da) / (Wa×Da)-Da···Formula (1) in, Ta: thickness of nonwoven fabric layer A, in μm da: The fineness of the thermoplastic resin fiber constituting the nonwoven fabric layer A, in dtex Wa: Weight per unit area of nonwoven fabric layer A, in g / m 2 Da: average single fiber diameter of the thermoplastic resin fibers constituting the nonwoven fabric layer A, in μm, For at least one of the nonwoven fabric layers B laminated in contact with the nonwoven fabric layer A, a ratio Rb / Ra of the inter-fiber void size Rb calculated by the following formula (2) to the Ra is greater than 1.1, where the unit of Rb is μm, and the nonwoven fabric layer B is laminated on the outermost surface in contact with the liquid on at least one side of the laminated nonwoven fabric, Rb=(100×Tb×db) / (Wb×Db)-Db···Formula (2) in, Tb: thickness of nonwoven fabric layer B, in μm db: The fineness of the thermoplastic resin fiber constituting the nonwoven fabric layer B, in dtex Wb: Weight per unit area of nonwoven fabric layer B, in g / m 2 Db: average single fiber diameter of the thermoplastic resin fibers constituting the nonwoven fabric layer B, in μm, When physiological saline is absorbed on both sides of the laminated nonwoven fabric by the following steps, at least one of the four surfaces, namely, the surface absorbing the physiological saline and the surface on the opposite side thereof, has a water distribution ratio defined by the following formula (3) of 40% or less. Step 1: Cut a 5 cm × 5 cm sample from the laminated nonwoven fabric; Step 2: Prepare 2 pieces of filter paper in accordance with JIS P3801 for each measurement. Cut the filter paper into 5 cm x 5 cm pieces and measure the mass of each piece. Step 3: drip 0.250±0.005 mL of saline onto the polypropylene film. At this time, measure the mass of the saline dripped in advance. Step 4: Place the laminated nonwoven fabric on the dripped saline with the absorption surface of the saline facing downward, and keep it for 1 minute; Step 5: After the step 4, the laminated nonwoven fabric is removed from the polypropylene film, and is placed on the first sheet of the filter paper with the absorption surface facing upward, and the second sheet of the filter paper is quickly placed thereon; Step 6: Apply pressure of 5 g / cm2 from above the second filter paper. 2 Place a 125g weight in the same way and keep it there for 1 minute; Step 7: After the step 6 is maintained, the weight is removed, the mass of each filter paper is measured, and the mass increment of each filter paper is calculated; Step 8: Calculate the water distribution ratio of each surface in the laminated nonwoven fabric according to the following formula; Water distribution ratio (%) = 100 × W1 / W0 in, W0: The mass of the saline solution dripped in step 3, in g W1: the mass increase of the filter paper abutting against its surface in step 7, in g.
2. The laminated nonwoven fabric according to claim 1, wherein: The water distribution ratio of the surface opposite to the surface having the water distribution ratio of 40% or less is 50% or more.
3. The laminated nonwoven fabric according to claim 1 or 2, wherein: On at least one surface, the water absorption rate measured by the dropping method according to JIS L1907:2010 is 20 seconds or less.
4. A sanitary material, at least a part of which is composed of the laminated nonwoven fabric according to any one of claims 1 to 3.
5. The sanitary material according to claim 4, wherein The sanitary material is a diaper.
6. The sanitary material according to claim 5, wherein The surface sheet is composed of the laminated nonwoven fabric.
7. The sanitary material according to claim 5, wherein At least a part of the waist region is formed of the laminated nonwoven fabric.
8. The sanitary material according to claim 5, wherein The sanitary material is a mask, and the inner surface layer of the mask is composed of the laminated non-woven fabric.
Citation Information
Patent Citations
Surface material of absorbent products
JP1995178133A
Layered nonwoven cloth, method for manufacturing same, absorbent article, and sweat-absorbing sheet
CN110325678A
Nonwoven fabric to be used as surface material of sanitary material
JP1995042057A
Composite nonwoven fabric
JP2004299356A
Filter material for air filter and air filter
JP2012125714A