A kind of inorganic fiber of uniform phase, barium aluminum borosilicate optical glass and preparation method thereof

Through spinning process and staged heat treatment, combined with fluxing components and clarification components, the problem of uneven raw material components during the high-temperature melting process of barium aluminum borosilicate glass is solved, and high uniformity and permeability of the finished glass are achieved. degree, meeting the demand for high-quality glass in the dental field.

CN115403261BActive Publication Date: 2024-10-01LIAONING UPCERA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211124453.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-15
Publication Date
2024-10-01
Estimated Expiration
2042-09-15

AI Technical Summary

Technical Problem

During the high-temperature melting process of barium aluminum borosilicate glass, differences in fluidity of raw material components lead to uneven mixing, resulting in poor quality and performance stability of the finished product.

Method used

The spinning process is used to mix glass raw materials, solvents and polymer additives to form a glass precursor solution. The fiber membrane is made through the spinning process and is heat treated in stages. The use of fluxing components and clarification components is combined to improve Uniformity and transparency of the glass melting process.

Benefits of technology

It effectively improves the uniformity and transparency of the finished glass, enhances the heat resistance and specific gravity of barium aluminum borosilicate glass, ensures the high quality and stable performance of the finished product, and is suitable for filler glass in the dental field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003847836650000081
    Figure BDA0003847836650000081
  • Figure BDA0003847836650000091
    Figure BDA0003847836650000091
  • Figure BDA0003847836650000101
    Figure BDA0003847836650000101
Patent Text Reader

Abstract

The present invention relates to the field of dental materials, and specifically to a uniform phase inorganic fiber, barium aluminum borosilicate optical glass and a preparation method. Specifically, it comprises: mixing glass raw materials, solvents and polymer additives to obtain a glass precursor solution, spinning the glass precursor solution into a fiber film, and then heat-treating the fiber film to obtain inorganic fibers; wherein, in the glass raw materials, the mass ratio of barium oxide, aluminum oxide, boron oxide and silicon dioxide is (5-40): (5-20): (5-20): (20-65) in terms of elemental oxides; the polymer additive is selected from one or more of polyvinyl alcohol, polyvinyl pyrrolidone, polyvinyl alcohol butyral ester and polyacrylonitrile. The preparation method of barium aluminum borosilicate optical glass provided by the present invention can effectively solve the problem of uneven components of finished glass, and better meet the application requirements of dental filler glass.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of dental materials, and in particular to a uniform phase inorganic fiber, barium aluminum borosilicate optical glass and a preparation method thereof. Background Art

[0002] High-transmittance optical barium aluminum borosilicate optical glass can be used as lenses and reflectors and is widely used in optoelectronics, aerospace and other fields. In addition, as a mother glass, it is also an important source of downstream high-transmittance glass powder. For example, in the field of dentistry, barium aluminum borosilicate glass can block X-rays and has good optical transmittance, which makes barium aluminum borosilicate glass have important applications in dental filling powder materials.

[0003] At present, glass compositions are mostly made by powder melting method, but the raw material powders are prone to agglomeration and uneven mixing, which can easily lead to uneven elemental composition of the powder.

[0004] Compared with conventional glass, barium aluminoborosilicate glass is more difficult to melt due to the large differences in melting points, particle sizes and weights of the raw material components. During the high-temperature melting process, different components of the raw materials have different fluidities in different temperature zones, and the time it takes for the quality and composition of the glass to reach a molten state is also different, resulting in uneven mixing of the raw materials, which in turn makes the quality and performance stability of the finished glass poor. Summary of the invention

[0005] The purpose of the present invention is to provide a uniform phase inorganic fiber, barium aluminum borosilicate optical glass and a preparation method to overcome the problem of poor quality and performance stability of finished products caused by uneven raw materials of barium aluminum borosilicate optical mother glass.

[0006] In order to achieve the above-mentioned object, in a first aspect, the present invention first provides a method for preparing an inorganic fiber, comprising: mixing glass raw materials, a solvent and a polymer additive to obtain a glass precursor solution, spinning the glass precursor solution into a fiber membrane through a spinning process, and then heat-treating the fiber membrane to obtain an inorganic fiber;

[0007] Among them, in the glass raw materials, the mass ratio of barium oxide, aluminum oxide, boron oxide and silicon dioxide is (5-40): (5-20): (5-20): (20-65) in terms of elemental oxides; the polymer additive is selected from one or more of PVA (polyvinyl alcohol), PVP (polyvinyl pyrrolidone), PVB (polyvinyl butyral), PVP (polyvinyl pyrrolidone), PAN (polyacrylonitrile) and PVP (polyvinyl pyrrolidone).

[0008] In the field of dentistry, the introduction of barium components is often difficult. In addition to the high melting point of the barium source compound barium carbonate and the abnormally violent reaction of barium hydroxide due to the presence of crystal water, the most important reason is that the density of the barium source compound is much higher than that of other powders. After the conventional mixing process, the material is very easy to be stratified, resulting in uneven distribution of raw material components. However, the present application found that the spinning process can expand the selection of barium sources to almost all soluble barium source compounds, and further found that under the aforementioned system, not only can the barium source stratification problem be avoided, but also the problems of incompatibility, slight solubility and solution turbidity of the components can be effectively improved, which greatly improves the uniformity and high transparency of the glass precursor solution, thereby improving the quality of barium aluminum borosilicate optical glass, which is more conducive to its application in the field of dentistry.

[0009] Preferably, the solvent is one or more of water, ethanol, dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF) and N,N-dimethylacetamide (DMAC).

[0010] More preferably, when the solvent is water, the polymer auxiliary agent is PVA (polyvinyl alcohol) and / or PVP (polyvinyl pyrrolidone);

[0011] When the solvent is ethanol, the polymer auxiliary agent is PVB (polyvinyl butyral) and / or PVP (polyvinyl pyrrolidone);

[0012] When the solvent is dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF) or N,N-dimethylacetamide (DMAC), the polymer auxiliary agent is PAN (polyacrylonitrile) and / or PVP (polyvinyl pyrrolidone).

[0013] Preferably, the mass ratio of the glass raw material to the solvent is (0.2-1.6):1, and more preferably the mass ratio is (0.5-1.6):1.

[0014] Preferably, the mass ratio of the solvent to the polymer auxiliary agent is (4-20):1, and more preferably the mass ratio is (4-10):1.

[0015] The present invention finds that the combination of the glass raw material, solvent and polymer additive is conducive to achieving high uniformity and high transparency of the glass precursor solution, and can also make it solidify quickly, thereby improving the quality of the spun fiber.

[0016] Preferably, in the glass raw material, the mass ratio of barium oxide, aluminum oxide, boron oxide and silicon dioxide, calculated as elemental oxides, is (10-30): (5-20): (5-20): (35-60).

[0017] Preferably, based on the total weight of oxides of various elements in the glass raw material, the content of silicon dioxide and aluminum oxide is 40-65 wt %.

[0018] Preferably, in the glass raw material, the mass ratio of boron trioxide to silicon dioxide is 0.05-0.35, preferably 0.1-0.35; the mass ratio of barium oxide to boron trioxide is 0.5-7, preferably 0.5-2.

[0019] The present invention unexpectedly discovered that, in glass raw materials, when the relationship between the components is within the above dosage range, the heat resistance and specific gravity of the glass can be effectively improved, while taking into account the uniformity of the raw materials and improving the overall performance of the final glass product.

[0020] Preferably, the dispersion is a dispersion of an organic metal salt and / or a metal oxide.

[0021] Preferably, the barium source is a water-soluble barium salt and / or a barium base, preferably one or more of barium hydroxide, barium chloride and barium nitrate; the silicon source is an organic silicate, preferably a silicate salt, more preferably tetraethyl orthosilicate and / or ethyl orthosilicate; the aluminum source is a hydrated acid, a hydrated base and a nitrate of aluminum, preferably one or more of aluminum hydroxide, aluminic acid and aluminum nitrate; and the boron source is boric acid.

[0022] Preferably, an acid is added to the glass precursor solution, and the acid is one or more of hydrochloric acid, nitric acid, acetic acid and oxalic acid.

[0023] More preferably, the pH value of the glass precursor solution is 2-6, and more preferably the pH value is 3-5.

[0024] The present application has found that, in the glass precursor solution system, when the pH is within the above range, the high uniformity and high transparency of the solution can be better ensured.

[0025] Preferably, the viscosity of the glass precursor solution is in the range of 200 to 20000 mPa·s, preferably 800 to 5000 mPa·s. The above viscosity range can not only better maintain the smoothness and stability of wire drawing, but more importantly, can effectively promote the solution system to achieve high uniformity.

[0026] In the present invention, extremely high requirements are placed on raw material purity and equipment control.

[0027] Preferably, the iron content in the barium aluminum borosilicate glass raw material is less than 1000ppm, preferably less than 300ppm. When the iron content is lower than the above range, the high light transmittance of the product can be guaranteed. In addition, the part of the equipment in contact with the material in the technical solution of the present invention does not contain any metal components, which can better improve the product color and achieve high transparency.

[0028] Preferably, the glass precursor solution is stirred at a stirring speed of 20 to 2000 r / min, preferably 200 to 1000 r / min; and the stirring time is greater than 2 h.

[0029] In the present invention, the spinning process includes pouring the glass precursor solution into a flat-head syringe to solidify it into filaments.

[0030] Preferably, the spinning process is electrospinning or centrifugal spinning, more preferably electrospinning.

[0031] Preferably, the electrospinning conditions include: static voltage of 5 to 30 kV, preferably 20 to 30 kV; receiving distance from receiving plate to needle of 2 to 35 cm, preferably 15 to 20 cm; propulsion speed of 0.1 to 10 ml / h, preferably 0.6 to 3 ml / h.

[0032] Preferably, the centrifugal spinning conditions are: a rotation speed of 300 to 500 r / min, and a receiving distance from the receiving plate to the needle head of 10 to 30 cm.

[0033] Preferably, the heat treatment is performed at 200-1400°C.

[0034] Preferably, the heat treatment is carried out in two stages;

[0035] The first stage is carried out at 600-1300°C, and the treatment time of the first stage is 1-10 hours; more preferably, the treatment time of the first stage is 2-5 hours;

[0036] The second stage is carried out at 200-900° C., and the treatment time of the second stage is 5-200 hours; more preferably, the treatment time of the second stage is 10-50 hours.

[0037] The present application found that when the fiber membrane is directly heat treated, the effect is not ideal. When the above-mentioned staged heat treatment is adopted, the temperature and time defined in the first stage are more conducive to the formation of oxide components of related elements, and the temperature and time defined in the second stage are more conducive to reducing the content of carbon and excess organic matter in the raw materials; the above two-stage heat treatment can promote the formation of homogeneous phase glass raw material oxides, thereby improving the quality of barium aluminum borosilicate glass.

[0038] In a second aspect, the present invention further provides an inorganic fiber, which is prepared by the above preparation method.

[0039] In a third aspect, the present invention further provides an optical glass prepared from the inorganic fiber.

[0040] In a fourth aspect, the present invention further provides a method for preparing the optical glass, comprising: preparing inorganic fibers using the above-mentioned preparation method, and then preparing optical glass from the inorganic fibers, specifically comprising the following steps:

[0041] (1) mixing and grinding the inorganic fiber, flux component and clarifying component so that the fiber diameter is 0.2 to 100 μm, preferably 0.7 to 50 μm;

[0042] The fluxing component is one or more of sodium salt, potassium salt, sodium oxide and potassium oxide; the amount of the fluxing component is 0.1-5wt% of the inorganic fiber, preferably 0.5-3wt%;

[0043] The clarification component is an oxide clarifier, a sulfate clarifier, a halide clarifier or a composite clarifier, preferably arsenic pentoxide and / or ammonium nitrate, and the amount of the clarification component is 0.1 to 10 wt %, preferably 1 to 5 wt % of the inorganic fiber;

[0044] (2) melting the ground fiber in step (1) at 1200 to 1800° C., preferably 1400 to 1700° C., for 0.5 to 24 hours, preferably 1 to 24 hours, to obtain glass liquid;

[0045] (3) cooling the molten glass after melting in step (2) to obtain mother glass;

[0046] Wherein, the mother glass is a non-shaped mother glass, and the cooling process is rapid cooling by low-temperature airflow or low-temperature liquid; the low-temperature liquid is liquid nitrogen, water or quenching oil;

[0047] The mother glass is a formed mother glass; the cooling process comprises: after the glass liquid is injected into the mold, it is first cooled to 400-800°C, preferably 500-650°C, and the heat preservation time is 3-120 minutes; then it is cooled to room temperature at 1°C / min and demolded.

[0048] In the specific implementation process, those skilled in the art can select grinding equipment and high-temperature furnace according to actual conditions. Grinding equipment includes dry grinding equipment such as disc grinder, air flow mill, mortar grinder, or wet grinding equipment such as high-energy ball mill, sand mill; high-temperature furnace includes high-temperature heating equipment such as box muffle furnace, glass frit furnace, lifting furnace or rotary furnace that can reach a specified temperature.

[0049] The present invention finds that the selection and dosage of the fluxing component and the clarifying component can better adjust the state of the glass liquid during melting, improve the glass melting point and the bubble degree and transparency of the formed glass product. At the same time, the fiber membrane is ground and crushed together with the fluxing component and the clarifying component under the above conditions to further obtain glass melting raw materials with uniform particle size, thereby improving the quality of the finished glass product.

[0050] During the specific implementation process, technicians in this field can select a cooling process according to the actual needs of the terminal.

[0051] As a preferred embodiment of the present invention, the method for preparing the barium aluminum borosilicate optical glass comprises:

[0052] (1) Preparation of precursor sol

[0053] The glass raw material is mixed with a solvent, a polymer additive and an acid and stirred to obtain a glass precursor solution; the viscosity of the glass precursor solution is 800 to 5000 mPa·s;

[0054] Calculated as elemental oxides, the mass ratio of barium oxide, aluminum oxide, boron oxide and silicon dioxide is (10-30): (5-20): (5-20): (35-60);

[0055] When the solvent is water, the polymer additive is polyvinyl alcohol and / or polyvinyl pyrrolidone; when the solvent is ethanol, the polymer additive is polyvinyl butyral ester and / or polyvinyl pyrrolidone; when the solvent is one or more of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, the polymer additive is polyacrylonitrile and / or polyvinyl pyrrolidone;

[0056] The pH value of the glass precursor solution is 3-5.

[0057] (2) Spinning solidification

[0058] The glass precursor solution is subjected to electrostatic spinning; the electrostatic voltage is 20-30 kV; the receiving distance from the receiving plate to the needle is 15-20 cm; the propulsion speed is 0.6-3 ml / h, and then a fiber membrane is obtained.

[0059] (3) Heat treatment of fiber membrane

[0060] The fiber membrane is placed in a high-temperature furnace for heat treatment, and the heat treatment is carried out in two stages; wherein the first stage is carried out at 600-1300°C, and the treatment time of the first stage is 2-5 hours; the second stage is carried out at 200-900°C, and the treatment time of the second stage is 10-50 hours; after natural cooling, it is taken out to obtain inorganic fibers.

[0061] (4) Blending and crushing

[0062] The cooled inorganic fiber is mixed with a fluxing component and a clarifying component and ground; the diameter of the ground fiber is 0.7 to 50 μm; the fluxing component is one or more of sodium salt, potassium salt, sodium oxide and potassium oxide, and the amount of the fluxing component accounts for 0.5 to 3 wt% of the inorganic fiber; the clarifying component is arsenic pentoxide and / or ammonium nitrate, and the amount of the clarifying component accounts for 0.1 to 10 wt%, preferably 1 to 5 wt%, of the inorganic fiber.

[0063] (5) Glass melting

[0064] The ground fibers are melted at 1400-1700° C. to obtain molten glass.

[0065] (6) Glass molding

[0066] The molten glass is cooled according to the needs of different finished products.

[0067] Based on the above technical solution, the beneficial effects of the present invention are as follows:

[0068] The preparation method of the barium aluminum borosilicate optical glass provided by the present invention can effectively solve the problems of uneven components and low transparency of the finished glass, thereby obtaining a highly uniform and highly transparent barium aluminum borosilicate glass product, and the quality and performance of the finished product are stable, which can better meet the application requirements of dental filler glass. DETAILED DESCRIPTION

[0069] The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.

[0070] Example 1 An inorganic fiber and a method for preparing the same

[0071] This embodiment provides an inorganic fiber, which is prepared by the following preparation method, and the specific steps are as follows:

[0072] 180.3002g of tetraethyl orthosilicate, 45.9592g of aluminum nitrate, 57.6077g of barium nitrate, 98.6018g of boric acid, 20ml of 80% acetic acid aqueous solution, 50g of water, 400g of ethanol and 100g of PVB were mixed and stirred for 24 hours. The viscosity was tested to be 4518mPa·s to obtain a glass precursor solution. The above glass precursor solution was poured into a 1L centrifugal spinning device, the speed was adjusted to 400r / min, the receiving distance was 20cm, the device was operated, and the fiber membrane on the receiving plate was collected. The collected fiber membrane was placed in a box-type muffle furnace, treated at 650℃ for 18h, and taken out after natural cooling.

[0073] Embodiment 2 An optical glass and its preparation method

[0074] This embodiment first provides an optical glass, which is prepared from the inorganic fiber described in Example 1, and subjected to scanning electron microscope EDS energy spectrum component analysis, and energy spectrum points are taken at 7 random positions. The results are shown in Table 1.

[0075] Table 1

[0076]

[0077] (Note: Boron is a light element and cannot be reflected in the energy spectrum)

[0078] This embodiment further provides a method for preparing the above optical glass, comprising: preparing inorganic fibers using the preparation method described in Embodiment 1, and then preparing optical glass from the inorganic fibers, specifically comprising the following steps:

[0079] 1 kg of the inorganic fiber in Example 1, 16 g of sodium hydroxide and 22 g of arsenic pentoxide were placed in a mortar grinding device and ground for 1 hour. Then, they were placed in a box furnace and melted at 1420°C for 24 hours. Finally, the melted glass liquid was poured into a container with nitrogen gas at 0°C supplied by a circulating air cooler and taken out after 20 minutes.

[0080] Example 3 An inorganic fiber and its preparation method

[0081] This embodiment provides a method for preparing inorganic fiber, which is prepared by the following preparation method, and the specific steps are as follows:

[0082] 138.6925g tetramethyl silicate, 7.6505g aluminum hydroxide, 61.7226g barium hydroxide octahydrate, 54.7788g boric acid, 10g oxalic acid, 100g water and 400g DMF were mixed, stirred for 2h, 50g PAN was added, and stirred for another 24h. The viscosity was tested to be 1782mPa·s to obtain a glass precursor solution. The above glass precursor solution was poured into a 50ml syringe, a 21G Ruhr interface flat needle was used, the static voltage was 30kV, the receiving distance from the receiving plate to the needle was 20cm, the propulsion speed was 2ml / h, and the fiber membrane on the receiving plate was collected. Then the above fiber membrane was placed in a box-type muffle furnace, treated at 750℃ for 48h, and taken out after natural cooling.

[0083] This embodiment further provides inorganic fibers prepared by the above preparation method.

[0084] Embodiment 4 An optical glass and its preparation method

[0085] This embodiment first provides an optical glass, which is prepared from the inorganic fiber described in Example 3, and performs scanning electron microscope EDS energy spectrum component analysis, and energy spectrum points are taken at 7 random positions. The results are shown in Table 2.

[0086] Table 2

[0087]

[0088] (Note: Boron is a light element and cannot be reflected in the energy spectrum)

[0089] This embodiment further provides a method for preparing the above optical glass, comprising: preparing inorganic fibers using the preparation method described in Embodiment 3, and then preparing optical glass from the inorganic fibers, specifically comprising the following steps:

[0090] 500g of the inorganic fiber in Example 3, 17g of potassium carbonate and 12.4g of arsenic pentoxide were placed in a disc grinder for grinding at a rotation speed of 120r / min, and the material particle size tested was 57.879μm; then placed in a 200ml crucible, the crucible was placed in a lifting furnace, and melted at 1550℃ for 5h; finally, the molten glass liquid was poured into -200℃ liquid nitrogen, and taken out after 1min to obtain an unformed mother glass.

[0091] Example 5 An inorganic fiber and its preparation method

[0092] The present embodiment provides an inorganic fiber, which is prepared by the following preparation method, and the specific steps are as follows: 138.6925g of tetraethyl orthosilicate, 83.5622g of aluminum nitrate, 34.0899g of barium nitrate, 219.1152g of boric acid, 200g of 0.1M / L hydrochloric acid, and 300g of ethanol are mixed, stirred for 2h, 50g of PVA is added, and stirred for another 24h. The viscosity is tested to be 2000mPa·s to obtain a glass precursor solution. The above glass precursor solution is poured into a 50ml syringe, a 21G Ruhr interface flat needle is used, the static voltage is 20kV, the receiving distance from the receiving plate to the needle is 15cm, the propulsion speed is 1ml / h, and the fiber film on the receiving plate is collected. Then the above fiber film is placed in a box-type muffle furnace, treated at 600°C for 24h, and taken out after natural cooling.

[0093] This embodiment further provides inorganic fibers prepared by the above preparation method.

[0094] Example 6 An optical glass and its preparation method

[0095] This example first provides an optical glass, which is prepared from the inorganic fiber described in Example 5, and subjected to scanning electron microscope EDS energy spectrum component analysis, and energy spectrum points are taken at 7 random positions. The results are shown in Table 3.

[0096] Table 3

[0097]

[0098] (Note: Boron is a light element and cannot be reflected in the energy spectrum)

[0099] This embodiment further provides a method for preparing the above optical glass, comprising: preparing inorganic fibers using the preparation method described in Embodiment 5, and then preparing optical glass from the inorganic fibers, specifically comprising the following steps:

[0100] 500g of the inorganic fiber in Example 5, 17g of potassium carbonate and 12.4g of arsenic pentoxide were placed in a disc grinder for grinding at a rotation speed of 120r / min, and the material particle size tested was 57.879μm; then placed in a 200ml crucible, the crucible was placed in a lifting furnace, and melted at 1550℃ for 5h; finally, the molten glass liquid was poured into -200℃ liquid nitrogen, and taken out after 1min to obtain an unformed mother glass.

[0101] 5 kg of the inorganic fiber in Example 5, 100 g of sodium carbonate and 168 g of arsenic pentoxide were placed in an air flow grinding device and ground for 1 hour, the frequency of the classifying wheel was 47 Hz, and the material particle size test was 6.231 μm; then placed in a 3L glass frit furnace and melted at 1490°C for 5 hours; the discharge port of the glass frit furnace was opened, and injected into a 10 cm*10 cm*10 cm graphite mold, and immediately transferred to a box furnace after the injection molding was completed, the temperature was set to 600°C, and kept warm for 1 hour, and then cooled to room temperature at a rate of 1°C / min for demolding, to obtain a formed mother glass product.

[0102] Comparative Example 1

[0103] The preparation method of the inorganic fiber in this comparative example is the same as that in Example 3, and the optical glass is the same as that in Example 4, the only difference being that the amount of barium hydroxide octahydrate used in the raw material is 270 g.

[0104] The prepared optical glass was subjected to scanning electron microscope EDS energy spectrum component analysis, and energy spectrum points were taken at 7 random positions. The results are shown in Table 4.

[0105] Table 4

[0106]

[0107] (Note: Boron is a light element and cannot be reflected in the energy spectrum)

[0108] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A method for preparing inorganic fiber, characterized in that: include: A glass precursor solution is obtained by mixing glass raw materials, a solvent and a polymer additive, the glass precursor solution is made into a fiber membrane by a spinning process, and then the fiber membrane is heat-treated to obtain an inorganic fiber; Wherein, in the glass raw material, the mass ratio of barium oxide, aluminum oxide, boron oxide and silicon dioxide, calculated as element oxides, is (5-40): (5-20): (5-20): (20-65); When the solvent is water, the polymer additive is polyvinyl alcohol and / or polyvinyl pyrrolidone; when the solvent is ethanol, the polymer additive is polyvinyl butyral ester and / or polyvinyl pyrrolidone; when the solvent is one or more of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, the polymer additive is polyacrylonitrile and / or polyvinyl pyrrolidone; The heat treatment is carried out in two stages; The first stage is carried out at 600-1300 °C, and the treatment time of the first stage is 1-10 h; The second stage is carried out at 200~900 ℃, and the processing time of the second stage is 5~200 h.

2. The method for preparing inorganic fiber according to claim 1, characterized in that: The mass ratio of the solvent to the polymer additive is (4-20):1; And / or, the mass ratio of the glass raw material to the solvent is (0.2-1.6):

1.

3. The method for preparing inorganic fiber according to claim 1, characterized in that: In the glass raw material, the mass ratio of barium oxide, aluminum oxide, boron oxide and silicon dioxide is (10-30): (5-20): (5-20): (35-60) in terms of elemental oxides.

4. The method for preparing inorganic fiber according to claim 3, characterized in that: Based on the total weight of oxides of each element in the glass raw material, the content of silicon dioxide and aluminum oxide is 40-65wt%.

5. The method for preparing inorganic fiber according to any one of claims 1 to 4, characterized in that: The mass ratio of boron trioxide to silicon dioxide is 0.05-0.35, and the mass ratio of barium oxide to boron trioxide is 0.5-7.

6. The method for preparing inorganic fiber according to any one of claims 1 to 4, characterized in that: In the glass precursor solution, the barium source is a water-soluble barium salt and / or a barium base; the silicon source is an organic silicate; the aluminum source is a hydrated acid, a hydrated base and a nitrate of aluminum; and the boron source is boric acid; And / or, the iron content in the glass raw material is less than 1000 ppm.

7. The method for preparing inorganic fiber according to claim 6, characterized in that: The barium source is one or more of barium hydroxide, barium chloride and barium nitrate; the silicon source is silicate; and the aluminum source is one or more of aluminum hydroxide, aluminic acid and aluminum nitrate.

8. The method for preparing inorganic fiber according to claim 6, characterized in that: The silicon source is ethyl orthosilicate and / or ethyl orthosilicate.

9. The method for preparing inorganic fiber according to claim 6, characterized in that: The iron content in the glass raw material is less than 300 ppm.

10. The method for preparing inorganic fiber according to any one of claims 1 to 4, characterized in that: In the glass precursor solution, the barium source is one or more of barium hydroxide, barium chloride and barium nitrate; the silicon source is tetraethyl orthosilicate and / or ethyl orthosilicate; the aluminum source is one or more of aluminum hydroxide, aluminic acid and aluminum nitrate; and the boron source is boric acid.

11. The method for preparing inorganic fiber according to any one of claims 1 to 4, characterized in that: The glass precursor solution further contains an acid, which is one or more of hydrochloric acid, nitric acid, acetic acid and oxalic acid.

12. The method for preparing inorganic fiber according to claim 11, characterized in that: The pH value of the glass precursor solution is 2-6.

13. The method for preparing inorganic fiber according to claim 11, characterized in that: The pH value of the glass precursor solution is 3-5.

14. The method for preparing inorganic fiber according to any one of claims 1 to 4, characterized in that: The viscosity of the glass precursor solution is 200-20000 mPa·s.

15. The method for preparing inorganic fiber according to claim 14, characterized in that: The viscosity of the glass precursor solution is 800-5000 mPa·s.

16. The method for preparing inorganic fiber according to any one of claims 1 to 4, characterized in that: The spinning process is electrostatic spinning or centrifugal spinning.

17. The method for preparing inorganic fiber according to claim 16, characterized in that: The conditions for the electrospinning are: an electrostatic voltage of 5 to 30 kV; a receiving distance from the receiving plate to the needle of 2 to 35 cm; and a propulsion speed of 0.1 to 10 ml / h.

18. The method for preparing inorganic fiber according to claim 17, characterized in that: The conditions for the electrospinning are: an electrostatic voltage of 20-30 kV; a receiving distance from the receiving plate to the needle of 15-20 cm; and a propulsion speed of 0.6-3 ml / h.

19. The method for preparing inorganic fiber according to claim 16, characterized in that: The centrifugal spinning conditions are: a rotation speed of 300-500 r / min, and a receiving distance from the receiving plate to the needle head of 10-30 cm.

20. An inorganic fiber, characterized in that Prepared by the preparation method according to any one of claims 1 to 19.

21. An optical glass, characterized in that: Prepared from the inorganic fiber described in claim 20.

22. A method for preparing optical glass, characterized in that: include: Inorganic fibers are prepared using the preparation method described in any one of claims 1 to 19, and then optical glass is prepared from the inorganic fibers.

23. The method for preparing optical glass according to claim 22, characterized in that: The steps include: (1) mixing and grinding the inorganic fiber, the flux component and the clarifying component so that the fiber diameter is 0.2-100 μm; Wherein, the fluxing component is one or more of sodium salt, potassium salt, sodium oxide and potassium oxide, and the amount of the fluxing component accounts for 0.1-5 wt% of the inorganic fiber; The clarification component is an oxide clarifier, a sulfate clarifier, a halide clarifier or a composite clarifier, and the amount of the clarification component is 0.1-10 wt % of the inorganic fiber; (2) melting the ground fiber in step (1) at 1200-1800° C. for 0.5-24 h to obtain glass liquid; (3) cooling the glass liquid melted in step (2) to obtain mother glass; Wherein, when the mother glass is an unformed mother glass, the cooling process is rapid cooling by low-temperature airflow or low-temperature liquid; the low-temperature liquid is liquid nitrogen, water or quenching oil; When the mother glass is a formed mother glass, the cooling process includes: after the glass liquid is injected into the mold, it is first cooled to 400-800°C; the heat preservation time is 3-120 min; then it is cooled to room temperature at 1°C / min and demolded.

24. The method for preparing optical glass according to claim 23, characterized in that: The steps include: (1) mixing and grinding the inorganic fiber, the flux component and the clarifying component so that the fiber diameter is 0.7-50 μm; Wherein, the fluxing component is one or more of sodium salt, potassium salt, sodium oxide and potassium oxide, and the amount of the fluxing component accounts for 0.5-3 wt% of the inorganic fiber; The clarifying component is arsenic pentoxide and / or ammonium nitrate, and the amount of the clarifying component accounts for 1-5wt% of the inorganic fiber; (2) melting the ground fiber in step (1) at 1400-1700° C. for 1-24 h to obtain glass liquid; (3) cooling the glass liquid melted in step (2) to obtain mother glass; Wherein, when the mother glass is an unformed mother glass, the cooling process is rapid cooling by low-temperature airflow or low-temperature liquid; the low-temperature liquid is liquid nitrogen, water or quenching oil; When the mother glass is a formed mother glass, the cooling process includes: after the glass liquid is injected into the mold, it is first cooled to 500-650°C; the heat preservation time is 3-120 min; and then cooled to room temperature at 1°C / min, and demolded.