By preparing a highly sensitive palladium diselenide film on a flexible substrate and combining it with polymer encapsulation materials, the problem of insufficient sensitivity of traditional strain sensors in monitoring fine deformations is solved, achieving high sensitivity, stability and low-cost large-scale Production and integration applications.
Patent Information
- Application Number
- CN202211039782.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-08
- Filing Date
- 2022-08-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-08-29
AI Technical Summary
Existing traditional metal-based strain sensors have insufficient sensitivity when monitoring subtle deformations (such as pulses), and the material preparation process is complex and costly, making it difficult to mass-produce and integrate applications.
A flexible substrate, magnetron sputtering or thermal evaporation method is used to prepare a palladium diselenide film, combined with plasma enhanced chemical vapor deposition technology to form a highly sensitive strain sensor, and polymer packaging materials are used to improve the stability and durability of the device. .
It achieves highly sensitive monitoring of fine deformation, reduces the complexity and cost of the preparation process, simplifies the production process, is suitable for large-scale integration applications, and has good durability and environmental stability.
Smart Images

Figure CN115420189B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of strain sensor devices, and in particular relates to a flexible strain sensor for human health monitoring and a preparation method thereof. Background Art
[0002] Flexible wearable devices are one of the important trends in the development of electronic devices. In particular, wearable electronic devices that are used for the huge clinical diagnosis and health assessment needs of human vital signs monitoring have attracted much attention due to their convenience and non-invasive advantages. Among them, strain sensors are devices that convert tensile or compressive strain into resistance changes. Flexible strain sensors are widely used in flexible wearable electronic devices. Generally, excellent flexible strain sensors have high gauge factors (GF), environmentally stable materials, and good durability. At the same time, they have the advantages of small size and easy integration and carrying. However, traditional metal-based strain sensors are limited by their poor sensitivity and it is difficult to monitor subtle deformations (such as pulse). Therefore, excellent nano-scale flexible materials are often used in flexible strain sensors, such as carbon nanotubes (CNTs), graphene, metal nanowires, etc. Although these devices have high performance, the material preparation process and device structure are often complex, costly, and difficult to mass produce and integrate for application. Summary of the invention
[0003] The purpose of the present invention is to provide a flexible strain sensor for human health monitoring and a preparation method thereof, which has the advantages of large GF, high sensitivity to monitor subtle deformation, good stability, good durability, simple preparation process, and easy large-scale production and integration.
[0004] In order to achieve the above object, the technical solution adopted by the present invention is:
[0005] Provided is a flexible strain sensor for human health monitoring, comprising (from bottom to top): a flexible substrate, a palladium diselenide film, a metal electrode, and a polymer encapsulation passivation film.
[0006] The flexible substrate of the flexible strain sensor for human health monitoring is PI, and the thickness of the substrate is 5-500 microns.
[0007] The palladium diselenide film is obtained by magnetron sputtering or thermal evaporation depositing a metal palladium film on the substrate and then performing plasma enhanced chemical vapor deposition selenization. The thickness of the palladium diselenide film is 2-50 nanometers.
[0008] The electrodes are metal electrodes or ITO electrodes, the length of the channel between the electrodes is 1-500 microns, and the thickness of the electrodes is 30-500 nanometers.
[0009] The packaging material is polymethyl methacrylate (PMMA), PI, and Parylene-C.
[0010] The method for preparing the flexible strain sensor for human health monitoring comprises the following steps:
[0011] Step 1: A palladium film is formed on a substrate by using vacuum coating technology such as magnetron sputtering or thermal evaporation, and the palladium film is selenized by plasma enhanced chemical vapor deposition to obtain a palladium diselenide film layer;
[0012] Step 2: Use photolithography and metal mask to form a two-terminal electrode structure, and use vacuum coating technology to plate metal electrodes or ITO electrodes on the palladium diselenide thin film layer;
[0013] Step 3: Spin-coat a layer of PMMA, PI, and Parylene-C film on the palladium diselenide film layer to encapsulate it into a flexible strain sensor for human health monitoring.
[0014] The method for preparing the flexible strain sensor for human health monitoring, the specific process of step 1 is:
[0015] Step 1-1 Magnetron sputtering method: Place the flexible substrate in a magnetron sputtering chamber, use metal palladium as the target material, and control the background vacuum of the chamber to be less than 8×10 -4 Pa, introducing argon gas with a flow rate of 30-150 sccm, a radio frequency power of 10-150 watts, a sputtering pressure of 1-10 Pa, sputtering for 0.5-6 minutes, and obtaining a palladium film sputtered on the substrate with a thickness of 2-15 nanometers;
[0016] Thermal evaporation method: The flexible substrate is placed in a thermal evaporation chamber, and metal palladium particles (purity 99.99%) are used as the evaporation material. The background vacuum of the chamber is controlled to be less than 1×10 -4 Pa, the thermal evaporation rate is controlled to be 0.3-2 angstroms / second, and the sputtering is performed for 1-10 minutes to obtain a palladium film sputtered on a flexible substrate with a thickness of 2-15 nanometers.
[0017] Step 1-2 plasma enhanced chemical vapor deposition method: the palladium film obtained in step 1-1 is placed in a quartz tube of a tubular furnace of an inductively coupled plasma generating device, the air pressure in the quartz tube is evacuated to a vacuum degree of 1-5Pa, and argon gas is injected into the front end of the tubular furnace, and its flow rate is controlled to be 5-25sccm; selenium powder (purity 99.9%) is placed upstream of the palladium film (10 cm away from the palladium film), the central area of the tubular furnace is raised from room temperature to 250°C within 20 minutes, the plasma is turned on, the radio frequency source power is 200-400 watts, the temperature is maintained for 30-120 minutes, and then the temperature is naturally lowered to obtain a palladium diselenide film.
[0018] The specific process of step 2 is as follows:
[0019] Step 2: Thermal evaporation of metal electrodes: Place the palladium diselenide film prepared in step 1 in a thermal evaporation chamber and control the background vacuum to be less than 1×10 -4 Pa, firstly evaporating indium / bismuth / chromium with a thickness of 5-20 nanometers, then evaporating gold / silver with a thickness of 30-500 nanometers, and controlling the width of the metal channel to 1-500 micrometers by metal mask or photolithography to obtain a metal electrode;
[0020] ITO electrode plating by magnetron sputtering: Place the palladium diselenide film prepared in step 1 in a magnetron sputtering chamber, use ITO as the target material, and control the background vacuum to be less than 8×10 -4 Pa, introduce argon gas with a flow rate of 50-150sccm, control the pressure in the chamber to be 1-10Pa, set the RF power to 100-200 watts, and the sputtering time to 0.5-4 hours. The thickness of ITO prepared by sputtering is 200-500 nanometers.
[0021] The specific process of step 3 is as follows:
[0022] Step 3: Spin coating packaging: Place the device prepared in step 2 on a spin coater, drop PMMA on the palladium diselenide film, and turn on the spin coater at a speed of 600-4000 rpm;
[0023] Spin coating PI: refer to the above steps;
[0024] Parylene-C deposition: Place it in the parylene vacuum chemical vapor deposition system to deposit a 5-50 micron film; after completion, it is packaged to prepare a stable flexible strain sensor for human health monitoring.
[0025] The present invention has the following advantages:
[0026] (1) The present invention selects palladium diselenide, a two-dimensional material with excellent mechanical properties and good environmental stability, as the strain material; it has a high GF, and therefore has high sensitivity, good stability and good durability as a flexible strain sensor for human health monitoring.
[0027] (2) The present invention prepares the palladium diselenide thin film by first using magnetron sputtering or thermal evaporation vacuum coating to prepare the palladium thin film, and then selenizing the palladium thin film; this method is simple, the film thickness is controllable, and a uniform thin film can be prepared over a large area without introducing other impurity ions and organic solvents. Then, the film is selenized by PECVD. This process has the advantages of low synthesis temperature, can be grown directly on a flexible substrate (PI), uniform film, clean surface, and fast synthesis speed.
[0028] (3) The flexible strain sensor for human health monitoring prepared by the present invention has a simple overall structure, a simple process, no need to transfer materials, and is easy to integrate. The device has low power consumption, high sensitivity, stable performance, and good durability, which is convenient for large-scale industrial production and has great application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a schematic diagram of the device structure provided by the present invention.
[0030] Figure 2 The Raman spectrum image of the prepared palladium diselenide film provided by the present invention.
[0031] Figure 3 A wrist activity monitoring diagram of the flexible strain sensor for human health monitoring provided by the present invention.
[0032] Figure 4 A pulse monitoring diagram of the flexible strain sensor for human health monitoring provided by the present invention.
[0033] Figure 5 7000 durability cycle tests of the flexible strain sensor for human health monitoring provided by the present invention. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the present invention more clear, the technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments of the present invention.
[0035] Example 1
[0036] A flexible strain sensor for human health monitoring includes a PI substrate, a palladium diselenide thin film layer on the PI substrate, and an indium-gold electrode plated on the palladium diselenide thin film layer; the palladium diselenide thin film layer has a thickness of 8 nanometers; the electrode is an indium-gold electrode, the electrode spacing is 20 micrometers, and the electrode thickness is 60 nanometers.
[0037] The preparation method of the above-mentioned flexible strain sensor for human health monitoring is:
[0038] (1) The PI substrate (thickness 50 μm) was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 5 minutes respectively, and then dried with nitrogen gas;
[0039] (2) The PI substrate processed in step (1) is placed in a magnetron sputtering vacuum chamber with the PI surface facing the target; a metal palladium target with a purity of 99.99% is placed on the corresponding target position, and the pressure in the vacuum chamber is pumped down to 1×10 -3Pa; introduce 100 sccm of argon, adjust the RF power of the RF source to 20 watts, adjust the air pressure in the vacuum chamber to 4 Pa by controlling the valve, and turn off the RF source after sputtering for 1 minute to obtain a palladium film sputtered on the PI substrate with a thickness of 4 nanometers.
[0040] (3) placing the PI substrate sputtered with the metal palladium film in step (2) in the central area of the PECVD tube furnace, placing 1 gram of selenium powder with a purity of 99.9% in a quartz boat, and placing the quartz boat upstream of the quartz tube (10 cm away from the palladium film); extracting the remaining air in the quartz tube by a mechanical pump, and then passing 250 sccm of argon gas to clean the quartz tube for 20 minutes, and adjusting the argon gas flow rate to 10 sccm after 20 minutes; turning on the tube furnace for heating, raising the temperature of the center of the furnace body to 250° C. within 20 minutes, and then turning on the RF power supply, adjusting the power to 400 watts, generating plasma and keeping it warm for 30 minutes; then cooling the product to room temperature by natural cooling to obtain a palladium diselenide film covering the PI substrate; Figure 2 This is a Raman spectrum image of a palladium diselenide thin film prepared in an embodiment of the present invention;
[0041] (4) The palladium diselenide film prepared in step (3) is placed on a thermal evaporation tray, the metal mask is fixed on the palladium diselenide film, and then placed in a thermal evaporation chamber, and the vacuum pressure is pumped to 1×10 -5 Pa, and then evaporate indium and gold with thicknesses of 8 nanometers and 50 nanometers respectively, to prepare a palladium diselenide device with a channel of 20 microns.
[0042] (5) Place the device prepared in step (4) on a spin coater, spin-coat PMMA on the device channel for encapsulation at a speed of 1500 rpm for 1 minute, and then place the device on a heating table at 80 degrees Celsius for drying for 5 minutes. Thus, a flexible strain sensor for human health monitoring is prepared.
[0043] The flexible strain sensor for human health monitoring prepared by the present invention is attached to the wrist for testing, and the following is obtained by moving the wrist up and down: Figure 3 As shown in the wrist activity monitoring diagram, the flexible strain sensor for human health monitoring can well reflect the resistance change signal caused by the bending and stretching strain of the material caused by the wrist movement, so the device can be used as a sensor for human movement. In addition, the device is attached to the pulse of the arm, and the test results are as follows Figure 4 As shown in the pulse monitoring diagram, it can be seen that the strain sensor has excellent sensitivity for weak vibration monitoring and can clearly reflect the human pulse signal, which is of great significance for promoting the automation and intelligence of human health monitoring.
[0044] Implementation Case 2
[0045] A flexible strain sensor for human health monitoring comprises a PI substrate, a palladium diselenide thin film layer on the PI substrate, and an ITO electrode plated on the palladium diselenide thin film layer; the palladium diselenide thin film layer has a thickness of 20 nanometers; the electrode is an ITO electrode, the electrode spacing is 30 micrometers, and the electrode thickness is 400 nanometers.
[0046] The preparation method of the above-mentioned flexible strain sensor for human health monitoring is:
[0047] (1) PI (thickness 100 μm) was ultrasonically cleaned in acetone, anhydrous ethanol, and deionized water for 5 min respectively, and then dried with nitrogen;
[0048] (2) Place the PI substrate processed in step (1) in a thermal evaporation vacuum chamber, and pump the pressure in the vacuum chamber to 5×10 -5 Pa; adjusting the thermal evaporation rate of palladium to 0.8 angstroms / second, evaporating for 2 minutes to obtain a palladium film sputtered on the PI substrate with a thickness of 10 nanometers;
[0049] (3) Place the PI substrate on which the metal palladium film is sputtered in step (2) in the central area of a PECVD tube furnace, place 2 g of selenium powder with a purity of 99.9% in a quartz boat, and place the quartz boat upstream of the quartz tube (10 cm away from the palladium film); extract the remaining air in the quartz tube by a mechanical pump, then introduce 250 sccm of argon gas to clean the quartz tube for 20 minutes, and after 20 minutes, adjust the argon gas flow rate to 7 sccm; turn on the tube furnace for heating, raise the temperature of the center of the furnace body to 250°C within 20 minutes, then turn on the RF power supply, adjust the power to 400 watts, generate plasma and keep it warm for 60 minutes; then cool the product to room temperature by natural cooling to obtain a palladium diselenide film on the PI substrate.
[0050] (4) The palladium diselenide film prepared in step (3) is placed in a magnetron sputtering chamber through a mold mask electrode pattern, and the vacuum pressure is pumped to 1×10 -3 Pa, and then ITO is used as the target material, argon gas is introduced with a flow rate of 80sccm, the pressure in the chamber is controlled to be 5Pa, the RF power is set to 150 watts, the sputtering time is 3 hours, and the thickness of the sputtered ITO electrode is 400 nanometers.
[0051] (5) The device prepared in step (4) is placed on a spin coater, and PMMA is spin-coated on the device channel for encapsulation at a rotation speed of 2000 rpm for 1 min. The device is then placed on a heating table at 80 degrees Celsius for drying for 5 minutes, thereby preparing a flexible strain sensor for human health monitoring.
[0052] The flexible strain sensor for human health monitoring prepared by the present invention was placed on a compression and tension test device driven by a stepper motor, and 7000 stretching cycles were set to measure the following Figure 5 The 7000 durability cycle test shown in the figure shows the tensile cycle signal from 3500s to 3520s during the test. Figure 5 It can be shown that the strain sensor has excellent durability.
Claims
1. Application of a flexible sensor in strain detection, characterized in that The flexible sensor comprises, from bottom to top: (1) a flexible polyimide (PI) polymer substrate, (2) a palladium diselenide thin film, (3) an electrode, and (4) a polymer film packaging layer; the palladium diselenide thin film layer is obtained by magnetron sputtering or thermal evaporation of a metal palladium thin film on the flexible polyimide (PI) polymer substrate, and then selenizing it by plasma enhanced chemical vapor deposition (PECVD), and the thickness of the palladium diselenide thin film is 2-50 nanometers.
2. The application of a flexible sensor in strain detection according to claim 1 is characterized in that: The thickness of the flexible polyimide (PI) polymer substrate is 5-500 microns.
3. The application of a flexible sensor in strain detection according to claim 1 is characterized in that: The electrodes are metal electrodes or indium tin oxide (ITO), the length of the channel between the electrodes is 1-500 microns, and the thickness of the electrodes is 30-500 nanometers.
4. The application of a flexible sensor in strain detection according to claim 1 is characterized in that: The packaging layer material is polymethyl methacrylate (PMMA) or PI or Parylene-C.
5. Application of the flexible sensor according to any one of claims 1 to 4 in strain detection, characterized in that: The method for preparing the flexible sensor comprises the following steps: Step 1: A palladium film is formed on the substrate by magnetron sputtering or thermal evaporation vacuum coating technology, and the palladium film is then selenized by PECVD to obtain a palladium diselenide film layer; Step 2: Use photolithography and metal mask to form a two-terminal electrode structure, and use vacuum coating technology to plate metal electrodes or ITO electrodes on the palladium diselenide thin film layer; Step 3: Spin-coat a layer of PMMA or PI, or deposit Parylene-C on the PdSe thin film layer to encapsulate it into a flexible strain sensor for human health monitoring.
6. The application of the flexible sensor in strain detection according to claim 5 is characterized in that: The specific process of step 1 in the method for preparing the flexible sensor is as follows: (1) Preparation of metal palladium film by magnetron sputtering or thermal evaporation: The palladium film is prepared by magnetron sputtering. Specifically, the flexible substrate is placed in the magnetron sputtering chamber, and metal palladium is used as the target material. The background vacuum of the chamber is controlled to be less than 8×10 -4 Pa, introduce argon gas with a flow rate of 30-150sccm, RF power of 10-150W, sputtering pressure of 1-10Pa, sputtering for 0.5-6 minutes, to obtain a palladium film with a thickness of 2-15 nanometers; Preparation of palladium thin film by thermal evaporation: The flexible substrate is placed in a thermal evaporation chamber, and metal palladium particles with a purity of 99.99% are used as the evaporation material. The background vacuum of the chamber is controlled to be less than 1×10 -4 Pa, controlling the thermal evaporation rate to 0.3-2 angstroms / second to obtain a palladium film on a flexible substrate with a thickness of 2-15 nanometers; (2) Preparation of palladium diselenide thin film by plasma enhanced high temperature selenization: The palladium thin film prepared as above is placed in a quartz tube of a tubular furnace that generates plasma by inductive coupling, the air pressure in the quartz tube is evacuated to a vacuum degree of 1-5 Pa, and argon gas is injected into the front end of the tubular furnace, and its flow rate is controlled to be 5-25 sccm; selenium powder with a purity of 99.9% is placed 10 cm upstream of the palladium film, and the central area of the tubular furnace is heated from room temperature to 250°C within 20 minutes, and the plasma RF source power is set to 200-400 watts. The temperature is maintained for 30-120 minutes, and then the temperature is naturally cooled to obtain a palladium diselenide thin film.
7. The application of the flexible sensor in strain detection according to claim 5 is characterized in that: The specific process of step 2 in the method for preparing the flexible sensor is as follows: Thermal evaporation metal electrode: Place the palladium diselenide film prepared in step 1 in a thermal evaporation chamber and control the background vacuum to be less than 1×10 -4 Pa, first evaporate indium or bismuth or chromium to a thickness of 5-20 nanometers, then evaporate gold or silver to a thickness of 30-500 nanometers, and control the width of the metal channel to 1-500 microns through a metal mask or photolithography to obtain a metal electrode; ITO electrode plating by magnetron sputtering: Place the palladium diselenide film prepared in step 1 in a magnetron sputtering chamber, use ITO as the target material, and control the background vacuum to be less than 8×10 -4 Pa, introduce argon gas with a flow rate of 50-150sccm, control the pressure in the chamber to be 1-10Pa, set the RF power to 100-200 watts, and the sputtering time to 0.5-4 hours. The thickness of ITO prepared by sputtering is 200-500 nanometers.
8. The application of the flexible sensor in strain detection according to claim 5 is characterized in that: The specific process of step 3 of the method for preparing the flexible sensor is as follows: Spin coating of PMMA encapsulation layer: Place the device prepared in step 2 on a spin coater, drip PMMA solution on the palladium diselenide film, spin at a speed of 600-4000 rpm for 1 minute, and place on a heating table at 80 degrees Celsius for drying for 5 minutes after spin coating. Or spin-coat the PI encapsulation layer: refer to the preparation method of the PMMA encapsulation layer in step 3; Alternatively, a Parylene-C encapsulation layer is deposited: the device prepared in step 2 is placed in a Parylene chemical vapor deposition system to deposit a 5-50 μm thin film; after completion, the flexible strain sensor is encapsulated and prepared.
Citation Information
Patent Citations
Anisotropy film for in-plane strain sensor, and preparation method thereof
CN104851968A
Bend sensor
CN106595469A
Strain sensor and manufacturing method thereof
CN108917582A
Strain sensor and manufacturing method thereof
CN109099832A
Graphene two-dimensional heterojunction flexible device structure and preparation method thereof
CN109285891A