Surface treatment method of permanent magnet, permanent magnet and protective film thereof

Through the double-layer process of zirconization treatment and passivation treatment, a moisture-resistant protective film is formed, which solves the corrosion problem of permanent magnet materials in humid environments, achieves high surface tension and corrosion resistance, and meets the bonding needs of the automotive field. In line with the concept of environmentally friendly production.

CN115584496BActive Publication Date: 2024-10-29FUJIAN CHANGTING GOLDEN DRAGON RARE EARTH CO LTD
View PDF 23 Cites 0 Cited by

Patent Information

Application Number
CN202211309391.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-25
Publication Date
2024-10-29
Estimated Expiration
2042-10-25

AI Technical Summary

Technical Problem

Existing permanent magnet materials are prone to corrosion in humid environments, resulting in a decrease in magnetic performance. Moreover, traditional coatings have uneven surfaces and poor corrosion resistance, making it difficult to meet high surface tension and moisture resistance requirements at the same time. Especially in automotive applications, there are bonding problems. .

Method used

Using a double-layer process of zirconium treatment and passivation treatment, a dense covering layer is formed through the zirconium film, and a passivation film is formed on it to repair cracks and defects, forming a moisture-resistant protective film. The zirconium treatment temperature is 5-40 ℃, the time is 5-30 minutes, pH value is 1.5-6, passivation treatment temperature is 15-50°C, time is 4-12 minutes, pH value is greater than or equal to 10, use special zirconium agent for rare earth NdFeB materials and weak acid passivation agent.

Benefits of technology

It achieves the formation of a uniform, dense and corrosion-resistant protective film on the surface of the permanent magnet. The moisture resistance time exceeds 7 cycles (168 hours), and the surface tension reaches more than 38mN/m. It conforms to the concept of green and environmentally friendly production and reduces pollutant emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115584496B_ABST
    Figure CN115584496B_ABST
Patent Text Reader

Abstract

The invention discloses a surface treatment method of a permanent magnet, a permanent magnet and a protective film thereof. The surface treatment method of the permanent magnet comprises the following steps: S1, zirconizing the permanent magnet to obtain a permanent magnet with a zirconized film; the temperature of the zirconization treatment is 5-40°C, the time is 5-30min, and the pH value of the zirconization treatment is 1.5-6; S2, passivating the permanent magnet with the zirconized film and drying it; the temperature of the passivation treatment is 15-50°C, the time is 4-12min, and the pH value is greater than or equal to 10. Through the treatment method of the present invention, the permanent magnet obtained has good moisture resistance and large surface tension at the same time; the treatment method of the present invention reduces pollutant emissions and conforms to the green ecological and environmental protection production concept.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a surface treatment method of a permanent magnet, a permanent magnet and a protective film thereof. Background Art

[0002] Permanent magnet material is a porous material prepared by powder metallurgy process. The neodymium-rich phase, neodymium iron boron main phase and boundary phase are prone to intergranular corrosion. In humid air, the crystal particles of the magnet are oxidized and broken, causing failure, which eventually leads to the decline or damage of the magnetic properties of the material, seriously affecting the service life of the permanent magnet and reducing the stability and reliability of the product.

[0003] With the continuous improvement of energy conservation, environmental protection and sewage discharge requirements at home and abroad, the traditional ternary phosphating pretreatment materials for coating are gradually banned by local regulations due to the presence of pollutants such as P, Mn, Ni, etc. The new green phosphorus-free conversion film technology has gradually matured and developed rapidly. This process can completely avoid the use of harmful substances such as P, Mn, Ni, nitrite, etc. However, the coating surface prepared by the existing zirconium salt pretreatment process is uneven, the corrosion resistance is not high, and after high temperature and high pressure test, wet heat test and neutral salt spray test, its anti-corrosion effect is poor.

[0004] In addition, in automotive applications, magnets need to be glued and assembled with other workpieces. For this reason, this type of application has higher requirements for the adhesiveness of the magnet surface protective film. For example, in car audio, the surface tension of the magnet needs to reach 38mN / m or more to meet the adhesive requirements during assembly. However, although conventional organic coatings have a certain degree of moisture resistance, their surface energy is low, which makes it difficult for the surface tension of the coating to reach a high level.

[0005] Therefore, when preparing a protective film on the surface of NdFeB, it is necessary not only to consider that the protective film has better protection in conventional environments and high temperature and high humidity environments, that is, good moisture resistance, but also good surface tension to meet the requirements of subsequent processing. Summary of the invention

[0006] In order to overcome the defects of the prior art that permanent magnet materials are difficult to have good moisture resistance and surface tension at the same time, and the preparation process has large pollution, a surface treatment method, a permanent magnet and a protective film thereof are provided. Through the treatment method of the present invention, the obtained permanent magnet has good moisture resistance and large surface tension at the same time; the treatment method of the present invention reduces pollutant emissions and conforms to the green ecological and environmental protection production concept.

[0007] The present invention solves the above technical problems through the following technical solutions.

[0008] The present invention provides a surface treatment method for a permanent magnet, which comprises the following steps:

[0009] S1. Performing zirconization treatment on the permanent magnet to obtain a permanent magnet with a zirconization film; the temperature of the zirconization treatment is 5-40° C., the time of the zirconization treatment is 5-30 min; the pH value of the zirconization treatment is 1.5-6;

[0010] S2. Passivating the permanent magnet with the zirconium film and drying it; the temperature of the passivation treatment is 15-50° C., the time of the passivation treatment is 4-12 minutes, and the pH value of the passivation treatment is greater than or equal to 10.

[0011] In S1, preferably, the zirconization treatment is performed by immersing the permanent magnet in an aqueous solution containing a zirconization agent.

[0012] Among them, the zirconizing agent can be a conventional zirconizing agent in the art; preferably, the zirconizing agent includes fluorozirconate and / or fluorozirconic acid; more preferably, the zirconizing agent is a special zirconizing agent for rare earth neodymium iron boron materials, which comes from Hainan Hongxiang Industrial Co., Ltd.

[0013] Preferably, the concentration of the aqueous solution containing the zirconizing agent is 10%-60%, and the concentration of the aqueous solution containing the zirconizing agent is the mass percentage of the zirconizing agent in the aqueous solution containing the zirconizing agent.

[0014] The immersion may be direct immersion or indirect immersion. The direct immersion refers to immersing the permanent magnet in the aqueous solution containing the zirconizing agent. The indirect immersion is preferably drum immersion. The drum immersion refers to placing the permanent magnet in a drum and then immersing it in the aqueous solution containing the zirconizing agent, and rotating the drum during the treatment process so that all surfaces of the permanent magnet are fully in contact with the zirconizing agent.

[0015] In S1, preferably, the temperature of the zirconization treatment is 20-30°C.

[0016] In S1, preferably, the zirconization treatment time is 10-25 min, more preferably 15 min-20 min.

[0017] In S1, the adhesion effect of the zirconization film on the permanent magnet is related to the concentration of the aqueous solution containing the zirconization agent, the pH value, temperature, time of the zirconization treatment and the surface cleanliness of the permanent magnet.

[0018] In S2, preferably, before the passivation treatment, the permanent magnet with the zirconium film is sequentially washed and dried for a third time.

[0019] Preferably, the third washing time is 10-20 seconds.

[0020] Preferably, the overflow water flow rate of the third water washing is 100 cubic meters per hour.

[0021] Preferably, the drying temperature is 80°C.

[0022] Preferably, the drying time is 30 minutes.

[0023] In S2, the passivation treatment is physical passivation; compared with other passivation processes, the passivation treatment of the present invention can be performed at a lower temperature.

[0024] In S2, preferably, the passivation treatment is carried out in an aqueous solution containing a passivating agent.

[0025] Wherein, the passivator can be a conventional passivator in the art, preferably a mixture of weakly acidic organic acid salts and inorganic salts; wherein, the organic acid salt preferably includes one or more of trisodium citrate, sodium salicylate and tetrasodium EDTA; preferably, the inorganic salt is preferably barium titanate; more preferably, the passivator includes trisodium citrate, sodium salicylate, tetrasodium EDTA and barium titanate.

[0026] Preferably, the concentration of the aqueous solution containing the passivator is 10%-20%, and the concentration of the aqueous solution containing the passivator is the mass percentage of the passivator in the aqueous solution containing the passivator.

[0027] In S2, preferably, the temperature of the passivation treatment is 25-50°C, more preferably 25-30°C.

[0028] In S2, preferably, the passivation treatment time is 6-10 min, more preferably 8-10 min.

[0029] In S2, preferably, the passivation treatment is achieved by immersing or spraying; the immersion refers to immersing the permanent magnet in an aqueous solution containing a passivating agent; the spraying refers to spraying the aqueous solution containing a passivating agent on the permanent magnet.

[0030] In S2, preferably, the drying temperature is 70-90°C, more preferably 75-85°C.

[0031] In S2, preferably, the drying time is 25-40 minutes, more preferably 25-35 minutes.

[0032] In the present invention, the preparation process includes zirconization treatment and passivation treatment; after the zirconization treatment, a layer of locally dense zirconization film will be formed on the surface of the permanent magnet, but dried cracks will appear on its surface; the passivation film formed after the passivation treatment can cover its surface to form a closed layer, which will not damage the zirconization film, but can also seal and fill the defects or weak points of the zirconization film and repair the cracks of the zirconization film. The above inner and outer layers cooperate with each other to form a moisture-resistant protective film.

[0033] In the present invention, the aqueous solution containing the zirconizing agent is acidic, and the aqueous solution containing the passivating agent is alkaline. During the treatment process, mutual contamination between the two needs to be avoided.

[0034] In the present invention, the permanent magnet may be pretreated before the zirconization treatment; wherein, preferably, the pretreatment steps include in sequence: ① grinding; ② degreasing; ③ first water washing; ④ pickling and rust removal; ⑤ second water washing; ⑥ ultrasonic deashing.

[0035] In step ①, the grinding can be a conventional operation in the art.

[0036] In step ①, preferably, a rust inhibitor is added during the grinding process.

[0037] Wherein, the rust inhibitor can be a conventional rust inhibitor in the art; preferably, the rust inhibitor includes one or more of sodium phosphate, sodium carbonate, sodium hydroxide and OP-10 emulsifier; more preferably, the concentration of sodium phosphate is 60-80g / L, sodium carbonate is 40-60g / L, sodium hydroxide is 5-10g / L or OP-10 emulsifier is 0.05-1g / L.

[0038] In step ①, preferably, the grinding is carried out in a vibrating grinder.

[0039] In step ①, preferably, the grinding temperature is 10-40°C.

[0040] In step ①, preferably, the grinding time is 2-36h.

[0041] In step ②, the degreasing can be a conventional operation in the art.

[0042] In step ②, preferably, degreasing powder is added during the degreasing process.

[0043] Wherein, the degreasing powder may be conventional degreasing powder in the art.

[0044] In step ②, preferably, the degreasing temperature is 45-55°C.

[0045] In step ②, preferably, the degreasing time is 3-7 minutes.

[0046] In step ③, the first water washing can be a conventional operation in the art.

[0047] In step ③, preferably, the first water washing is carried out in the first water washing tank and the second water washing tank respectively.

[0048] In step ③, preferably, the first washing time is 10-20 seconds.

[0049] In step ③, preferably, the overflow water flow rate of the first water wash is 100 cubic meters per hour.

[0050] In step ④, preferably, the pickling and rust removal time is 30-50s.

[0051] In step ④, preferably, the acid used for pickling and rust removal is dilute nitric acid; more preferably, the concentration of the dilute nitric acid is 1%-3%.

[0052] In step ④, the pickling and rust removal is to remove the oxide layer on the surface of the permanent magnet, so as to facilitate the subsequent zirconization film to better cover the surface of the permanent magnet.

[0053] In step ⑤, the first water washing can be a conventional operation in the art.

[0054] In step ⑤, preferably, the second water washing is carried out in the third water washing tank.

[0055] In step ⑤, preferably, the second washing time is 10-20 seconds.

[0056] In step ⑤, preferably, the overflow water flow rate of the second water washing is 100 cubic meters per hour.

[0057] In step ⑥, preferably, the ultrasonic deashing is carried out in the fourth water washing tank.

[0058] In step ⑥, preferably, an ultrasonic protective agent is added before the ultrasonic deashing. During the ultrasonic deashing process, adding an ultrasonic protective agent can achieve a better ultrasonic effect, and the magnet surface is more clean, which is conducive to subsequent film formation.

[0059] Wherein, the ultrasonic protective agent is a conventional ultrasonic protective agent in the art; preferably, the concentration of the ultrasonic protective agent is 0.1-1%, and the concentration of the ultrasonic protective agent is the mass percentage of the ultrasonic protective agent in the washing water of the fourth washing tank.

[0060] In step ⑥, preferably, the ultrasonic deashing time is 2-5 minutes.

[0061] The present invention also provides a permanent magnet, which is obtained by using the surface treatment method of the permanent magnet as described above.

[0062] The present invention also provides a permanent magnet protective film, which is obtained by the surface treatment method of the permanent magnet as described above.

[0063] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0064] The reagents and raw materials used in the present invention are commercially available.

[0065] The positive and progressive effects of the present invention are:

[0066] 1. By adopting the process of the present invention, a chemically extremely stable protective film can be formed on the surface of the NdFeB material in a short time. The protective film has excellent corrosion resistance, dense and uniform film crystals, and good rust resistance. In the condensation test of alternating air temperature and humidity (AHT test), the moisture resistance time of the permanent magnet reaches more than 7 cycles (168h), and the appearance does not change color or have rust spots after the test.

[0067] 2. The protective film on the surface of the permanent magnet obtained by the process of the present invention also has a large surface tension and has good adhesion in the subsequent application of the permanent magnet.

[0068] 3. The process of the present invention is in line with the green ecological and environmental protection production concept, avoiding the problem of sediment and the emission of a large amount of pollutants.

[0069] 4. By adopting the process of the present invention, a double-layer surface protection film of a zirconization layer and a passivation layer is obtained, which has better uniformity and appearance consistency. BRIEF DESCRIPTION OF THE DRAWINGS

[0070] Figure 1 These are sample photos of the product prepared in Example 1 before and after being tested in a wet heat chamber for 15 cycles (360 hours).

[0071] Figure 2 These are sample photos of the product prepared in Comparative Example 1 before and after being tested in a wet heat chamber for 4 cycles (96 hours).

[0072] Figure 3 These are sample photos of the product prepared in Comparative Example 2 before and after being tested in a wet heat chamber for 5 cycles (120 hours). DETAILED DESCRIPTION

[0073] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0074] Example 1

[0075] This embodiment is a surface treatment method for a permanent magnet, which comprises the following steps:

[0076] S0, pre-processing the permanent magnet comprises the following steps:

[0077] ①Put the permanent magnet into a vibration grinder and add a rust inhibitor for grinding. The grinding temperature is 25°C and the grinding time is 10 hours. The rust inhibitor is 70g / L sodium phosphate, 50g / L sodium carbonate and 8g / L sodium hydroxide.

[0078] ② Mix the ground permanent magnet with degreasing powder and degrease it at a temperature of 50°C for 5 minutes;

[0079] ③ Place the degreased permanent magnet in the first washing tank and the second washing tank in turn for the first washing. The first washing time is 20 seconds, and the overflow water flow rate of the first washing is 100 cubic meters per hour;

[0080] ④ Use 3% dilute nitric acid to pickle and remove rust from the permanent magnet after the first water washing. The pickling and rust removal time is 40s;

[0081] ⑤ Place the permanent magnet after pickling and rust removal in the third water washing tank for a second water washing. The second water washing time is 10s, and the overflow water flow rate of the second water washing is 100 cubic meters per hour;

[0082] ⑥ Place the permanent magnet after the second water washing in the fourth water washing tank, and add an ultrasonic protective agent for ultrasonic deashing. The ultrasonic deashing time is 4 minutes, the concentration of the ultrasonic protective agent is 0.5%, and the concentration of the ultrasonic protective agent is the mass percentage of the ultrasonic protective agent in the washing water of the fourth water washing tank;

[0083] S1, placing the pretreated permanent magnet S0 in a zirconizing agent with a concentration of 50%, zirconizing for 15 minutes at 25°C and a pH value of 3.8, and obtaining a zirconized permanent magnet by immersion coating; the concentration of the zirconizing agent is the mass percentage of the zirconizing agent in the aqueous solution containing the zirconizing agent; the zirconizing agent is a special zirconizing agent for rare earth neodymium iron boron materials, which comes from Hainan Hongxiang Industrial Co., Ltd. and includes fluorozirconate and fluorozirconic acid;

[0084] S2. Before the passivation treatment, the zirconized permanent magnet is washed and dried for the third time in sequence; the time of the third washing is 15 seconds; the overflow water flow of the third washing is 100 cubic meters per hour; the drying temperature is 80° C.; and the drying time is 30 minutes;

[0085] Subsequently, the zirconizing agent is immersed in a passivating agent with a concentration of 20% for 8 minutes at 25°C and a pH value greater than or equal to 10, and then dried at a temperature of 80°C for 30 minutes; the zirconizing agent is a mixture of trisodium citrate, sodium salicylate, tetrasodium EDTA and barium titanate.

[0086] Example 2

[0087] The permanent magnet is pretreated by adopting step S0 in embodiment 1;

[0088] S1, placing the pretreated permanent magnet S0 in a zirconizing agent with a concentration of 50%, zirconizing for 20 minutes at 5°C and a pH value of 3.5, and obtaining a zirconized permanent magnet by immersion coating; the concentration of the zirconizing agent is the mass percentage of the zirconizing agent in the aqueous solution containing the zirconizing agent; the zirconizing agent is a special zirconizing agent for rare earth neodymium iron boron materials, which comes from Hainan Hongxiang Industrial Co., Ltd. and includes fluorozirconate and fluorozirconic acid;

[0089] S2. Before the passivation treatment, the zirconized permanent magnet is sequentially washed and dried for the third time; the time of the third washing is 10 seconds; the overflow water flow of the third washing is 100 cubic meters per hour; the drying temperature is 80° C.; and the drying time is 30 minutes;

[0090] Subsequently, a passivation treatment is carried out by spraying in a passivating agent with a concentration of 20% at 50° C. and a pH value of 10 for 4 minutes, and then drying is carried out at a temperature of 80° C. for 30 minutes; the zirconizing agent is a mixture of trisodium citrate, sodium salicylate, tetrasodium EDTA and barium titanate.

[0091] Example 3

[0092] The permanent magnet is pretreated by adopting step S0 in embodiment 1;

[0093] S1, placing the pretreated permanent magnet S0 in a zirconizing agent with a concentration of 50%, zirconizing for 5 minutes at 40°C and a pH value of 3.5, and obtaining a zirconized permanent magnet by roller coating; the concentration of the zirconizing agent is the mass percentage of the zirconizing agent in the aqueous solution containing the zirconizing agent; the zirconizing agent is a special zirconizing agent for rare earth neodymium iron boron materials, which comes from Hainan Hongxiang Industrial Co., Ltd. and includes fluorozirconate and fluorozirconic acid;

[0094] S2. Before the passivation treatment, the zirconized permanent magnet is sequentially washed and dried for the third time; the time of the third washing is 20 seconds; the overflow water flow of the third washing is 100 cubic meters per hour; the drying temperature is 80° C.; and the drying time is 30 minutes;

[0095] Subsequently, the passivation treatment is carried out by immersion or spraying in a passivating agent with a concentration of 20% for 12 minutes at 15°C and a pH value of 10, and then drying is carried out at a temperature of 80°C for 30 minutes; the zirconizing agent is a mixture of trisodium citrate, sodium salicylate, tetrasodium EDTA and barium titanate.

[0096] Comparative Example 1

[0097] The existing phosphating process is adopted to perform phosphating treatment on the surface of the permanent magnet to obtain the permanent magnet.

[0098] Comparative Example 2

[0099] The treatment method of Example 1 is adopted. The difference between this comparative example and Example 1 is that the temperature of the zirconization treatment in step S1 is 50° C., and the time of the zirconization treatment is 40 minutes.

[0100] Comparative Example 3

[0101] The treatment method of Example 1 is adopted. The difference between this comparative example and Example 1 is that the pH value of the zirconization treatment in step S1 is 7.

[0102] Comparative Example 4

[0103] The treatment method of Example 1 is adopted. The difference between this comparative example and Example 1 is that the temperature of the passivation treatment in step S2 is 10° C., and the time of the passivation treatment is 10 minutes.

[0104] Comparative Example 5

[0105] The treatment method of Example 1 is adopted. The difference between this comparative example and Example 1 is that the pH value of the passivation treatment in step S2 is 9.

[0106] Effect Example 1

[0107] AHT Test

[0108] The permanent magnets of Examples 1 to 3 and Comparative Examples 1 to 5 were subjected to AHT tests, i.e., condensation tests under alternating air temperature and humidity. The results are as follows: Figures 1 to 3 And as shown in Table 1.

[0109] Figure 1 The product prepared in Example 1 is a sample before and after being tested in a wet heat chamber for 15 cycles (360 hours). Figure 1 (a) is the sample picture before testing. Figure 1 (b) is a sample picture after the test. The moisture resistance time of the permanent magnet of Example 1 can reach more than 15 cycles (360 hours), and the appearance does not change color or have rust spots after the test.

[0110] Figure 2 The permanent magnet prepared in Comparative Example 1 is a sample before and after being tested in a wet heat chamber for 4 cycles (96 hours). Figure 2 (a) is the sample picture before testing. Figure 2 (b) is a sample image after the test. After the permanent magnet of Comparative Example 1 has been in the wet heat box for 4 cycles (96 hours), although there are no rust spots on the surface, obvious discoloration has occurred, which is regarded as a precursor to corrosion failure.

[0111] Figure 3 The permanent magnet prepared in Comparative Example 2 is a sample before and after being tested in a wet heat chamber for 5 cycles (120 hours). Figure 3 (a) is the sample picture before testing. Figure 3(b) is a sample image after the test. After the permanent magnet of Comparative Example 2 was placed in a wet heat chamber for 5 cycles (120 h), obvious red rust spots appeared on the surface.

[0112] Table 1

[0113]

[0114]

[0115] Effect Example 2 Surface Tension Test

[0116] The surface tension of the permanent magnets of Examples 1-3 and Comparative Examples 1-5 was tested using a conventional dyne pen test method in the art, and the results shown in Table 2 were obtained:

[0117] Table 2

[0118] Surface tension (mN / m) Example 1 42 Example 2 40 Example 3 40 Comparative Example 1 40 Comparative Example 2 38 Comparative Example 3 38 Comparative Example 4 38 Comparative Example 5 38

[0119] It can be seen that the surface tension of the permanent magnet moisture-resistant protective film prepared by the treatment method of the present application can reach 40 mN / m or above.

Claims

1. A method for surface treatment of a permanent magnet, characterized in that: It includes the following steps: S1. Performing zirconization treatment on the permanent magnet to obtain a permanent magnet with a zirconization film; the temperature of the zirconization treatment is 5-40° C., the time of the zirconization treatment is 5-30 min; the pH value of the zirconization treatment is 1.5-6; S2, passivating the permanent magnet with zirconium film and drying it; the temperature of the passivation treatment is 15-50° C., the time of the passivation treatment is 4-12 minutes, and the pH value of the passivation treatment is greater than or equal to 10; The passivation treatment is carried out in an aqueous solution containing a passivating agent; The passivating agent is a mixture of weakly acidic organic acid salts and inorganic salts; wherein the organic acid salt includes one or more of trisodium citrate, sodium salicylate and tetrasodium EDTA; and the inorganic salt is barium titanate.

2. The surface treatment method of a permanent magnet according to claim 1, characterized in that: In S1, the zirconization treatment is performed by immersing the permanent magnet in an aqueous solution containing a zirconization agent; And / or, the temperature of the zirconization treatment is 20-30°C; And / or, the zirconization treatment time is 10-25min; And / or, the pH of the zirconization treatment is 3.2-5.

5.

3. The surface treatment method of a permanent magnet according to claim 2, characterized in that: In S1, the zirconating agent includes fluorozirconate and / or fluorozirconic acid; And / or, the concentration of the aqueous solution containing the zirconizing agent is 10%-60%, and the concentration of the aqueous solution containing the zirconizing agent is the mass percentage of the zirconizing agent in the aqueous solution containing the zirconizing agent; And / or, the immersion is direct immersion or indirect immersion; And / or, the zirconization treatment time is 15-20 minutes.

4. The surface treatment method of a permanent magnet according to claim 1, characterized in that: In S2, before the passivation treatment, the permanent magnet with the zirconium film is sequentially washed and dried for the third time; And / or, the temperature of the passivation treatment is 25-50°C; And / or, the passivation treatment time is 6-10min; And / or, the passivation treatment is achieved by immersion or spraying; And / or, the drying temperature is 70-90°C; And / or, the drying time is 25-40 minutes.

5. The surface treatment method of a permanent magnet according to claim 4, characterized in that: In S2, the third washing time is 10-20 seconds; And / or, the overflow water flow rate of the third water washing is 100 cubic meters per hour; And / or, the drying temperature is 80°C; And / or, the drying time is 30 min; and / or, the passivating agent comprises trisodium citrate, sodium salicylate, tetrasodium EDTA and barium titanate; And / or, the concentration of the aqueous solution containing the passivator is 10%-20%, and the concentration of the aqueous solution containing the passivator is the mass percentage of the passivator in the aqueous solution containing the passivator; And / or, the temperature of the passivation treatment is 25-30°C; And / or, the passivation treatment time is 8-10min; And / or, the drying temperature is 75-85°C; And / or, the drying time is 25-35 minutes.

6. The surface treatment method of a permanent magnet according to claim 1, characterized in that: The permanent magnet is pretreated before the zirconization treatment; wherein the pretreatment steps include in sequence: ① grinding; ② degreasing; ③ first water washing; ④ pickling and rust removal; ⑤ second water washing; ⑥ ultrasonic deashing.

7. The surface treatment method of a permanent magnet according to claim 6, characterized in that: In step ①, adding a rust inhibitor during the grinding process; And / or, in step ①, the grinding is carried out in a vibrating grinder; And / or, in step ①, the grinding temperature is 10-40°C; And / or, in step ①, the grinding time is 2-36h; and / or, in step ②, adding degreasing powder during the degreasing process; And / or, in step ②, the degreasing temperature is 45-55°C; And / or, in step ②, the degreasing time is 3-7 minutes; And / or, in step ③, the first water washing is carried out in the first water washing tank and the second water washing tank respectively; And / or, in step ③, the first washing time is 10-20 seconds; And / or, in step ③, the overflow water flow rate of the first water wash is 100 cubic meters per hour; And / or, in step ④, the pickling and rust removal time is 30-50s; And / or, in step ④, the acid used for pickling and rust removal is dilute nitric acid; And / or, in step ⑤, the second water washing is carried out in a third water washing tank; And / or, in step ⑤, the second washing time is 10-20 seconds; And / or, in step ⑤, the overflow water flow rate of the second water washing is 100 cubic meters per hour; And / or, in step ⑥, the ultrasonic deashing is carried out in the fourth washing tank; And / or, in step ⑥, before the ultrasonic deashing, an ultrasonic protective agent is added; And / or, in step ⑥, the ultrasonic deashing time is 2-5 minutes.

8. The surface treatment method of a permanent magnet according to claim 7, characterized in that: In step ①, the rust inhibitor includes one or more of sodium phosphate, sodium carbonate, sodium hydroxide and OP-10 emulsifier; And / or, in step ④, the concentration of the dilute nitric acid is 1%-3%; And / or, in step ⑥, the concentration of the ultrasonic protective agent is 0.1-1%, and the concentration of the ultrasonic protective agent is the mass percentage of the ultrasonic protective agent to the washing water in the fourth washing tank.

9. The surface treatment method of a permanent magnet according to claim 8, characterized in that: The concentration of the sodium phosphate is 60-80 g / L, the concentration of the sodium carbonate is 40-60 g / L, the concentration of the sodium hydroxide is 5-10 g / L or the concentration of the OP-10 emulsifier is 0.05-1 g / L.

10. A permanent magnet, characterized in that: The permanent magnet is obtained by using the surface treatment method of the permanent magnet as described in any one of claims 1 to 9.

11. A permanent magnet protective film, characterized in that: The permanent magnet is obtained by the surface treatment method of the permanent magnet as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Steel ultra-low temperature multifunctional derusting phosphatization antirust solution

    CN101660149A

  • Nd-Fe-B magnet material double-layered protecting method employing titanium / zirconium conversion coating and organic coating

    CN102400125A

  • Zirconate surface treatment technology of permanent magnet

    CN102453890A

  • Surface treatment method of sintered neodymium-iron-boron magnetic materials

    CN102605361A

  • Stainless steel passivation water solution and preparation method thereof

    CN102899653A