Composite coating and preparation method thereof

By adopting a composite structure of the chromium oxynitride coating with a face-centered cubic structure in the coating, the problems of coating cracking and falling off at high temperatures are solved, and the high temperature stability and oxidation resistance are improved. Tools suitable for high temperature environments.

CN115572945BActive Publication Date: 2024-11-22NAXAU NEW MATERIALS CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211106051.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-09
Publication Date
2024-11-22
Estimated Expiration
2042-09-09

AI Technical Summary

Technical Problem

The existing coatings crack and fall off due to thermal stress differences in high temperature environments, and their oxidation resistance is insufficient, which affects its use effect at high temperatures.

Method used

The composite structure of the chromium oxynitride coating with a face-centered cubic structure and the chromium oxide coating is used. The columnar crystal axis of the chromium oxynitride coating is arranged vertically and is connected to the chromium oxide coating, which delays the Cr-N bond through the Cr-O bond. It breaks and absorbs thermal stress through columnar crystals to improve the bonding force and high temperature stability of the coating and substrate.

Benefits of technology

It achieves good bonding and stability between the coating and the substrate at high temperature, has high-temperature oxidation resistance and corrosion resistance, and extends the service life of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115572945B_ABST
    Figure CN115572945B_ABST
Patent Text Reader

Abstract

The present application relates to a composite coating and a method for preparing the same. A composite coating according to some embodiments of the present application includes a first layer and a second layer formed on a substrate, wherein the first layer is an oxynitride chromium coating, and the second layer is a dense chromium oxide coating, and the oxynitride chromium coating contains oxynitride chromium columnar crystals with a face-centered cubic structure, wherein the crystal axes of the oxynitride chromium columnar crystals are arranged vertically on the coating surface of the oxynitride chromium coating. The composite coating of the present application can optimize the coating structure, present a dense chromium oxide surface layer, and provide bonding strength between the substrate and the coating through the oxynitride chromium coating with a face-centered cubic structure, and the coating is particularly suitable for use in high-temperature environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of coatings, and more specifically, to a composite coating and a preparation method thereof. Background Art

[0002] In the field of industrial manufacturing, physical vapor deposition (PVD) coatings are widely used on the surface of molds or tools to improve the surface properties of the base material, which is an effective way to adapt to the process environment and increase the service life. With the development of surface composite coating technology, its application field is more extensive, and various fields have put forward higher requirements on the process performance of surface coatings. In order to adapt to more complex surface coatings, the bonding strength between the surface coating and the substrate, wear resistance, impact resistance and corrosion resistance are improved to meet the requirements of modern industrial technology.

[0003] In the prior art, the thermal stress generated by the difference in thermophysical properties between the coating material and the base material in a high temperature environment may cause the coating to crack and fall off. For composite coatings, the difference in thermophysical properties between the composite material layers may lead to uneven distribution of thermal stress between the coatings, which in turn seriously affects the normal use of the composite coating.

[0004] Therefore, there are still many technical problems to be solved in the industry, such as how to improve the bonding strength and high-temperature stability of the coating and optimize the application effect of the coating in high-temperature environments. Summary of the invention

[0005] One of the purposes of the embodiments of the present application is to provide a composite coating, which includes at least one layer of oxynitride chromium coating and at least one layer of chromium oxide coating, wherein the oxynitride chromium coating has columnar crystals with a face-centered cubic structure, and the crystal axes of the columnar crystals of the oxynitride chromium coating are vertically arranged and bonded to the surface of the chromium oxide coating. Through the design of the above-mentioned coating crystal arrangement, the oxynitride chromium coating of the present application, on the one hand, will delay the fracture oxidation of the Cr-N bond at high temperature due to the presence of the existing Cr-O bond, and on the other hand, the columnar crystals can absorb part of the thermal stress from the chromium oxide, thereby ensuring good bonding and stability between the coating and the substrate at high temperature. The composite coating of the present application is particularly suitable for use in a high-temperature anti-oxidation environment.

[0006] According to one aspect of the present application, some embodiments of the present application provide a composite coating, which includes a first layer and a second layer configured to be formed sequentially on the surface of a substrate, wherein the first layer is an oxynitride chromium coating, and the second layer is a chromium oxide coating, and the oxynitride chromium coating comprises oxynitride chromium columnar crystals with a face-centered cubic structure, wherein the crystal axes of the oxynitride chromium columnar crystals are vertically arranged on the coating surface of the oxynitride chromium coating.

[0007] In some embodiments, the first layer has a thickness of 500 nm to 1 μm.

[0008] In some embodiments, the diameter of the chromium oxynitride columnar crystals of the first layer is 200 nm to 500 nm.

[0009] In some embodiments, the second layer has a porosity of 0% to 1.5%.

[0010] In some embodiments, the composite coating further includes a composite layer in which chromium oxynitride coatings and chromium oxide coatings are alternately arranged, and the composite layer is arranged on the second layer, wherein the coating of the composite layer close to the substrate is the chromium oxynitride coating, and the outermost coating of the composite layer is the chromium oxide coating.

[0011] According to another aspect of the present application, some embodiments of the present application provide a tool having the composite coating described in any of the above embodiments.

[0012] According to another aspect of the present application, some embodiments of the present application provide a method for preparing the composite coating of the above embodiment, which comprises the following steps:

[0013] (1) Providing a base material (substrate);

[0014] (2) using a vacuum cathode electron gun technique to perform physical vapor deposition, with chromium as a target, in an environment where a nitrogen flow rate is 300 sccm to 700 sccm and an oxygen flow rate is 10 sccm to 200 sccm, to form a chromium oxynitride coating on the substrate;

[0015] (3) Physical vapor deposition is performed using vacuum cathode electron gun technology, with chromium as the target material, and a chromium oxide coating is formed on the surface of the chromium oxynitride coating in an environment where an oxygen flow rate is 250 sccm to 500 sccm.

[0016] In some embodiments, during step (2), the current of ion beam evaporation needs to be increased over time, with an initial current of 80A to 120A and an increasing current set to 1A / min-5A / min.

[0017] In some embodiments, the final value of the current of the cathode electron gun is less than or equal to 200A.

[0018] In some embodiments, during physical vapor deposition, a bias voltage is set to 100V to 200V.

[0019] In some embodiments, during physical vapor deposition, a temperature of 300-600° C. is set.

[0020] The composite coating provided in the embodiment of the present application, through the alternating arrangement of the chromium oxynitride coating and the chromium oxide coating, the chromium oxide coating can prevent external oxygen from diffusing into the coating, and the chromium oxynitride coating with columnar crystals of face-centered cubic structure can absorb the thermal stress from the chromium oxide coating, so as to optimize the high-temperature thermal stress distribution of different coatings in the composite coating. Therefore, the composite coating provided in the present application has good high-temperature stability and high-temperature oxidation resistance.

[0021] Additional aspects and advantages provided by the embodiments of the present application will be partially described, shown, or explained through the implementation of the embodiments of the present application in the subsequent description. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The following will briefly describe the drawings necessary for describing the embodiments of the present application or the prior art to facilitate the description of the embodiments of the present application. Obviously, the drawings described below are only some of the embodiments in the present application. For those skilled in the art, without the need for creative work, drawings of other embodiments can still be obtained based on the structures illustrated in these drawings.

[0023] Figure 1 It is a schematic longitudinal cross-sectional view of a composite coating according to some embodiments of the present application.

[0024] Figure 2 It is a schematic longitudinal cross-sectional view of a composite coating according to some embodiments of the present application.

[0025] Figure 3 The present invention is a flow chart of the preparation of a composite coating according to some embodiments of the present application.

[0026] Figure 4 This is the X-ray diffraction pattern of the chromium oxynitride coating of Example 1 of the present application.

[0027] Figure 5 This is the X-ray diffraction pattern of the chromium oxynitride coating of Example 3 of the present application. DETAILED DESCRIPTION

[0028] The embodiments of the present application will be described in detail below. The embodiments of the present application should not be interpreted as limiting the present application.

[0029] Unless expressly stated otherwise, the following terms used herein have the meanings indicated below.

[0030] As used herein, the terms "substantially," "substantially," "essentially," and "about" are used to describe and illustrate small variations. When used in conjunction with an event or circumstance, the terms may refer to instances where the event or circumstance occurred exactly as well as instances where the event or circumstance occurred very approximately. For example, when used in conjunction with a numerical value, the terms may refer to a range of variation less than or equal to ±10% of the numerical value, such as less than or equal to ±5%, less than or equal to ±4%, less than or equal to ±3%, less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.1%, or less than or equal to ±0.05%. For example, two values ​​may be considered “substantially” the same if the difference between them is less than or equal to ±10% of the average of the values ​​(e.g., less than or equal to ±5%, less than or equal to ±4%, less than or equal to ±3%, less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.1%, or less than or equal to ±0.05%).

[0031] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "one or more of," "one or more of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "one or more of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "one or more of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.

[0032] Furthermore, for ease of description, "first", "second", "third", etc. may be used herein to distinguish different components of one figure or a series of figures. Unless otherwise specifically specified or limited, "first", "second", "third", etc. are not intended to describe corresponding components.

[0033] In the field of industrial manufacturing, coating processes are widely used on the surfaces of various objects or tool parts to improve their surface properties, including wear resistance, heat resistance, corrosion resistance, etc. However, as the scope of coating application gradually expands, the demand for the tolerance of the coating in a specific environment also increases. Especially in high-temperature application environments, due to the difference in thermophysical properties between the coating and the base material, it often leads to uneven distribution of thermal stress between the coating and the base material, which in severe cases will further cause the coating to peel off and fall off. In addition, the lack of antioxidant properties of the coating itself at high temperatures will cause the coating to be internally diffused by oxygen at high temperatures, which will lead to oxidation and failure of the coating material, which in severe cases will further cause the coating to peel off and fall off.

[0034] In view of the above problems, according to one aspect of the present application, some embodiments of the present application provide a composite coating, which includes at least one layer of chromium oxynitride coating and at least one layer of chromium oxide coating, wherein the chromium oxynitride coating has columnar crystals of face-centered cubic structure, and the crystal axes of the columnar crystals of the chromium oxynitride coating are vertically arranged and bonded to the surface of the chromium oxide coating. The coating arrangement of the composite coating of the present application can withstand a high temperature of 800°C in an aerobic environment, and keep the hardness and structure of the coating unchanged.

[0035] Figure 1 It is a schematic longitudinal cross-sectional view of a composite coating according to some embodiments of the present application.

[0036] like Figure 1 As shown, a composite coating 10 according to some embodiments of the present application includes a chromium oxynitride coating 101 and a chromium oxide coating 102 which are sequentially formed on the surface of a substrate 100. The composite coating 10 of the present application has thermal stability and high oxidation resistance in a high-temperature oxidizing environment, and also has extremely high corrosion resistance and wear resistance at high temperatures, and can provide excellent high-temperature protection for the tool parts coated thereon.

[0037] Without violating the spirit of the present application, the substrate 100 can be any suitable industrial material in the art without being limited thereto. In some embodiments, the substrate 100 is a cemented carbide material. In some embodiments, the cemented carbide material includes one or more of tungsten carbide, titanium carbide, niobium carbide and vanadium carbide. The binder in the cemented carbide material can be any suitable doped metal in the art without being limited thereto. In some embodiments, the cemented carbide material also includes one or more doped metals of metal cobalt or metal nickel. The face-centered cubic chromium oxynitride columnar crystals in the present application can form a tight fitting structure at the bonding interface between the cemented carbide material, so that the chromium oxynitride columnar crystals have excellent stability and bonding force on the surface of the substrate of the cemented carbide material. In some embodiments, the substrate is a cobalt tungsten carbide alloy, wherein the weight ratio of cobalt (Co) is about 8% based on the total weight of the substrate.

[0038] The chromium oxynitride 101 coating is disposed on the surface of the substrate 100, wherein the chromium oxynitride coating comprises chromium oxynitride columnar crystals of a face-centered cubic structure. In some embodiments, the chromium oxynitride coating is a chromium oxynitride columnar crystal of a face-centered cubic structure, and the crystal axis of the chromium oxynitride columnar crystal is perpendicular to the surface of the substrate. In some embodiments, the diameter of the chromium oxynitride columnar crystals of the first layer is 200nm-500nm to optimize the bonding force between the chromium oxynitride coating and the substrate. In some embodiments, the thickness of the chromium oxynitride coating is approximately: 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1.0μm or a numerical range consisting of any two of the above values. In some embodiments, the thickness of the chromium oxynitride coating is 500nm to 1μm to optimize the thermal stress distribution of the chromium oxynitride coating and the substrate, and to improve the structural stability of the composite coating. The chromium oxynitride columnar crystals in the chromium oxynitride coating will delay the fracture oxidation of the Cr-N bond at high temperature due to the existence of the existing Cr-O bond, thereby preventing the diffusion of oxygen at high temperature. At the same time, the chromium oxynitride columnar crystals can absorb part of the thermal stress from the chromium oxide coating, thereby ensuring a good thermal stress distribution between the composite coating and the substrate at high temperature, thereby improving the high temperature stability and bonding strength of the composite coating.

[0039] The chromium oxide coating 102 is disposed on the surface of the chromium oxide nitride coating 101, wherein the crystal axes of the chromium oxide nitride columnar crystals in the chromium oxide nitride coating 101 are vertically arranged on the coating surface of the chromium oxide coating 102. In some embodiments, the bonding interface formed by the vertically arranged chromium oxide nitride columnar crystals and the chromium oxide coating has excellent stability, which can improve the bonding force and high temperature stability of the composite coating. In some embodiments, the porosity of the chromium oxide coating is 0% to 1.5% to form a dense chromium oxide coating. In a high temperature environment of about 800°C, the dense chromium oxide coating can effectively prevent external oxygen from diffusing into the interior of the coating. At the same time, the Cr-O bond of the chromium oxide coating will basically not break at high temperatures, has high structural stability and high temperature red hardness, and can effectively improve the high temperature hardness and high temperature durability of the composite coating. In some embodiments, the thickness of the chromium oxide coating is approximately: 1.0μm, 1.1μm, 1.2μm, 1.3μm, 1.5μm, 2.0μm or a numerical range consisting of any two of the above values. In some embodiments, the thickness of the chromium oxide coating is 1 μm to 2 μm to optimize the anti-oxidation performance of the chromium oxide coating and improve the structural stability of the composite coating.

[0040] The composite coating of the present application can be disposed on any suitable surface without limitation, including, but not limited to, a flat surface, a curved surface, an uneven surface, etc.

[0041] In some embodiments, the material crystal structure of the chromium oxynitride coating in the composite coating can be detected by an X-ray Diffractometer (XRD). In some embodiments, the face-centered cubic chromium oxynitride columnar crystals under XRD detection have three characteristic peaks, and the characteristic peaks are respectively between 30° and 40°, between 40° and 50°, and between 60° and 70°. In some embodiments, the characteristic peaks of the face-centered cubic chromium oxynitride columnar crystals are respectively located at about 38°, about 44°, and about 64°.

[0042] Figure 2 It is a schematic longitudinal cross-sectional view of a composite coating according to some embodiments of the present application.

[0043] like Figure 2 As shown, a composite coating 20 according to some embodiments of the present application further includes at least one composite layer 200 in which oxynitride chromium coatings 101 and chromium oxide coatings 102 are alternately arranged, and the composite layer is arranged on the chromium oxide coating 102, wherein the coating of the composite layer 200 close to the substrate is the oxynitride chromium coating 101, and the outermost coating of the composite layer 200 is the chromium oxide coating 102.

[0044] The number of composite layers can be adjusted according to actual thermal insulation performance or tolerance performance requirements. In some embodiments, the number of composite layers is one. In some embodiments, the number of composite layers is 1 to 10.

[0045] According to another aspect of the present application, some embodiments of the present application provide a tool having the composite coating described in any of the above embodiments.

[0046] The tool parts of the present application are not particularly limited, and can be any suitable industrial parts known in the prior art. In some embodiments, the tool parts can include, but are not limited to, high temperature visors, cutting devices, mobile device housings, aircraft housings, etc.

[0047] Figure 3 The present invention is a flow chart of the preparation of a composite coating according to some embodiments of the present application.

[0048] According to another aspect of the present application, some embodiments of the present application provide a method for preparing the composite coating of the above embodiment, such as Figure 3 As shown, it includes the following steps:

[0049] (1) providing a substrate;

[0050] (2) using a vacuum cathode electron gun technique to perform physical vapor deposition, with chromium as a target, in an environment where a nitrogen flow rate is 300 sccm to 700 sccm and an oxygen flow rate is 10 sccm to 200 sccm, to form a chromium oxynitride coating on the substrate;

[0051] (3) Physical vapor deposition is performed using vacuum cathode electron gun technology, with chromium as the target material, and a chromium oxide coating is formed on the surface of the chromium oxynitride coating in an environment with an oxygen flow rate of 250 sccm to 500 sccm.

[0052] In some embodiments, by adjusting the flow rates of oxygen and nitrogen, the arrangement structure of the chromium oxynitride columnar crystals can be optimized, and the density of the chromium oxide coating can be effectively improved. In some embodiments, in the deposition step of the chromium oxynitride coating, the flow rate of nitrogen is 300 sccm to 500 sccm and the flow rate of oxygen is 30 sccm to 1000 sccm. In some embodiments, in the deposition step of the chromium oxynitride coating, the flow rate of nitrogen is 300 sccm and the flow rate of oxygen is 50 sccm.

[0053] In some embodiments, the target material is a non-uniform cylindrical particle, the size of which does not exceed φ48*30 mm, so as to adjust the diameter of the chromium oxynitride columnar crystals.

[0054] In some embodiments, during physical vapor deposition, the deposition temperature is 300° C. to 600° C.

[0055] In some embodiments, during step (2), the current of ion beam evaporation needs to be increased over time, with an initial current of 80A to 120A and an increasing current set to 1A / min-5A / min to optimize the arrangement structure of the chromium oxynitride columnar crystals.

[0056] In some embodiments, the final value of the current of the cathode electron gun is less than or equal to 200 A to optimize the arrangement structure of the chromium oxynitride columnar crystals.

[0057] In some embodiments, during physical vapor deposition, a bias voltage is set to 100V to 200V.

[0058] In some embodiments, during physical vapor deposition, a temperature of 300-600° C. is set.

[0059] In some embodiments, step (2) and step (3) are repeated to further alternately arrange chromium oxynitride coatings and chromium oxide coatings on the existing composite coating to form a multi-layer composite layer. Specific embodiments

[0061] Some specific embodiments are listed below and the composite coatings are subjected to microstructure tests, high-temperature natural oxidation tests, hardness tests and bonding strength tests to better illustrate the technical solution of the present application.

[0062] I. Test Method

[0063] Microstructure testing:

[0064] The qualitative XRD detection scheme adopted was to detect the crystal structure of the chromium oxynitride coating deposited in the following examples through an XRD detector, wherein the detection range of XRD was 30°-90° and the step length was 0.02.

[0065] High temperature natural oxidation test:

[0066] The thermostat was heated to 800°C at a heating rate of 3°C / min. After the temperature reached 800°C, the cemented carbide sheet coated with the composite coating was placed in the thermostat for 2 hours. Afterwards, the sheet was taken out and the bonding condition of the surface coating was observed.

[0067] Bonding strength test:

[0068] The test sample was left to stand in a dry environment for 5 minutes, and the substrate and the composite coating were respectively placed at the test ends of the tensile machine (Anton Paar Scratch) with the parameters set as a loading load of 100N, a dynamic load scratch length of 3mm, and a loading rate of 100N / min to conduct an interface peeling adhesion test.

[0069] Hardness test:

[0070] The hardness of the composite coating surface in the following examples was tested using a nanoindentation device (Fischer, Scope HM2000).

[0071] II. Preparation method

[0072] Example 1

[0073] A hard alloy test piece is used as the substrate, and the size of the substrate is 25 cm×25 cm×6 cm. The substrate is pre-cleaned: after wiping the surface of the substrate with acetone, the substrate is placed in an ultrasonic cleaning machine for ultrasonic rinsing.

[0074] Provide substrate: Load the pretreated carbide test piece into the deposition furnace, set the rotating frame speed to 3 rpm, and adjust the gas pressure to 1×10 -3 Pa, heating to 300℃.

[0075] Plasma cleaning: open the argon flow valve, adjust the gas pressure in the deposition furnace to 0.1 Pa, set the negative bias voltage and negative bias duration of the substrate to 1200 V and 1 minute, 1000 V and 1 minute, 800 V and 1 minute, and 600 V and 5 minutes in sequence, and then complete the plasma cleaning.

[0076] Deposition of chromium oxynitride coating: adjust the negative bias voltage of the substrate to 150 V, the gas pressure in the deposition furnace to 1 Pa, the initial current to 80 A, increase to 200 A at a rate of 2 A / min, set the nitrogen flow rate to 300 sccm, the oxygen flow rate to 50 sccm, the temperature to 300 ° C, and the deposition time to 900 s.

[0077] Deposition of chromium oxide coating: adjust the substrate negative bias voltage to 150 V, the gas pressure in the deposition furnace to 1 Pa, the coating current to 200 A, the oxygen flow rate to 500 sccm, the temperature to 300 ° C, and the deposition time to 2400 s.

[0078] Example 2

[0079] The preparation method is substantially the same as that of Example 1, except that when depositing the chromium oxynitride coating, the nitrogen flow rate is 300 sccm and the oxygen flow rate is 0 sccm, and when depositing the chromium oxide coating, the oxygen flow rate is 500 sccm.

[0080] Example 3

[0081] The preparation method is substantially the same as that of Example 1, except that when depositing the chromium oxynitride coating, the nitrogen flow rate is 300 sccm and the oxygen flow rate is 50 sccm, and when depositing the chromium oxide coating, the oxygen flow rate is 100 sccm.

[0082] Example 4

[0083] The preparation method is substantially the same as that of Example 1, except that when depositing the chromium oxynitride coating, the nitrogen flow rate is 300 sccm and the oxygen flow rate is 50 sccm, and when depositing the chromium oxide coating, the oxygen flow rate is 1000 sccm.

[0084] III. Test Results

[0085] Results of high temperature natural oxidation test, bonding strength test and hardness test of cemented carbide coatings of Examples 1-4 It is recorded in the following Table 1.

[0086] Table 1

[0087]

[0088] Crystal structure of the coating:

[0089] As shown in the table above, the present invention can form a more detailed crystal structure by adjusting the preparation process of the chromium oxynitride coating. Figure 4 As shown, the characteristic peak of the single columnar crystal of the chromium oxynitride coating of Example 1 of the present application between 30° and 40° has a higher half-peak width, which means that the crystal grains are extremely small, and the average diameter can reach 20nm. The fine and tight coating structure effectively optimizes the bonding force to the substrate and improves the surface hardness of the composite coating. In contrast, referring to Example 3, as Figure 5 As shown, the characteristic peak of a single columnar crystal of the chromium oxynitride coating of Example 3 of the present application between 30° and 40° has a lower half-peak width, which indicates that its grains are larger, which also leads to lower bonding strength of the coating of Example 3 to the substrate and lower surface hardness.

[0090] Bonding strength test:

[0091] The above-mentioned embodiments were subjected to a natural oxidation test at 800°C. Embodiments 2, 3, and 4 all showed a decrease in the adhesion of the coating, while Embodiment 1 remained intact, and the adhesion between the coating and the substrate remained above 60N. By comparing Embodiments 1-4 of the present application, it can be seen that the fine coating crystals can improve the adhesion of the coating structure to the chromium oxide coating and the cemented carbide material substrate. From the results of the adhesion test, it can be seen that the chromium oxynitride coating in the composite coating of the present application can effectively optimize the adhesion between the composite coating and the substrate, and still maintain its adhesion after passing the high-temperature oxidation test, which means that the composite coating of the present application has excellent high-temperature stability and can maintain the coating in a high-temperature environment.

[0092] Hardness test:

[0093] The surface hardness of the coating of Example 1 is 22 GPa ± 1.2 GPa, the surface hardness of the coating of Example 2 is 18 GPa ± 1.5 GPa, the surface hardness of the coating of Example 3 is 15 GPa ± 1.2 GPa, and the surface hardness of the coating of Example 4 is 14 GPa ± 1.7 GPa. The surface hardness of the coating of Example 1 after high temperature oxidation test is 21 GPa ± 1.5 GPa.

[0094] Through the comparison of Examples 1-4 of the present application, it can be seen that the fine coating crystals can greatly improve the hardness performance of the coating structure after high temperature. From the hardness test results, it can be seen that the composite coating of the present application still has excellent hardness performance in a high temperature and oxygen-rich environment, indicating that the composite coating of the present application has excellent high temperature stability and can maintain the wear resistance of the coating in a high temperature environment.

[0095] References throughout the specification to "embodiment", "part of an embodiment", "one embodiment", "another example", "example", "specific example" or "part of an example" mean that at least one embodiment or example in the present application includes the specific features, structures, materials or characteristics described in the embodiment or example. Therefore, descriptions appearing in various places throughout the specification, such as: "in some embodiments", "in an embodiment", "in one embodiment", "in another example", "in an example", "in a specific example" or "example" do not necessarily refer to the same embodiment or example in the present application. In addition, the specific features, structures, materials or characteristics herein may be combined in one or more embodiments or examples in any suitable manner.

[0096] Although illustrative embodiments have been demonstrated and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions and modifications may be made to the embodiments without departing from the spirit, principles and scope of the present application.

Claims

1. A composite coating, comprising a first layer and a second layer configured to be sequentially formed on a surface of a substrate, wherein the first layer is a chromium oxynitride coating, the second layer is a chromium oxide coating, the chromium oxynitride coating comprises chromium oxynitride columnar crystals of a face-centered cubic structure, wherein the crystal axes of the chromium oxynitride columnar crystals are vertically arranged on the coating surface of the chromium oxynitride coating; The preparation method of the composite coating comprises the following steps: (1) providing a substrate; (2) Plasma cleaning; (3) using a vacuum cathode electron gun technique to perform physical vapor deposition, with chromium as a target, in an environment where a nitrogen flow rate is 300 sccm and an oxygen flow rate is 50 sccm, to form a chromium oxynitride coating on the substrate; (4) Physical vapor deposition is performed using a vacuum cathode electron gun technique, with chromium being the target material, and a chromium oxide coating is formed on the surface of the chromium oxynitride coating in an environment where an oxygen flow rate is 500 sccm. The composite coating according to claim 1 , wherein the thickness of the first layer is 500 nm to 1 μm. 3 . The composite coating according to claim 1 , wherein the diameter of the chromium oxynitride columnar crystals of the first layer is 200 nm to 500 nm. The composite coating according to claim 1 , wherein the porosity of the second layer is 0% to 1.5%.

5. The composite coating according to claim 1 further comprises a composite layer in which the chromium oxynitride coating and the chromium oxide coating are alternately arranged, the composite layer is arranged on the second layer, wherein the coating layer of the composite layer close to the substrate is the chromium oxynitride coating, and the outermost coating layer of the composite layer is the chromium oxide coating.

6. A tool part having the composite coating according to any one of claims 1 to 5.

7. A method for preparing a composite coating according to any one of claims 1 to 5, comprising the following steps: (1) providing a substrate; (2) Plasma cleaning; (3) using a vacuum cathode electron gun technique to perform physical vapor deposition, with chromium as a target, in an environment where a nitrogen flow rate is 300 sccm and an oxygen flow rate is 50 sccm, to form a chromium oxynitride coating on the substrate; (4) Physical vapor deposition is performed using a vacuum cathode electron gun technique, with chromium being the target material, and a chromium oxide coating is formed on the surface of the chromium oxynitride coating in an environment where an oxygen flow rate is 500 sccm.

8. The method according to claim 7, wherein during step (3), the current of the cathode electron gun needs to be increased over time, the initial current is 80A to 120A, and the increasing current is set to 1A / min-5A / min.

9. The method of claim 8, wherein a final value of the current of the cathode electron gun is less than or equal to 200A.

10. The method according to claim 7, wherein: During physical vapor deposition, the bias voltage was set to 100V to 200V.

11. The method according to claim 7, wherein: During physical vapor deposition, the temperature was set at 300-600°C.