A kind of anti-ultraviolet and oxygen-blocking protective liquid and nano-silver conductive film

By using an ultraviolet-resistant and oxygen-retardant protective liquid in the nano-silver conductive film, including nano-zinc oxide particles and nano-copper powder, the problem of easy oxidation of nano-silver wires is solved, and the service life and performance of the conductive film are improved.

CN115588526BActive Publication Date: 2024-11-29SHENZHEN HUAKE COMM TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211345652.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-31
Publication Date
2024-11-29
Estimated Expiration
2042-10-31

AI Technical Summary

Technical Problem

Nanosilver wires in nano-silver conductive films are easily oxidized, and long-term light will cause touch failure, jump points, and affect service life and performance.

Method used

A protective layer of nano-silver conductive film is prepared by optimizing its particle size and proportion to prevent nano-silver conductive film from oxidizing.

Benefits of technology

Effectively resist ultraviolet and oxygen resistance, prevent nano silver wires from being oxidized in nano-silver conductive film, improve service life and performance, and ensure the stability and durability of the conductive film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115588526B_ABST
    Figure CN115588526B_ABST
Patent Text Reader

Abstract

The present invention provides an anti-ultraviolet and oxygen-blocking protective liquid, the protective liquid comprising the following components in percentage by mass: 15-25% of nano zinc oxide particles, 4-6% of nano copper powder, and the remainder being a solvent; the particle size of the nano zinc oxide particles is 45-65nm. The present invention also provides a nano silver conductive film. The protective liquid of the present invention can effectively resist ultraviolet rays and oxygen, prevent the nano silver wires in the nano silver conductive film from being oxidized, ensure the stability of its square resistance, and improve the service life and performance; and the preparation process is clean and efficient, and the controllability is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of conductive films, and in particular relates to an anti-ultraviolet and oxygen-blocking protective liquid and a nano-silver conductive film. Background Art

[0002] With the promotion and application of large-size capacitive screens, nano silver wire conductive film has become the main material for touch TP due to its low resistance, high transmittance and low cost. However, due to the differences in the environment in which it is located, the film material cannot be repaired if it fails, so ensuring the stability of the nano silver wire is crucial to product performance and service life.

[0003] The nanosilver wires in the nanosilver conductive film are easily oxidized. If the nanosilver capacitive screen is not protected, long-term exposure to light can easily lead to touch failure and point jump. Therefore, it is necessary to effectively isolate the nanosilver wires in the nanosilver conductive film from ultraviolet rays and oxygen, so as to improve the service life and use effect of the nanosilver conductive film. Summary of the invention

[0004] Based on this, the purpose of the present invention is to provide an anti-ultraviolet and oxygen-blocking protective liquid, which can effectively inhibit the oxidation of nano silver wires and improve the service life and use effect of nano silver conductive films.

[0005] To achieve the above object, the present invention adopts the following technical solution.

[0006] An anti-ultraviolet and oxygen-blocking protective liquid comprises the following components in percentage by mass: 15-25% of nano zinc oxide particles, 4-6% of nano copper powder, and the remainder is solvent; the particle size of the nano zinc oxide particles is 45-65nm.

[0007] In some preferred embodiments, the particle size of the nano zinc oxide particles is 50-60 nm.

[0008] In some embodiments, the particle size of the nano copper powder is 30-60 nm.

[0009] In some embodiments, the solvent comprises isopropanol, ethanol, and diacetone alcohol, and the weight ratio of the isopropanol, ethanol, and diacetone alcohol is (8-9):(0.75-1):(0.25-1).

[0010] The present invention also provides the use of the above-mentioned anti-ultraviolet and oxygen-blocking protective liquid in the preparation of nano silver conductive film.

[0011] The present invention also provides a nano silver conductive film, which comprises a base film, and one side of the base film is provided with a nano silver wire layer and a protective layer comprising the protective liquid as described above in sequence.

[0012] In some embodiments, the dry film thickness of the silver nanowire layer is 100-150 nm; and / or the dry film thickness of the protective layer is 80-100 nm.

[0013] In some embodiments, the solid content of the silver nanowire layer is 0.3-0.5%.

[0014] In some embodiments, the diameter of the silver nanowires in the silver nanowire layer is 20-25 nm, and the length is 30-35 μm.

[0015] The present invention also provides a method for preparing the nanosilver conductive film as described above, comprising the following steps: (1) preparing a nanosilver wire dispersion liquid, coating it on one side of the substrate, and drying it to form the nanosilver wire layer; (2) coating the protective liquid as described above on the nanosilver wire layer, and curing it to form the protective layer to obtain the nanosilver conductive film.

[0016] The present invention obtains an anti-ultraviolet and oxygen-blocking protective liquid through optimization, and the protective liquid contains nano zinc oxide particles and nano copper powder in a suitable ratio. The inventor also found through research that the particle size of the nano zinc oxide particles has a significant effect on the anti-ultraviolet and oxygen-blocking effects of the protective liquid, and screened and obtained a suitable particle size range, so that the protective liquid has a strong scattering effect on ultraviolet light. The protective liquid of the present invention can effectively resist ultraviolet rays and oxygen, prevent the nano silver wires in the nano silver conductive film from being oxidized, ensure the stability of its square resistance, and improve the service life and performance; and the preparation process is clean and efficient, and the controllability is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a SEM effect diagram of the nanosilver conductive film prepared in Example 1 without xenon lamp test.

[0018] Figure 2 This is the SEM effect diagram of the nanosilver conductive film prepared in Example 1 subjected to a xenon lamp test for 100 hours.

[0019] Figure 3 This is a SEM effect diagram of the nanosilver conductive film prepared in Comparative Example 3 without xenon lamp test.

[0020] Figure 4 This is the SEM effect diagram of the xenon lamp test for 100 hours on the nano-silver conductive film prepared in Comparative Example 3. DETAILED DESCRIPTION

[0021] The experimental methods in the following examples of the present invention, where no specific conditions are specified, are usually carried out under conventional conditions or under conditions recommended by the manufacturers. The various commonly used chemical reagents used in the examples are all commercially available products.

[0022] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0023] The terms "including" and "having" and any variations thereof of the present invention are intended to cover non-exclusive inclusions. For example, a process, method, device, product or equipment comprising a series of steps is not limited to the listed steps or modules, but may optionally include steps not listed, or may optionally include other steps inherent to these processes, methods, products or equipment.

[0024] In the present invention, the term "multiple" refers to two or more than two. "And / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent the following three situations: A exists alone, A and B exist at the same time, and B exists alone. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0025] The following describes the invention in conjunction with specific embodiments.

[0026] Example 1

[0027] This embodiment provides an anti-ultraviolet and oxygen-blocking protective liquid, which contains the following components in percentage by mass: 20% of nano zinc oxide particles, 5% of nano copper powder, and the balance is solvent;

[0028] The particle size of the nano zinc oxide particles is 50-60nm; the particle size of the nano copper powder is 30-60nm;

[0029] The solvent comprises isopropyl alcohol, ethanol, and diacetone alcohol, and the weight ratio of the isopropyl alcohol, ethanol, and diacetone alcohol is 8.5:0.9:0.75.

[0030] The anti-ultraviolet and anti-oxygen protective liquid is prepared by the following method:

[0031] (1) Heat methanol to 65°C, add zinc acetate dihydrate and stir at a constant speed until dissolved. Add methanol dropwise to the KOH solution at 60°C within 15 minutes. Stir the reaction mixture at 65-70°C for 2.5 hours; after cooling to room temperature, pour out the supernatant, wash the precipitate twice with methanol, filter the nano zinc oxide particle solution through a 0.45mm PVDF syringe filter and add it to a centrifuge tube, centrifuge at a speed of 5000r / min for 5 minutes, remove the supernatant, dry and solidify to obtain nano zinc oxide particles with a particle size of 50-60nm;

[0032] (2) Quantitatively weigh copper sulfate and polyvinyl pyrrolidone (PVP) and dissolve them in a reactor with deionized water, control the concentration of copper sulfate to 0.2-0.3 mol / L, and the amount of PVP to 10% of the mass of CuSO4·5H2O, then add antioxidants, adjust the pH value, and prepare solution A. Weigh a certain amount of reducing agent and add it to deionized water to prepare a hydrazine hydrate solution of 4.12 mol / L, i.e., solution B. Slowly drip solution B into solution A, control the temperature at 30-35°C and stir magnetically. After the addition is completed, continue stirring for 10-20 minutes, and the reaction is completed. After standing and cooling, centrifuge to separate the copper powder, wash it with anhydrous ethanol three times, and the obtained nano copper powder has a spherical morphology, good dispersibility, and a particle size of about 30-60nm.

[0033] (3) Preparation of 1 kg of anti-ultraviolet and anti-oxygen protective liquid: Take 200 g of the above-mentioned nano zinc oxide particles and 50 g of nano copper powder, add them to the solvent (remainder), stir them thoroughly, and mix them using an oscillator to obtain the protective liquid.

[0034] The present embodiment also provides a nanosilver conductive film, which is prepared by the following method: (1) preparing a nanosilver wire (diameter 20-25 nm, length 30-35 μm) dispersion with a solid content of 0.5%, and then coating it on one side of a PET substrate, drying it to form a nanosilver wire layer with a dry film thickness of 120 nm; (2) coating the above-mentioned protective liquid on the nanosilver wire layer, curing it to form a protective layer with a dry film thickness of 90 nm, thereby obtaining the nanosilver conductive film.

[0035] Example 2

[0036] This embodiment provides an anti-ultraviolet and oxygen-blocking protective liquid, which contains the following components in percentage by mass: 22% of nano zinc oxide particles, 4.5% of nano copper powder, and the balance is solvent;

[0037] The particle size of the nano zinc oxide particles is 50-60nm; the particle size of the nano copper powder is 30-60nm;

[0038] The solvent comprises isopropyl alcohol, ethanol, and diacetone alcohol, and the weight ratio of the isopropyl alcohol, ethanol, and diacetone alcohol is 8.5:0.9:0.75.

[0039] The anti-ultraviolet and anti-oxygen protective liquid is prepared by the following method:

[0040] (1) Heat methanol to 65°C, add zinc acetate dihydrate and stir at a constant speed until dissolved. Add methanol dropwise to the KOH solution at 60°C within 15 minutes. Stir the reaction mixture at 65-70°C for 2.5 hours; after cooling to room temperature, pour out the supernatant, wash the precipitate twice with methanol, filter the nano zinc oxide particle solution through a 0.45mm PVDF syringe filter and add it to a centrifuge tube, centrifuge at a speed of 5000r / min for 5 minutes, remove the supernatant, dry and solidify to obtain nano zinc oxide particles with a particle size of 50-60nm;

[0041] (2) Quantitatively weigh copper sulfate and polyvinyl pyrrolidone (PVP) and dissolve them in a reactor with deionized water, control the concentration of copper sulfate to 0.2-0.3 mol / L, and the amount of PVP to 10% of the mass of CuSO4·5H2O, then add antioxidants, adjust the pH value, and prepare solution A. Weigh a certain amount of reducing agent and add it to deionized water to prepare a hydrazine hydrate solution of 4.12 mol / L, i.e., solution B. Slowly drip solution B into solution A, control the temperature at 30-35°C and stir magnetically. After the addition is completed, continue stirring for 10-20 minutes, and the reaction is completed. After standing and cooling, centrifuge to separate the copper powder, wash it with anhydrous ethanol three times, and the obtained nano copper powder has a spherical morphology, good dispersibility, and a particle size of about 30-60nm.

[0042] (3) Preparation of 1 kg of anti-ultraviolet and anti-oxygen protective liquid: Take 220 g of the above-mentioned nano zinc oxide particles and 45 g of nano copper powder, add them to the solvent (remainder), stir them thoroughly, and mix them using an oscillator to obtain the protective liquid.

[0043] This embodiment also provides a nano silver conductive film, and the preparation method of the nano silver conductive film is the same as that of embodiment 1.

[0044] Example 3

[0045] This embodiment provides an anti-ultraviolet and anti-oxygen protective solution, which contains the following components in percentage by weight: 18% of nano zinc oxide particles, 6% of nano copper powder, and the remainder is a solvent;

[0046] The particle size of the nano zinc oxide particles is 50-60nm; the particle size of the nano copper powder is 30-60nm;

[0047] The solvent comprises isopropyl alcohol, ethanol, and diacetone alcohol, and the weight ratio of the isopropyl alcohol, ethanol, and diacetone alcohol is 8.5:0.9:0.75.

[0048] The anti-ultraviolet and anti-oxygen protective liquid is prepared by the following method:

[0049] (1) Heat methanol to 65°C, add zinc acetate dihydrate and stir at a constant speed until dissolved. Add methanol dropwise to the KOH solution at 60°C within 15 minutes. Stir the reaction mixture at 65-70°C for 2.5 hours; after cooling to room temperature, pour out the supernatant, wash the precipitate twice with methanol, filter the nano zinc oxide particle solution through a 0.45mm PVDF syringe filter and add it to a centrifuge tube, centrifuge at a speed of 5000r / min for 5 minutes, remove the supernatant, dry and solidify to obtain nano zinc oxide particles with a particle size of 50-60nm;

[0050] (2) Quantitatively weigh copper sulfate and polyvinyl pyrrolidone (PVP) and dissolve them in a reactor with deionized water, control the concentration of copper sulfate to 0.2-0.3 mol / L, and the amount of PVP to 10% of the mass of CuSO4·5H2O, then add antioxidants, adjust the pH value, and prepare solution A. Weigh a certain amount of reducing agent and add it to deionized water to prepare a hydrazine hydrate solution of 4.12 mol / L, i.e., solution B. Slowly drip solution B into solution A, control the temperature at 30-35°C and stir magnetically. After the addition is completed, continue stirring for 10-20 minutes, and the reaction is completed. After standing and cooling, centrifuge to separate the copper powder, wash it with anhydrous ethanol three times, and the obtained nano copper powder has a spherical morphology, good dispersibility, and a particle size of about 30-60nm.

[0051] (3) Preparation of 1 kg of anti-ultraviolet and anti-oxygen protective liquid: 180 g of the above-mentioned nano zinc oxide particles and 60 g of nano copper powder are added to the solvent (remainder), stirred thoroughly, and mixed using an oscillator to obtain the protective liquid.

[0052] This embodiment also provides a nano silver conductive film, and the preparation method of the nano silver conductive film is the same as that of embodiment 1.

[0053] Comparative Example 1

[0054] This comparative example provides an anti-ultraviolet and oxygen-blocking protective solution, which contains the following components in percentage by mass: 20% of nano zinc oxide particles, 5% of nano copper powder, and the balance is solvent;

[0055] The particle size of the nano zinc oxide particles is 80-100 nm; the particle size of the nano copper powder is 30-60 nm;

[0056] The solvent comprises isopropyl alcohol, ethanol, and diacetone alcohol, and the weight ratio of the isopropyl alcohol, ethanol, and diacetone alcohol is 8.5:0.9:0.75.

[0057] The anti-ultraviolet and anti-oxygen protective liquid is prepared by the following method:

[0058] (1) Heat methanol to 65°C, add zinc acetate dihydrate and stir at a constant speed until dissolved. Add methanol dropwise to the KOH solution at 60°C within 15 minutes. Stir the reaction mixture at 65-70°C for 2 hours; after cooling to room temperature, pour out the supernatant, wash the precipitate twice with methanol, filter the nano zinc oxide particle solution through a 0.75mm PVDF syringe filter and add it to a centrifuge tube. Centrifuge at a speed of 5000r / min for 5 minutes, remove the supernatant, dry and solidify to obtain nano zinc oxide particles with a particle size of 80-100nm;

[0059] (2) Quantitatively weigh copper sulfate and polyvinyl pyrrolidone (PVP) and dissolve them in a reactor with deionized water, control the concentration of copper sulfate to 0.2-0.3 mol / L, and the amount of PVP to 10% of the mass of CuSO4·5H2O, then add antioxidants, adjust the pH value, and prepare solution A. Weigh a certain amount of reducing agent and add it to deionized water to prepare a hydrazine hydrate solution of 4.12 mol / L, i.e., solution B. Slowly drip solution B into solution A, control the temperature at 30-35°C and stir magnetically. After the addition is completed, continue stirring for 10-20 minutes, and the reaction is completed. After standing and cooling, centrifuge to separate the copper powder, wash it with anhydrous ethanol three times, and the obtained nano copper powder has a spherical morphology, good dispersibility, and a particle size of about 30-60nm.

[0060] (3) Preparation of 1 kg of anti-ultraviolet and anti-oxygen protective liquid: Take 200 g of the above-mentioned nano zinc oxide particles and 50 g of nano copper powder, add them to the solvent (remainder), stir them thoroughly, and mix them using an oscillator to obtain the protective liquid.

[0061] This comparative example also provides a nano silver conductive film, and the preparation method of the nano silver conductive film is the same as that of Example 1.

[0062] Comparative Example 2

[0063] This comparative example provides an anti-ultraviolet and oxygen-blocking protective solution, which contains the following components in percentage by mass: 10% of nano zinc oxide particles, 5% of nano copper powder, and the balance is solvent;

[0064] The particle size of the nano zinc oxide particles is 50-60nm; the particle size of the nano copper powder is 30-60nm;

[0065] The solvent comprises isopropyl alcohol, ethanol, and diacetone alcohol, and the weight ratio of the isopropyl alcohol, ethanol, and diacetone alcohol is 8.5:0.9:0.75.

[0066] The anti-ultraviolet and anti-oxygen protective liquid is prepared by the following method:

[0067] (1) Heat methanol to 65°C, add zinc acetate dihydrate and stir at a constant speed until dissolved. Add methanol dropwise to the KOH solution at 60°C within 15 minutes. Stir the reaction mixture at 65-70°C for 2.5 hours; after cooling to room temperature, pour out the supernatant, wash the precipitate twice with methanol, filter the nano zinc oxide particle solution through a 0.45mm PVDF syringe filter and add it to a centrifuge tube, centrifuge at a speed of 5000r / min for 5 minutes, remove the supernatant, dry and solidify to obtain nano zinc oxide particles with a particle size of 50-60nm;

[0068] (2) Quantitatively weigh copper sulfate and polyvinyl pyrrolidone (PVP) and dissolve them in a reactor with deionized water, control the concentration of copper sulfate to 0.2-0.3 mol / L, and the amount of PVP to 10% of the mass of CuSO4·5H2O, then add antioxidants, adjust the pH value, and prepare solution A. Weigh a certain amount of reducing agent and add it to deionized water to prepare a hydrazine hydrate solution of 4.12 mol / L, i.e., solution B. Slowly drip solution B into solution A, control the temperature at 30-35°C and stir magnetically. After the addition is completed, continue stirring for 10-20 minutes, and the reaction is completed. After standing and cooling, centrifuge to separate the copper powder, wash it with anhydrous ethanol three times, and the obtained nano copper powder has a spherical morphology, good dispersibility, and a particle size of about 30-60nm.

[0069] (3) Preparation of 1 kg of anti-ultraviolet and anti-oxygen protective liquid: Take 200 g of the above-mentioned nano zinc oxide particles and 50 g of nano copper powder, add them to the solvent (remainder), stir them thoroughly, and mix them using an oscillator to obtain the protective liquid.

[0070] This comparative example also provides a nano silver conductive film, and the preparation method of the nano silver conductive film is the same as that of Example 1.

[0071] Comparative Example 3

[0072] This comparative example provides a nanosilver conductive film, which is prepared by the following method: preparing a nanosilver wire (diameter 20-25nm, length 30-35μm) dispersion with a solid content of 0.5%, then coating it on one side of a PET substrate, and drying it to form a nanosilver wire layer with a dry film thickness of 120nm, thereby obtaining the nanosilver conductive film.

[0073] The performance of the nanosilver film of the nanosilver conductive film in the above embodiments and comparative examples was tested using a xenon lamp aging box to obtain relevant weather resistance test results, and its square resistance change rate was tested and failure observation was performed using a scanning electron microscope to determine whether the silver wire was broken and failed.

[0074] The square resistance change rate test method is: test the resistance of the initial film material, use Suzhou lattice four-probe tester to test the resistance of the film material, record the test data of 5 points, and take the average. Further, according to the test time requirements, perform the same square resistance test on the film material in the xenon lamp box and record the data.

[0075] The test results of square resistance change rate are shown in Table 1:

[0076] Table 1 Test results of square resistance change rate

[0077]

[0078]

[0079] The above results show that the square resistance change of the nanosilver conductive film (Examples 1 to 3) of the present invention is still less than 2% after being treated with double 85 xenon lamps for 100 hours, indicating that the protective solution of the present invention can effectively resist ultraviolet and oxygen and prevent the nanosilver film from failing.

[0080] Compared with Example 1, the particle size of the nano zinc oxide particles in the protective solution used for the nano silver conductive film prepared in Comparative Example 1 is too large, and the ultraviolet scattering effect of the particles becomes weak, resulting in poor anti-ultraviolet protection effect on the conductive film in a simulated sunlight environment.

[0081] Compared with Example 1, the amount of the nano zinc oxide particles in the protective solution used in the nano silver conductive film prepared in Comparative Example 2 is too low, so that the film material is more likely to turn yellow and fail in the aging experiment.

[0082] Compared with Example 1, the nanosilver conductive film prepared in Comparative Example 3 does not contain a protective layer. After being treated with a double 85 xenon lamp for 10 hours, its square resistance changes by more than 50%; after being treated with a double 85 xenon lamp for 50 hours, its resistance value is unstable and slightly yellowed; after being treated with a double 85 xenon lamp for 100 hours, it turns yellow and becomes ineffective. The SEM effect picture of the nanosilver conductive film prepared in Example 1 without the xenon lamp test is shown in the figure below. Figure 1 As shown in the SEM effect diagram of the xenon lamp test for 100 hours Figure 2 The SEM effect diagram of the nano silver conductive film prepared in Comparative Example 3 without xenon lamp test is shown in Figure 3 As shown in the SEM effect diagram of the xenon lamp test for 100 hours Figure 4 shown.

[0083] In summary, the protective liquid of the present invention can effectively resist ultraviolet rays and oxygen, prevent the nanosilver wires in the nanosilver conductive film from being oxidized, ensure the stability of its square resistance, and improve the service life and performance.

[0084] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0085] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. An anti-ultraviolet and oxygen-blocking protective liquid, characterized in that: The protective solution comprises the following components in percentage by weight: 15-25% of nano zinc oxide particles, 4-6% of nano copper powder, and the remainder is solvent; the particle size of the nano zinc oxide particles is 45-65nm; the particle size of the nano copper powder is 30-60nm; the solvent comprises isopropanol, ethanol, and diacetone alcohol, and the weight ratio of the isopropanol, ethanol, and diacetone alcohol is (8-9):(0.75-1):(0.25-1).

2. The anti-ultraviolet and anti-oxygen protective liquid according to claim 1, characterized in that: The particle size of the nano zinc oxide particles is 50-60nm.

3. Use of the anti-ultraviolet and oxygen-blocking protective solution as claimed in any one of claims 1 to 2 in the preparation of nano-silver conductive films.

4. A nano silver conductive film, characterized in that: The nanosilver conductive film comprises a substrate, and a nanosilver wire layer and a protective layer comprising the protective solution according to any one of claims 1 to 2 are sequentially provided on one side of the substrate.

5. The nanosilver conductive film according to claim 4, characterized in that: The dry film thickness of the nano silver wire layer is 100-150 nm; and / or the dry film thickness of the protective layer is 80-100 nm.

6. The nanosilver conductive film according to claim 4, characterized in that: The solid content of the nano silver wire layer is 0.3-0.5%.

7. The nanosilver conductive film according to claim 4, characterized in that: The diameter of the nano silver wires in the nano silver wire layer is 20-25 nm, and the length is 30-35 μm.

8. The method for preparing a nano silver conductive film according to any one of claims 4 to 7, characterized in that: The following steps are involved: (1) preparing a nano silver wire dispersion, and then coating it on one side of the substrate, and curing it to form the nano silver wire layer; (2) coating the protective liquid according to any one of claims 1 to 2 on the nano silver wire layer, and curing it to form the protective layer, thereby obtaining the nano silver conductive film.

Citation Information

Patent Citations

  • Method for protecting silver nanowire heating film

    CN113411923A