Dehydration and shaping method of water-saturated wooden cultural relics
Through the combination method of low molecular weight branched polyethyleneimine and glutaraldehyde, the problems of complex operation, potential safety hazards and long cycle in the dehydration and shaping process of water-saturated wooden cultural relics in the existing technology have been solved, and simple and efficient protection of cultural relics has been achieved. The dimensional stability and mechanical properties of cultural relics are ensured.
Patent Information
- Application Number
- CN202211215975.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-30
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing technology has problems such as complex operations, potential safety hazards, long cycles, and poor mechanical properties during the dehydration and shaping process of water-saturated wooden cultural relics. In particular, the solution impregnation method and the polymer impregnation method have deficiencies in permeability and safety.
It is soaked in an aqueous solution of low molecular weight branched polyethyleneimine, and glutaraldehyde is sprayed on the surface to strengthen the internal structure of the cultural relics through hydrogen bonding and cross-linking reactions. It is wrapped in a perforated plastic film for natural drying, simplifying the operation and shortening the dehydration and shaping cycle. .
It achieves dehydration and shaping of water-saturated wooden cultural relics with simple operation, short cycle, good dimensional stability and mechanical properties, reducing the difficulty of operation and improving work efficiency without the need for special equipment.
Smart Images

Figure CN115519642B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cultural relic protection and restoration, and particularly relates to a dehydration and shaping method for water-saturated wooden cultural relics. Background Art
[0002] The earliest use of wood by humans can be traced back to the primitive period, and then developed into wood-based lacquerware and other utensils. Its production process has been continuously improved and changed with the development of history. Therefore, ancient lacquer wood is one of the valuable physical materials for studying ancient Chinese history. The main components of ancient lacquer wood are cellulose, hemicellulose, and lignin. They have been buried underground for a long time and have been soaked and eroded by groundwater for a long time. Their internal molecular structure has degraded and is completely saturated with water. After the cultural relics in a saturated state are unearthed, they are affected by the sudden change of the environment, and their surface shrinks rapidly while the internal drying speed is relatively slow, resulting in a large difference in the shrinkage of the inside and outside, which will cause irreversible and destructive changes such as warping, cracking, peeling, and deformation. Therefore, the unearthed saturated wooden cultural relics cannot be allowed to dry naturally, and protective treatment must be taken.
[0003] The protective treatment of water-saturated wooden cultural relics mainly needs to achieve the following two purposes of dehydration and shaping: first, to remove most of the moisture in the fibers until its moisture content returns to normal levels while maintaining the original shape of the object; second, to infiltrate fillers or adhere to the surface to properly reinforce the object.
[0004] There are many methods for the protection and treatment of lacquered wooden artifacts, and the principles of the treatment methods for wooden artifacts and lacquer artifacts are basically the same. At present, typical methods for the protection and treatment of lacquered wooden artifacts include natural drying, solution impregnation, monomer impregnation polymerization, polymer impregnation, freeze-drying and other methods. Most of the solution impregnation and monomer impregnation polymerization methods use volatile and flammable organic solvents such as ether and ethanol. The actual operation, material storage and safety protection requirements are high during the treatment process, and there are certain hazards to the human body and the environment during the application process; the aqueous solution system used in some polymer impregnation methods has a relatively large molecular weight of the polymer, which makes the penetration cycle of the polymer filler in the saturated lacquered wooden artifacts longer; the freeze-drying method uses the principle of direct sublimation of water molecules after freezing for dehydration, so it can effectively shorten the dehydration cycle to a certain extent, but this method is generally used in combination with methods such as polymer impregnation, which is complicated to operate and will also be affected by the poor permeability of the polymer filler. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a dehydration and shaping method for water-saturated wooden cultural relics. The dehydration and shaping method is simple to operate, has a short processing cycle, can effectively dehydrate and shape water-saturated wooden cultural relics, and the treated water-saturated wooden cultural relics have good dimensional stability and mechanical properties.
[0006] The technical solution of the present invention is achieved in this way:
[0007] The dehydration and shaping method of water-saturated wooden cultural relics specifically comprises the following steps:
[0008] (1) dissolving low molecular weight branched polyethyleneimine in water to prepare a branched polyethyleneimine aqueous solution with a mass concentration of 10-60%;
[0009] (2) Soaking the water-saturated wooden cultural relic in the branched polyethyleneimine aqueous solution until the branched polyethyleneimine penetrates into the water-saturated wooden cultural relic;
[0010] (3) Remove the water-saturated wood artifacts and remove the excess branched polyethyleneimine on the surface of the water-saturated wood artifacts;
[0011] (4) Spray 2-10% glutaraldehyde on the surface of the water-saturated wooden cultural relics several times, then wrap the water-saturated wooden cultural relics with perforated plastic film and dry them naturally in a cool place until the water-saturated wooden cultural relics reach a constant weight, thereby completing the dehydration and shaping of the water-saturated wooden cultural relics.
[0012] Furthermore, the molecular weight of the branched polyethyleneimine is 600-1200.
[0013] Furthermore, the mass concentration of the branched polyethyleneimine aqueous solution is 10-30%.
[0014] Furthermore, in step (2), the saturated wooden cultural relic is immersed in the branched polyethyleneimine aqueous solution until the density of the branched polyethyleneimine aqueous solution no longer changes, and then the branched polyethyleneimine aqueous solution is replaced with a new branched polyethyleneimine aqueous solution, and the infiltration process is continued, and this is repeated until the difference between the density of the branched polyethyleneimine aqueous solution after the saturated wooden cultural relic is immersed and the density of the new branched polyethyleneimine aqueous solution is no more than 10%.
[0015] Furthermore, in step (3), qualitative filter paper is used to remove branched polyethyleneimine on the surface of the water-saturated wooden cultural relic.
[0016] Furthermore, in step (4), when spraying glutaraldehyde, the spraying is performed 1 to 10 times in total, with an interval of 5 to 20 hours between each spraying, depending on the actual application scenario.
[0017] Furthermore, the mass concentration of glutaraldehyde is 6-10%.
[0018] Furthermore, in step (4), the temperature during natural drying is not higher than 25°C.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The present invention adopts low molecular weight branched polyethyleneimine as a filler, which has good permeability and can effectively shorten the penetration cycle, thereby effectively shortening the dehydration and shaping cycle (treatment cycle); and the branched polyethyleneimine has many active sites and contains a large amount of amino groups. When the branched polyethyleneimine penetrates into the pores of the water-saturated wooden cultural relics, the amino groups in the branched polyethyleneimine form hydrogen bonds with the hydroxyl groups and ether bonds in the water-saturated wooden cultural relics, which play a supporting role in the pores of the water-saturated wooden cultural relics, thereby strengthening the internal structure of the water-saturated wooden cultural relics.
[0021] When glutaraldehyde is sprayed on the surface of water-saturated wooden cultural relics, the primary amine in the branched polyethyleneimine structure and the aldehyde group in the glutaraldehyde structure undergo a Schiff base reaction. At the same time, glutaraldehyde also undergoes nucleophilic reaction with the hydroxyl group in the saturated wooden cultural relics, thereby forming a strong cross-linked structure on the surface of the water-saturated wooden cultural relics, thereby improving the dimensional stability of the water-saturated wooden cultural relics.
[0022] In this way, the interior and surface of the water-saturated wooden cultural relics are effectively reinforced, which can effectively guarantee the mechanical properties of the water-saturated wooden cultural relics.
[0023] 2. The dehydration and shaping method of the present invention is used to treat water-saturated wooden cultural relics. No equipment is required, the operating environment requirements are simple, the operation is simple, and the difficulty of operation for cultural relic protection staff can be effectively reduced, work efficiency can be improved, and it has universal applicability and is easy to promote and apply. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 -Macrograph of the naturally dried water-saturated wood sample obtained in Example 1.
[0025] Figure 2 -SEM image of the naturally dried water-saturated wood sample obtained in Example 1.
[0026] Figure 3 -Macroscopic image of the reinforced water-saturated wood specimen obtained in Example 2.
[0027] Figure 4 -SEM image of the reinforced water-saturated wood specimen obtained in Example 2.
[0028] Figure 5 -Macroscopic image of the reinforced water-saturated wood specimen obtained in Example 3.
[0029] Figure 6 -SEM image of the reinforced water-saturated wood specimen obtained in Example 3.
[0030] Figure 7 -XRD pattern of the naturally dried saturated wood sample obtained in Example 1.
[0031] Figure 8 -XRD pattern of the reinforced water-saturated wood sample obtained in Example 3.
[0032] Fig. 9 - Mechanical properties test results diagram. DETAILED DESCRIPTION
[0033] The dehydration and shaping method of water-saturated wooden cultural relics specifically comprises the following steps:
[0034] (1) dissolving low molecular weight branched polyethyleneimine in water to prepare a branched polyethyleneimine aqueous solution with a mass concentration of 10-60%;
[0035] (2) Soaking the water-saturated wooden cultural relic in the branched polyethyleneimine aqueous solution until the branched polyethyleneimine penetrates into the water-saturated wooden cultural relic;
[0036] (3) Remove the water-saturated wood artifacts and remove the excess branched polyethyleneimine on the surface of the water-saturated wood artifacts;
[0037] (4) Spray 2-10% glutaraldehyde on the surface of the water-saturated wooden cultural relics several times, then wrap the water-saturated wooden cultural relics with perforated plastic film and dry them naturally in a cool place until the water-saturated wooden cultural relics reach a constant weight, thereby completing the dehydration and shaping of the water-saturated wooden cultural relics.
[0038] Branched polyethyleneimine has many active sites and contains a large amount of amino groups. When branched polyethyleneimine penetrates into the pores of water-saturated wood cultural relics, the amino groups in the branched polyethyleneimine form hydrogen bonds with the hydroxyl groups and ether bonds in the water-saturated wood cultural relics, supporting the pores of the water-saturated wood cultural relics, thereby reinforcing the internal structure of the water-saturated wood cultural relics. Glutaraldehyde is sprayed on the surface of the water-saturated wood cultural relics, and the primary amine in the branched polyethyleneimine structure and the aldehyde group in the glutaraldehyde structure undergo a Schiff base reaction. At the same time, glutaraldehyde also undergoes nucleophilic reaction with the hydroxyl groups in the saturated wood cultural relics, thereby forming a strong cross-linked structure on the surface of the water-saturated wood cultural relics, thereby improving the dimensional stability of the water-saturated wood cultural relics. In this way, the interior and surface of the water-saturated wood cultural relics are effectively reinforced, which can effectively guarantee the mechanical properties of the water-saturated wood cultural relics.
[0039] The mass concentrations of branched polyethyleneimine and glutaraldehyde need to be controlled within a reasonable range. If the mass concentration of branched polyethyleneimine is too low, the amount of branched polyethyleneimine entering the saturated wood cultural relics is not enough, and the pores of the saturated wood cultural relics cannot be supported. After drying, the shrinkage rate will be high, and the purpose of shaping cannot be achieved; on the contrary, if the mass concentration of branched polyethyleneimine is too large, it will affect the penetration effect. More importantly, branched polyethyleneimine makes the internal structure of saturated wood cultural relics stronger, and produces expansion stress inside the saturated wood cultural relics, but the shaping effect of saturated wood cultural relics is not good. If the mass concentration of glutaraldehyde is too low, glutaraldehyde cannot form a cross-linked network shell structure with branched polyethyleneimine on the surface of saturated wood cultural relics, thereby causing the saturated wood cultural relics to collapse and twist when naturally drying; if the mass concentration of glutaraldehyde is too large, glutaraldehyde and branched polyethyleneimine form a dense cross-linked protective film on the surface of saturated wood cultural relics, and the stress generated is too large, thereby causing the saturated wood cultural relics to deform.
[0040] In a specific implementation, the molecular weight of the branched polyethyleneimine is 600-1200.
[0041] The branched polyethyleneimine here has a low molecular weight and good permeability. It can effectively penetrate into the interior of water-saturated wooden cultural relics and effectively shorten the dehydration and shaping time of water-saturated wooden cultural relics.
[0042] Optimally, the mass concentration of the branched polyethyleneimine aqueous solution is 10-30%.
[0043] Through research, it was found that by limiting the mass concentration of the branched polyethyleneimine aqueous solution to 10-30%, saturated wooden cultural relics with different water saturation rates can be treated, making this dehydration and shaping method universal, reducing the operating difficulty of cultural relic protection staff and helping to improve work efficiency.
[0044] In the specific implementation, in step (2), the saturated wooden cultural relic is immersed in the branched polyethyleneimine aqueous solution until the density of the branched polyethyleneimine aqueous solution no longer changes. At this time, the branched polyethyleneimine aqueous solution after immersion is replaced with a new branched polyethyleneimine aqueous solution, and the infiltration process is continued. This is repeated until the difference between the density of the branched polyethyleneimine aqueous solution after the saturated wooden cultural relic is immersed and the density of the new branched polyethyleneimine aqueous solution is no more than 10%.
[0045] Ensure that the branched polyethyleneimine effectively penetrates into the saturated wood cultural relics and makes the branched polyethyleneimine reach osmotic equilibrium. The new branched polyethyleneimine aqueous solution is the branched polyethyleneimine aqueous solution that has just been prepared without soaking the saturated wood cultural relics.
[0046] In the specific implementation, in step (3), qualitative filter paper is used to remove the branched polyethyleneimine on the surface of the water-saturated wooden cultural relic.
[0047] In specific implementation, in step (4), when spraying glutaraldehyde, according to the actual application scenario, a total of 1 to 10 sprayings are performed, with an interval of 5 to 20 hours between each spraying.
[0048] Here, the specific number of spraying times is determined according to the degree of repair of the water-saturated cultural relics. For severely decayed water-saturated wooden cultural relics, the number of spraying times is increased to achieve the stability of the shell structure, while for water-saturated cultural relics in better preservation conditions, the number of spraying times can be reduced.
[0049] During specific implementation, the mass concentration of glutaraldehyde is 6-10%.
[0050] Through research, it was found that the mass concentration of glutaraldehyde is limited to 6~10%, so that saturated wooden cultural relics with different water saturation rates can be treated, making this dehydration and shaping method universal, reducing the operating difficulty of cultural relics staff and helping to improve work efficiency.
[0051] In a specific implementation, in step (4), the temperature during natural drying is not higher than 25°C.
[0052] Natural drying means drying naturally in a place without direct sunlight.
[0053] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0054] Example 1
[0055] Take an ancient water-saturated wooden sample with a length, width and height of about 3 cm*2 cm*1 cm, wrap the water-saturated wooden sample with a perforated plastic film, and then place the water-saturated wooden sample in a cool place to dry until the water-saturated wooden sample has a constant weight.
[0056] Example 2
[0057] Take 10 g of branched polyethyleneimine with a molecular weight of 600 and dissolve it in 90 g of water to prepare a 10 wt% branched polyethyleneimine aqueous solution, and measure its density. Take an ancient water-saturated wood sample with a length, width and height of about 3 cm*2 cm*1 cm, immerse it in the prepared branched polyethyleneimine aqueous solution, and test the density of the immersion solution every 3 days. When the density value drops by more than 10%, prepare a branched polyethyleneimine aqueous solution according to the concentration of the above branched polyethyleneimine aqueous solution to repeatedly immerse the water-saturated wood sample. Repeat the above process until the density drop of the immersion solution for two consecutive times does not exceed 10% of the density of the original prepared solution.
[0058] When the density of the branched polyethyleneimine aqueous solution after the saturated wood sample is soaked is not higher than 10% of the density of the branched polyethyleneimine aqueous solution without soaking the saturated wood sample, the saturated wood sample is taken out and the branched polyethyleneimine remaining on the surface of the saturated wood sample is gently wiped off with qualitative filter paper.
[0059] Wrap the water-saturated wood sample with a perforated plastic film, and then place the water-saturated wood sample in a cool place to dry until the water-saturated wood sample reaches a constant weight.
[0060] Example 3
[0061] Take 10 g of branched polyethyleneimine with a molecular weight of 600 and dissolve it in 90 g of water to prepare a 10wt% branched polyethyleneimine aqueous solution, and measure its density. Take an ancient water-saturated wood sample with a length, width and height of about 3cm*2cm*1cm, immerse it in the prepared branched polyethyleneimine aqueous solution, and test the density of the immersion solution every 3 days. When the density value drops by more than 10%, prepare a branched polyethyleneimine aqueous solution according to the concentration of the above branched polyethyleneimine aqueous solution to repeatedly immerse the water-saturated wood sample. Repeat the above process until the density drop of the immersion solution for two consecutive times does not exceed 10% of the density of the original prepared solution.
[0062] When the density of the branched polyethyleneimine aqueous solution after the saturated wood sample is soaked is not higher than 10% of the density of the branched polyethyleneimine aqueous solution without soaking the saturated wood sample, the saturated wood sample is taken out and the residual polyethyleneimine on the surface of the saturated wood sample is gently wiped off with qualitative filter paper.
[0063] Take 8 g of glutaraldehyde and dissolve it in 92 g of water to prepare an 8 wt % glutaraldehyde aqueous solution. Use a spray bottle to spray 8 wt % glutaraldehyde on the saturated wood sample. The glutaraldehyde solution is sprayed twice a day with an interval of 8 h between each spraying, and the spraying is continued for 3 days.
[0064] The water-saturated wood sample treated by spraying glutaraldehyde is taken out, and the water-saturated wood sample is wrapped with a plastic film with holes, and then the water-saturated wood sample is placed in a cool place to dry until the water-saturated wood sample has a constant weight.
[0065] Example 4
[0066] This embodiment is the same as embodiment 3, except that the mass concentration of the branched polyethyleneimine aqueous solution is 30%.
[0067] Example 5
[0068] This embodiment is the same as embodiment 3, except that the mass concentration of the branched polyethyleneimine aqueous solution is 60%.
[0069] Example 6
[0070] This embodiment is the same as embodiment 3, except that the mass concentration of glutaraldehyde is 2%.
[0071] Example 7
[0072] This embodiment is the same as embodiment 3, except that the mass concentration of glutaraldehyde is 6%.
[0073] Example 8
[0074] This embodiment is the same as embodiment 3, except that the mass concentration of glutaraldehyde is 10%.
[0075] 1. Example 1 adopts natural drying method. The macroscopic image and SEM image of the water-saturated wood sample obtained after natural drying are as follows: Figure 1 and Figure 2 As shown; Example 2 uses a branched polyethyleneimine aqueous solution to strengthen and then dry, and the macroscopic and SEM images of the saturated wood sample obtained after drying are as shown Figure 3 and Figure 4 Example 3 uses branched polyethyleneimine aqueous solution and glutaraldehyde to strengthen and dry, and the macroscopic and SEM images of the saturated wood sample obtained after drying are as shown respectively. Figure 5 and Figure 6 shown.
[0076] By comparing and analyzing Examples 1, 2, and 3, we can see that Figure 2 As shown in the figure, if the water-saturated wood sample is not treated in any way and then dried naturally, the fiber channels inside the water-saturated wood sample will collapse violently and shrink and curl in an disordered manner. Figure 4 As shown in the figure, if the water-saturated wood sample is immersed in the branched polyethyleneimine solution (10wt%) for 7 days, the branched polyethyleneimine plays a filling and supporting role inside the water-saturated wood sample. After drying, the drying shrinkage and collapse of the water-saturated wood sample are hindered to a certain extent, and its fiber pores are supported to a certain extent so that no collapse occurs. Figure 6 As shown in the figure, if the water-saturated wood specimens are immersed in a branched polyethyleneimine solution (10wt%) for 7 days and then sprayed with a glutaraldehyde solution (8wt%) (spraying 6 times in three days, twice a day, and each time interval of 8h), the branched polyethyleneimine and glutaraldehyde are cross-linked on the outer surface of the water-saturated wood specimens to form a tight shell structure. Under the tensile action of the internal filling support of the branched polyethyleneimine and the shell structure formed by the cross-linking of the branched polyethyleneimine and the surface of the glutaraldehyde, the fiber pores inside the water-saturated wood specimens are effectively prevented from collapsing and curling after the water-saturated wood specimens are dried, thereby achieving a good protective effect.
[0077] 2. The XRD pattern of the naturally dried water-saturated wood sample obtained in Example 1 is as follows: Figure 7As shown, the XRD pattern of the reinforced water-saturated wood sample obtained in Example 3 is as follows Figure 8 As shown, through Figure 7 and Figure 8 From the comparison, it can be seen that after the dual treatment of branched polyethylene imine and glutaraldehyde, the XRD characteristic peak of the water-saturated wood specimen has basically not shifted, while the peak intensity has been significantly increased. Therefore, it can be seen that the internal structure regularity of the water-saturated wood specimen treated with branched polyethylene imine and glutaraldehyde has been improved, and the mechanical properties have been improved.
[0078] 3. The water-saturated wood specimens treated in Examples 1 to 8 were measured. The shrinkage rates and mass loss rates of the longitudinal, radial and chordal lengths of the water-saturated wood specimens in each example are shown in the table below.
[0079] Table 1 Shrinkage and mass loss of water-saturated wood specimens after treatment in Example 1 to Example 8
[0080]
[0081] Referring to Table 1, it is found through comparison that when branched polyethyleneimine and glutaraldehyde are used simultaneously to dehydrate and protect the water-saturated wood specimens, the shrinkage rate in all aspects is the smallest, and the appearance shape of the water-saturated wood specimens when unearthed can be maintained to the greatest extent.
[0082] 4. The mechanical properties test results of water-saturated wooden cultural relics are as follows: Fig. 9 As shown, from Fig. 9 It can be seen that whether in the transverse or longitudinal direction, the addition of branched polyethyleneimine (PEI) molecules to the water-soaked wood matrix will increase its mass density and form weak cross-links in the wood matrix, thereby improving its stiffness and load-bearing capacity to a certain extent ( Fig. 9 B, 9C, 9E, and 9F). In addition, when compressed along the longitudinal direction, the samples treated with branched polyethyleneimine showed greatly improved toughness compared with the other groups, which may be attributed to the high elasticity of the weakly cross-linked porous wood matrix ( Fig. 9 G). In contrast, the samples treated with branched polyethyleneimine / glutaraldehyde showed further improved elastic modulus and compression modulus due to the formation of a dense cross-linked shell around the weakly cross-linked interior. However, compared with the loosely cross-linked structure (branched polyethyleneimine experimental group), the structure with high surface cross-linking and low internal cross-linking (branched polyethyleneimine / glutaraldehyde experimental group) did not seem to show a significant advantage in mechanical buffering capacity, but the energy dissipation value of the saturated wood specimens treated with branched polyethyleneimine and glutaraldehyde (GA) at the first fracture was still several times higher than that of the original saturated wood specimens ( Fig. 9 G). It can be seen that the samples treated with branched polyethyleneimine / glutaraldehyde have high strength, stiffness and mechanical buffering capacity, thus preventing the shrinkage and collapse of the wet wood matrix during the drying process.
[0083] Finally, it should be noted that the above embodiments of the present invention are only examples for illustrating the present invention, and are not intended to limit the implementation methods of the present invention. For those skilled in the art, other different forms of changes and modifications can be made based on the above description. It is impossible to list all implementation methods here. Any obvious changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.
Claims
1. A method for dehydrating and shaping water-saturated wooden cultural relics, characterized in that: The specific steps include: (1) dissolving branched polyethyleneimine with a molecular weight of 600 to 1200 in water to prepare a branched polyethyleneimine aqueous solution with a mass concentration of 10 to 30%; (2) Soaking the water-saturated wooden cultural relic in the branched polyethyleneimine aqueous solution until the branched polyethyleneimine penetrates into the water-saturated wooden cultural relic; (3) Remove the water-saturated wood artifacts and remove the excess branched polyethyleneimine on the surface of the water-saturated wood artifacts; (4) Spray 2-10% glutaraldehyde on the surface of the water-saturated wooden cultural relics several times, then wrap the water-saturated wooden cultural relics with perforated plastic film and dry them naturally in a cool place until the water-saturated wooden cultural relics reach a constant weight, thereby completing the dehydration and shaping of the water-saturated wooden cultural relics.
2. The method for dehydrating and shaping water-saturated wooden cultural relics according to claim 1, characterized in that: In step (2), the saturated wooden cultural relic is immersed in the branched polyethyleneimine aqueous solution until the density of the branched polyethyleneimine aqueous solution no longer changes. At this time, the branched polyethyleneimine aqueous solution after immersion is replaced with a new branched polyethyleneimine aqueous solution, and the infiltration process is continued. This is repeated until the difference between the density of the branched polyethyleneimine aqueous solution after the saturated wooden cultural relic is immersed and the density of the new branched polyethyleneimine aqueous solution is no more than 10%.
3. The method for dehydrating and shaping water-saturated wooden cultural relics according to claim 1, characterized in that: In step (3), qualitative filter paper is used to remove branched polyethyleneimine on the surface of the water-saturated wooden cultural relic.
4. The method for dehydrating and shaping water-saturated wooden cultural relics according to claim 1, characterized in that: In step (4), when spraying glutaraldehyde, according to the actual application scenario, a total of 1 to 10 sprays are performed, with an interval of 5 to 20 hours between each spray.
5. The method for dehydrating and shaping water-saturated wooden cultural relics according to claim 1 or 4, characterized in that: The mass concentration of glutaraldehyde is 6~10%.
6. The method for dehydrating and shaping water-saturated wooden cultural relics according to claim 1, characterized in that: In step (4), the temperature is not higher than 25°C during natural drying.