A short-process manufacturing process for ultra-high-power giant wind turbine hollow main shaft

Through the multi-element synergistic ratio and upsetting-drawing-rolling forging process, the problems of hydrogen-induced cracking of wind power spindles and lengthy manufacturing processes are solved, energy saving, material saving and performance improvement are achieved, and an efficient short-process manufacturing process is formed.

CN115608908BActive Publication Date: 2024-11-08JIANGYIN ZENKUNG FORGING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211568660.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-08
Publication Date
2024-11-08
Estimated Expiration
2042-12-08

AI Technical Summary

Technical Problem

During the forging of high-power giant wind power spindles, hydrogen-induced cracking tends to be severe, the manufacturing process is lengthy, and the energy and material consumption are serious, resulting in waste of materials and poor performance.

Method used

Multi-element collaborative ratio (C, Mn, Cr, Ni, Cu) combined with multiple upsetting-drawing-round forging processes is used to form a diffusely distributed ultrafine precipitation phase, which improves the irreversible hydrogen trap density and hydrogen diffusion coefficient inside the material. , through medium and low temperature rounding finishing process, remove internal stress and residual materials, and realize short-process manufacturing.

Benefits of technology

Effectively prevent hydrogen-induced cracking, shorten manufacturing processes, save energy and materials, and improve the service life and performance of wind power hollow spindles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115608908B_ABST
    Figure CN115608908B_ABST
Patent Text Reader

Abstract

This invention discloses a short-process manufacturing process for ultra-high power giant hollow wind turbine main shafts. The manufacturing process includes: S1, preparing metal raw materials according to the design formula, casting and forming steel ingots, and cooling the cast steel ingots to 750~850℃ after demolding, holding them at that temperature, and hot-sending them for pre-forging heating and holding; S2, heating the hot-sent steel ingots from S1 to 1220~1260℃ at a heating rate of 80~100℃ / h, holding them at that temperature for 7~8h, and then removing them from the furnace for forging; S3, chamfering the hot steel ingots from S2 and removing the risers and the bottom of the ingots; S4, using a turntable to perform rotary upsetting of the steel ingots after S3, with an upsetting forging ratio of 7:1~9:1, followed by downward punching with a long punch, and a final forging temperature of 1050~980℃. This invention solves a series of problems existing in wind turbine hollow main shafts, such as severe hydrogen-induced cracking tendency, lengthy manufacturing process, and high energy and material consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a short-process manufacturing process for an ultra-high-power giant wind power hollow main shaft, belonging to the technical field of wind power main shaft manufacturing. Background Art

[0002] As the global energy structure shifts toward low-carbonization and the energy consumption structure continues to be optimized, the trend of continued growth in demand for renewable energy is certain. With its outstanding advantages such as abundant resources, environmental protection, high degree of automation in operation and management, and continuously lowering cost per kilowatt-hour, wind energy has become one of the most widely developed and applied renewable energy sources and an important component of global renewable energy development and utilization. Its development is gradually shifting from supplementary energy to alternative energy, and its application is an important driving force for promoting energy structure optimization and low-carbonization of energy.

[0003] Wind turbine products and their components and related technologies are all highly complex, especially large wind turbines have high requirements for key components of wind turbines, such as wind turbine main shafts, gearboxes, etc. The wind turbine main shaft is the core component of the wind turbine, which plays an important role in absorbing the aerodynamic load of the impeller and transmitting power. It is known as the "heart" of the wind turbine, so wind turbine manufacturers have very strict quality requirements for it. At present, the manufacturing of wind turbine main shafts includes forging and casting. Casting can make castings quickly formed in one time, with high production efficiency and material utilization rate. It is suitable for the production of large or complex components, but its mechanical properties are lower than those of forgings of the same material. Forging can ensure the continuity of the metal fiber structure inside the forging, so that the forging has good mechanical properties and longer service life, and ultra-high power giant wind turbine main shaft manufacturing. In recent years, with the rapid development of wind power generation, wind turbines have developed rapidly in the direction of high power, and the size of the main shaft bearings supporting it has also developed in the direction of giantization, and the inner hole of the main shaft has become larger and larger. At present, the shaft of the wind turbine main shaft is formed by free forging, which is solid forging, and the inner hole is completed by subsequent machining. However, as the inner hole continues to increase, the waste of materials caused by solid forging becomes more and more serious, and the hollow forging of the wind turbine main shaft is imperative. However, in the forging process of large-power giant wind turbine main shafts, there is a general problem of serious tendency of hydrogen-induced cracking. Once cracking occurs, the entire main shaft will be scrapped. In addition, the forging process of large-power giant wind turbine main shafts is long. In addition to the necessary forging process, post-forging normalizing-tempering treatment is also required to achieve the purpose of grain refinement, uniform organization, dehydrogenation and elimination of internal stress, which makes the entire process lengthy and energy consumption serious. Finally, with the large-scale development of wind power equipment, the specifications of the main shaft are getting larger and larger, but with the continuous increase in the size of the inner hole of the main shaft, more and more residual materials are produced from the inner hole processing, and this part of the residual materials is of no significance to the wind turbine shaft itself, resulting in a large amount of waste.

[0004] In summary, those skilled in the art urgently need to study a short-process manufacturing process for ultra-high-power giant wind turbine hollow main shafts to solve the above-mentioned problems such as serious tendency of hydrogen-induced cracking, lengthy manufacturing process, and serious energy and material consumption. Summary of the invention

[0005] The present invention aims to provide a short-process manufacturing process for an ultra-high-power giant wind power hollow main shaft, which solves a series of problems such as serious tendency of hydrogen-induced cracking, lengthy manufacturing process, and serious energy and material consumption.

[0006] At the same time, the present invention provides an ultra-high power giant wind power hollow main shaft, which saves energy and materials and has a long service life.

[0007] At the same time, the present invention provides a large-scale wind power generator set using the ultra-high-power giant wind power hollow main shaft of the present invention, and the generator set can convert a large amount of wind energy into electrical energy.

[0008] At the same time, the present invention provides an application of an ultra-high power giant wind power hollow main shaft in a large wind power generator set.

[0009] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0010] A short-process manufacturing process for a hollow main shaft of an ultra-high-power giant wind power generator comprises the following steps:

[0011] S1, prepare metal raw materials according to the designed formula, cast and form steel ingots, and when the cast steel ingot is demoulded and cooled to 750~850℃, keep it warm and send it hot for heating and heat preservation before forging;

[0012] S2, heat the hot-delivered steel ingot in S1 to 1220~1260℃ at a heating rate of 80~100℃ / h, keep it at this temperature for 7~8h, and then take it out of the furnace to prepare for forging;

[0013] S3, chamfering the hot steel ingot taken out of S2 and cutting off the riser and the ingot bottom;

[0014] S4, the steel ingot treated in S3 is subjected to rotary upsetting with a turntable, the upsetting ratio is 7:1-9:1, and then a long punch is used to punch downward, and the final forging temperature is 980-1050°C;

[0015] S5, after the punching in S4 is completed, the forging on the long punch is pulled down by a hanging clamp, and the pulled down forging is returned to the furnace, heated to 1230~1270℃ at a heating rate of 90~110℃ / h, and kept warm for 7~8h;

[0016] S6, turn over the forgings heated and insulated in S5 and perform upsetting. The upsetting ratio is 6.5:1~8.5:1. Use a short punch to punch downwards. The final forging temperature is 1020~1080℃;

[0017] S7, returning the forged piece with holes obtained after forging in S6 to the furnace and reheating it to 1220-1260°C at a heating rate of 65-75°C / h, and keeping it at this temperature for 5-6h;

[0018] S8, placing the forged piece with holes heated in S7 inside the die, inserting a mandrel into the forged piece with holes and the center hole of the die, extruding, obtaining an integrally connected flange and shaft body, performing rotary upsetting on the flange, upsetting to 8-10% of the original height of the flange, and stretching the shaft body, the stretching process is: the anvil angle is 6-10°, the anvil width ratio is 0.8-1.2, the pressing amount is 10-13%, the turning method of 0°, -180° or -90° is adopted, and the feed amount is 0.8-0.9; the final forging temperature is 950-980°C;

[0019] S9, after the forging in S8, the forged part with holes is subjected to surface rounding and finishing, and the shaft is straightened;

[0020] S10, the perforated forgings after S9 finishing are returned to the furnace at 450~500℃, slowly heated to 660~670℃ at 80~120℃ / h, kept warm for 15~18h, cooled to 140~150℃ with the furnace, taken out of the furnace and air-cooled to room temperature to produce the finished steel ingot.

[0021] Furthermore, the length of the long punch is 2 / 3 of the height of the forging; the length of the short punch is 1 / 3 of the height of the forging.

[0022] Furthermore, in S2, the temperature of the hot-delivered steel ingot is 650-780°C.

[0023] Furthermore, in S9, the surface rounding finishing is performed at medium to low temperature, the rounding starting temperature is 950-980°C, and the rounding ending temperature is 600-630°C.

[0024] Furthermore, the grain size of the cast structure of the steel ingot is large, ranging from 50 to 150 microns; the grain size of the finished steel ingot is small, ranging from 10 to 20 microns, and ultrafine black precipitates are dispersed.

[0025] The invention discloses a super-power giant wind power hollow main shaft manufactured by a short-process manufacturing process, comprising the following components in percentage by mass: C: 0.40%-0.45%, Si: 0.20%-0.40%, Mn: 0.90%-1.20%, V: 0.06-0.10%, Mo: 0.16%-0.25%, Cr: 1.00%-1.44%, Ni: 0.35%-0.81%, Cu: 0.20%-0.25%, S≤0.02%, P≤0.02%, and the balance is Fe.

[0026] Furthermore, the mass ratio of Mn, Cr, Ni and Cu is Mn:Cr:Ni:Cu=(3.60~6.00):(4.00~7.20):(1.40~4.05):1.00.

[0027] Furthermore, the power of the ultra-high power giant wind power hollow main shaft is >8MW and its weight is >46 tons.

[0028] A large wind turbine generator set with an ultra-high power giant wind turbine hollow main shaft manufactured by a short-process manufacturing process for the ultra-high power giant wind turbine hollow main shaft.

[0029] The invention discloses an ultra-high power giant wind power hollow main shaft manufactured by a short process manufacturing process and its application in large wind turbine generator sets.

[0030] In summary, the present invention has the following beneficial effects:

[0031] 1. Anti-hydrogen embrittlement: Hydrogen-induced cracking is a common technical problem in large complex structural forgings, and is also a key point that restricts the forming of large complex forgings. In a short-process manufacturing process for a super-high-power giant wind turbine hollow main shaft of the present invention, a multi-element synergistic ratio of elements C, Mn, Cr, Ni and Cu is used, combined with multiple upsetting-drawing-rolling forging processes to achieve: (1) Refining grains and forming precipitated phases through element ratios. At the same time, through multiple upsetting-drawing-rolling forging processes, large strains and stresses are used to crush and blend the precipitated phases, so that the internal and external structures of the forgings tend to be uniform, forming a dispersed ultrafine precipitated phase. At the same time, large plastic deformation is used to refine the material grains to produce a large number of grain boundaries and phase interfaces, thereby increasing the irreversible hydrogen trap density inside the material, enhancing the ability to capture hydrogen, and reducing the concentration of active hydrogen atoms inside the material. (2) By combining multiple upsetting-drawing-rolling forging processes, a stress and strain distribution gradient is formed under high temperature conditions during the material forming process, thereby increasing the hydrogen diffusion coefficient in the material and allowing more hydrogen to diffuse out during the forging process. (3) The present invention adopts a medium-low temperature (800-600°C) rolling finishing process at the end of forging. During the hollow forging process, the inner hole and the outer surface can both undergo surface plastic deformation, forming a directional (from inside to outside) stress and strain gradient distribution, which increases the hydrogen diffusion coefficient in the material and promotes the active internal hydrogen caused by the decrease in hydrogen solubility due to the temperature reduction to accelerate the diffusion and escape outward along the gradient direction. (4) When the formed giant wind power hollow main shaft is used in a hydrogen (hydrogen ion) atmosphere, the surface Cr and Cu will form a dense passivation film, thereby preventing the entry of external hydrogen, effectively inhibiting the hydrogen-induced cracking phenomenon of large complex structure forgings.

[0032] 2. Short process: In the short process manufacturing process of the ultra-high power giant wind turbine hollow main shaft of the present invention, the medium and low temperature rolling finishing process is used to achieve the dehydrogenation grain refinement and internal stress release of the hollow forged main shaft. Compared with the traditional wind turbine main shaft preparation process, it can save the long time (usually 3-5 days) normalizing process after forging, while ensuring the performance of the forged main shaft, reducing the manufacturing process and realizing short process manufacturing.

[0033] 3. Energy saving and material saving: In the short-process manufacturing process of a super-high-power giant wind turbine hollow main shaft of the present invention, (1) hot-feeding steel ingots are used for forging, which can effectively utilize the waste heat from casting; (2) medium-low temperature spherical finishing is used to save the post-forging normalizing process, effectively saving the energy consumption of the normalizing process; (3) The preparation method of the present invention produces a wind turbine hollow main shaft, and the hollow forging method is used to reduce the machining allowance of various parts of the wind turbine main shaft, reduce the excess material from the inner hole machining, avoid a large amount of waste of raw materials, and achieve the effect of saving materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1is a microscopic image of the as-cast structure of the steel ingot in the present invention;

[0035] Figure 2 It is a microstructure diagram of the ultra-high power giant wind power hollow main shaft in the present invention;

[0036] Figure 3 is a microstructure diagram of a dense passivation film in the present invention;

[0037] Figure 4 This is an XPS test diagram of the Cr component in the dense passivation film of the present invention;

[0038] Figure 5 This is an XPS test graph of the Cu component contained in the dense passivation film of the present invention;

[0039] Figure 6 This is a site construction drawing of the ultra-high power giant wind power hollow main shaft in the present invention;

[0040] Figure 7 It is a structural schematic diagram of an existing mold used in the present invention. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solution and advantages of the present invention more clear, the device proposed by the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. According to the following description, the advantages and features of the present invention will be more clear.

[0042] Example 1

[0043] A super-high power giant wind power hollow main shaft, characterized in that it comprises the following components in percentage by mass: C: 0.40%, Si: 0.20%, Mn: 1.20%, V: 0.10%, Mo: 0.16%, Cr: 1.44%, Ni: 0.81%, Cu: 0.20%, S: 0.02%, P: 0.02%, and the balance is Fe.

[0044] The mass ratio of Mn, Cr, Ni and Cu is Mn:Cr:Ni:Cu=6.00:7.20:4.05:1.00.

[0045] The power of the ultra-high power giant wind turbine hollow main shaft is >8MW and its weight is >46 tons.

[0046] A short-process manufacturing process for a super-high-power giant wind power hollow main shaft comprises the following steps:

[0047] S1, prepare the metal raw materials according to the above design formula, cast and form steel ingots, and when the cast steel ingots are demoulded and cooled to 800°C, place them in an 800°C heat preservation transfer barrel and heat them before forging;

[0048] S2, heat the hot-delivered steel ingot (temperature 780°C) in S1 to 1250°C at a heating rate of 90°C / h, keep it at this temperature for 7h, and prepare for forging after taking it out of the furnace;

[0049] S3, chamfering the hot steel ingot taken out of S2 and cutting off the riser and the ingot bottom;

[0050] S4, the steel ingot treated in S3 is subjected to rotary upsetting with a turntable, the upsetting ratio is 8:1, and then a long punch (the length is 2 / 3 of the forging height) is used to punch downward, and the final forging temperature is 1000℃;

[0051] S5, after the punching in S4 is completed, the forging on the long punch is pulled down by a hanging clamp, and the pulled down forging is returned to the furnace, heated to 1250℃ at a heating rate of 100℃ / h, and kept warm for 7h;

[0052] S6, turn over the forgings heated and insulated in S5 and perform upsetting. The upsetting ratio is 7:1. Use a short punch (the length is 1 / 3 of the forging height) to punch downwards. The final forging temperature is 1050℃.

[0053] S7, returning the forged piece with holes obtained after forging in S6 to the furnace and reheating it to 1250°C at a heating rate of 70°C / h, and keeping the temperature for 5h;

[0054] S8, place the forging with holes heated in S7 on Figure 7 Inside the mold shown, the mold includes a matching bottom barrel 1 and a fetal membrane 3, a core rod 4 is inserted into the hole forging and the center hole 5 of the mold, and extrusion is performed to obtain an integrally connected flange 6 and shaft body 2, and the flange 6 is rotary upset to 9% of the original height of the flange 6, and the shaft body 2 is stretched, and the stretching process is: the anvil angle is 8°, the anvil width ratio is 1.0, the pressing amount is 11%, the -180° flipping method is adopted, and the feed amount is 0.8; the final forging temperature is 965°C;

[0055] S9, the forging with holes after forging in S8 is subjected to surface rounding finishing, the surface rounding finishing is carried out at medium and low temperature, the starting temperature of rounding is 965°C, the ending temperature of rounding is 615°C, and the shaft is straightened;

[0056] S10, the perforated forgings after S9 finishing are returned to the furnace at 480℃, slowly heated to 665℃ at 100℃ / h, kept at this temperature for 16h, cooled to 145℃ with the furnace, taken out of the furnace and air-cooled to room temperature to produce the finished steel ingot.

[0057] A large wind turbine generator set using an ultra-high power giant wind turbine hollow main shaft according to the embodiment.

[0058] The present embodiment provides an application of a super-high power giant wind power hollow main shaft in a large wind power generator set.

[0059] like Figure 1 As shown in FIG. 1 , it is a microscopic picture of the cast structure of the steel ingot in this embodiment. It can be seen from the picture that the grain size of the steel ingot (i.e. the structure before forging) is large, ranging from 50 to 150 microns, and large pieces of black precipitate phases are gathered at the grain boundaries.

[0060] like Figure 2 As shown in FIG. 1 , it is a microscopic picture of the finished product in this embodiment. It can be seen from the picture that the grain size of the finished product (structure after forging) is small, 10 to 20 microns, and ultrafine black precipitates are dispersed.

[0061] In the forging process of this embodiment, the medium-low temperature rounding finishing process is used to eliminate the post-forging normalizing process, thereby realizing short-process manufacturing; in addition, the hollow wind turbine main shaft is obtained by hollow forging, which has the effects of energy saving and material saving.

[0062] When the wind power hollow main shaft forging of this embodiment is used in a hydrogen (hydrogen ion) atmosphere, the surface Cr and Cu will form the following Figure 3 The dense passivation film shown, Figure 3 In the figure, the dark area is the dense passivation film.

[0063] like Figure 4~Figure 5 As shown, they are the XPS test graphs of the dense passivation film containing Cr components and the XPS test graphs of the dense passivation film containing Cu components in this embodiment.

[0064] like Figure 6 As shown, this is the on-site construction drawing of the ultra-high power giant wind turbine hollow main shaft obtained in this embodiment. It can be seen that this embodiment obtains an ultra-high power, giant wind turbine hollow main shaft, with an ultra-high power of 8MW and a giant tonnage of 46.5 tons.

[0065] The hydrogen diffusion coefficient of the ultra-high power giant wind power hollow main shaft obtained in this embodiment is calculated. The hydrogen diffusion coefficient of the cast state (before forging, i.e., steel ingot) is: D0=8.17×10-9m2 / s (the calculation method is shown in the reference: A new method for calculating the hydrogen diffusion coefficient). The hydrogen diffusion coefficient of the forging (during forging pressure): D0=17.24×10-9 m2 / s (the calculation method is shown in the reference: Experimental study of hydrogen diffusion in stress field). It can be seen that the hydrogen diffusion coefficient of the forging of the present application becomes larger during the forging pressure process, which facilitates the escape of free active hydrogen.

[0066] In order to characterize the material's resistance to hydrogen embrittlement, a hydrogen-induced test was conducted on the ultra-high power giant wind power hollow main shaft obtained in this embodiment. A forging tensile specimen (with a notch) was taken, and the notch was placed in a Walpole corrosion inhibitor (hydrochloric acid, sodium acetate, deionized water) for a constant load notch tensile test to measure the notch tensile delayed fracture strength ratio (DFSR) before and after hydrogen charging. The higher the DFSR value, the stronger the material's resistance to hydrogen embrittlement.

[0067] Embodiment 2:

[0068] A super-high power giant wind power hollow main shaft, characterized in that it comprises the following components in percentage by mass: C: 0.45%, Si: 0.40%, Mn: 0.90%, V: 0.06%, Mo: 0.25%, Cr: 1.00%, Ni: 0.35%, Cu: 0.25%, S: 0.01%, P: 0.01%, and the balance is Fe.

[0069] The mass ratio of Mn, Cr, Ni and Cu is Mn:Cr:Ni:Cu=3.60:4.00:1.40:1.00.

[0070] The power of the ultra-high power giant wind turbine hollow main shaft is >8MW and its weight is >46 tons.

[0071] A short-process manufacturing process for a super-high-power giant wind power hollow main shaft comprises the following steps:

[0072] S1, prepare the metal raw materials according to the above design formula, cast and form steel ingots, and when the cast steel ingots are demolded and cooled to 750°C, place them in a 750°C heat preservation transfer barrel and heat them before forging;

[0073] S2, heat the hot-delivered steel ingot in S1 (temperature is 650℃, heat loss occurs during the delivery process) to 1220℃ at a heating rate of 80℃ / h, keep it at this temperature for 8h, and then take it out of the furnace for forging;

[0074] S3, chamfering the hot steel ingot taken out of S2 and cutting off the riser and the ingot bottom;

[0075] S4, the steel ingot treated in S3 is subjected to rotary upsetting with a turntable, the upsetting ratio is 7:1, and then a long punch (the length is 2 / 3 of the forging height) is used to punch downward, and the final forging temperature is 1050℃;

[0076] S5, after the punching in S4 is completed, the forging on the long punch is pulled down by a hanging clamp, and the pulled down forging is returned to the furnace, heated to 1230℃ at a heating rate of 90℃ / h, and kept warm for 8h;

[0077] S6, turn over the forgings heated and insulated in S5 and perform upsetting. The upsetting ratio is 6.5:1. Use a short punch (the length is 1 / 3 of the forging height) to punch downwards. The final forging temperature is 1080℃.

[0078] S7, returning the forged piece with holes obtained after forging in S6 to the furnace and reheating it to 1220°C at a heating rate of 65°C / h, and keeping the temperature for 6h;

[0079] S8, place the forging with holes heated in S7 on Figure 7 Inside the mold shown, the mold includes a matching bottom barrel 1 and a fetal membrane 3, a core rod 4 is inserted into the hole forging and the center hole 5 of the mold, and extrusion is performed to obtain an integrally connected flange 6 and shaft body 2, and the flange 6 is rotary upset to 8% of the original height of the flange 6, and the shaft body 2 is stretched. The stretching process is: the anvil angle is 6°, the anvil width ratio is 0.8, the pressing amount is 10%, the -90° flip method is adopted, and the feed amount is 0.9; the final forging temperature is 980°C;

[0080] S9, the forging with holes after forging in S8 is subjected to surface rounding finishing, the surface rounding finishing is performed at a medium-low temperature, the starting temperature of the rounding is 980°C, the ending temperature of the rounding is 630°C, and the shaft is straightened;

[0081] S10, the perforated forgings after S9 finishing are returned to the furnace at 450℃, slowly heated to 660℃ at 80℃ / h, kept at this temperature for 15h, cooled to 140℃ with the furnace, taken out of the furnace and air-cooled to room temperature to produce the finished steel ingot.

[0082] A large wind turbine generator set using an ultra-high power giant wind turbine hollow main shaft according to the embodiment.

[0083] The present embodiment provides an application of a super-high power giant wind power hollow main shaft in a large wind power generator set.

[0084] Embodiment 3:

[0085] A super-high power giant wind power hollow main shaft, characterized in that it comprises the following components in percentage by mass: C: 0.42%, Si: 0.30%, Mn: 1.00%, V: 0.08%, Mo: 0.20%, Cr: 1.10%, Ni: 0.60%, Cu: 0.22%, S: 0.005%, P: 0.01%, and the balance is Fe.

[0086] The mass ratio of Mn, Cr, Ni and Cu is Mn:Cr:Ni:Cu=4.55:5.00:2.73:1.00.

[0087] The power of the ultra-high power giant wind turbine hollow main shaft is >8MW and its weight is >46 tons.

[0088] A short-process manufacturing process for a super-high-power giant wind power hollow main shaft comprises the following steps:

[0089] S1, prepare the metal raw materials according to the above design formula, cast and form steel ingots, and when the cast steel ingots are demoulded and cooled to 850°C, place them in an 850°C heat preservation transfer barrel and heat them before forging;

[0090] S2, heat the hot-delivered steel ingot in S1 (temperature is 750℃, heat loss occurs during the delivery process) to 1260℃ at a heating rate of 100℃ / h, keep it at this temperature for 7.5h, and then take it out of the furnace for forging;

[0091] S3, chamfering the hot steel ingot taken out of S2 and cutting off the riser and the ingot bottom;

[0092] S4, the steel ingot treated in S3 is subjected to rotary upsetting with a turntable, the upsetting ratio is 9:1, and then a long punch (the length is 2 / 3 of the forging height) is used to punch downward, and the final forging temperature is 980℃;

[0093] S5, after the punching in S4 is completed, the forging (blank) on the long punch is pulled down by a hanging clamp, and the pulled down forging is returned to the furnace, heated to 1270℃ at a heating rate of 110℃ / h, and kept warm for 7.5h;

[0094] S6, turn over the forging heated and insulated in S5 and perform upsetting. The upsetting ratio is 8.5:1 (the upsetting ratio is the height ratio of the forging obtained in the previous process). Use a short punch (the length is 1 / 3 of the forging height) to punch downwards. The final forging temperature is 1020℃.

[0095] S7, returning the forged piece with holes obtained after forging in S6 to the furnace and reheating it to 1260°C at a heating rate of 75°C / h, and keeping the temperature for 5.5h;

[0096] S8, place the forging with holes heated in S7 on Figure 7 Inside the mold shown, the mold includes a matching bottom barrel 1 and a fetal membrane 3, a core rod 4 is inserted into the hole forging and the center hole 5 of the mold, and extrusion is performed to obtain an integrally connected flange 6 and shaft body 2, and the flange 6 is rotary upset to 10% of the original height of the flange 6, and the shaft body 2 is stretched, and the stretching process is: the anvil angle is 10°, the anvil width ratio is 1.2, the pressing amount is 13%, the 0° method is adopted, and the feed amount is 0.9; the final forging temperature is 950°C;

[0097] S9, the forging with holes after forging in S8 is subjected to surface rounding finishing, the surface rounding finishing is performed at a medium-low temperature, the starting temperature of the rounding is 950°C, the ending temperature of the rounding is 600°C, and the shaft is straightened;

[0098] S10, the perforated forgings after S9 finishing are returned to the furnace at 500℃, slowly heated to 670℃ at 120℃ / h, kept at this temperature for 18h, cooled to 150℃ with the furnace, taken out of the furnace and air-cooled to room temperature to produce the finished steel ingot.

[0099] A large wind turbine generator set using an ultra-high power giant wind turbine hollow main shaft according to the embodiment.

[0100] The present embodiment provides an application of a super-high power giant wind power hollow main shaft in a large wind power generator set.

[0101] Performance testing of finished steel ingots:

[0102] The performance parameters of the finished products obtained in Example 1 to Example 3 are shown in Table 1.

[0103]

[0104] Table 1

[0105] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0106] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A short-process manufacturing process for ultra-high power giant wind power hollow main shaft, characterized in that: The following steps are involved: S1, prepare metal raw materials according to the designed formula, cast and form steel ingots, and when the cast steel ingot is demoulded and cooled to 750~850℃, keep it warm and send it hot for heating and heat preservation before forging; S2, heat the hot-delivered steel ingot in S1 to 1220~1260℃ at a heating rate of 80~100℃ / h, keep it at this temperature for 7~8h, and then take it out of the furnace to prepare for forging; S3, chamfering the hot steel ingot taken out of S2 and cutting off the riser and the ingot bottom; S4, the steel ingot treated in S3 is subjected to rotary upsetting with a turntable, the upsetting ratio is 7:1-9:1, and then a long punch is used to punch downward, and the final forging temperature is 980-1050°C; S5, after the punching in S4 is completed, the forging on the long punch is pulled down by a hanging clamp, and the pulled down forging is returned to the furnace, heated to 1230~1270℃ at a heating rate of 90~110℃ / h, and kept warm for 7~8h; S6, turn over the forgings heated and insulated in S5 and perform upsetting. The upsetting ratio is 6.5:1~8.5:

1. Use a short punch to punch downwards. The final forging temperature is 1020~1080℃; S7, returning the forged piece with holes obtained after forging in S6 to the furnace and reheating it to 1220-1260°C at a heating rate of 65-75°C / h, and keeping it at this temperature for 5-6h; S8, placing the forged piece with holes heated in S7 inside the die, inserting a mandrel into the forged piece with holes and the center hole of the die, extruding, obtaining an integrally connected flange and shaft body, performing rotary upsetting on the flange, upsetting to 8-10% of the original height of the flange, and stretching the shaft body, the stretching process is: the anvil angle is 6-10°, the anvil width ratio is 0.8-1.2, the pressing amount is 10-13%, the turning method of 0°, -180° or -90° is adopted, and the feed amount is 0.8-0.9; the final forging temperature is 950-980°C; S9, the forging with holes after forging in S8 is subjected to surface rounding finishing and the shaft body is straightened. In S9, the surface rounding finishing is performed at a medium-low temperature, the rounding starting temperature is 950-980°C, and the rounding ending temperature is 600-630°C; S10, returning the forged piece with holes after finishing in S9 to the furnace at 450-500°C, slowly heating it to 660-670°C at 80-120°C / h, keeping it at that temperature for 15-18h, cooling it to 140-150°C with the furnace, and then taking it out of the furnace and air cooling it to room temperature to produce the finished steel ingot; The ultra-high power giant wind power hollow main shaft manufactured by the short process manufacturing process includes the following components by mass percentage: C: 0.40%~0.45%, Si: 0.20%~0.40%, Mn: 0.90%~1.20%, V: 0.06~0.10%, Mo: 0.16%~0.25%, Cr: 1.00%~1.44%, Ni: 0.35%~0.81%, Cu: 0.20%~0.25%, S≤0.02%, P≤0.02%, and the balance is Fe; The mass ratio of Mn, Cr, Ni and Cu is Mn:Cr:Ni:Cu=(3.60-6.00):(4.00-7.20):(1.40-4.05):1.00; The power of the ultra-high power giant wind turbine hollow main shaft is >8MW and its weight is >46 tons.

2. The short-process manufacturing process of a hollow main shaft of a super-high-power giant wind power generator according to claim 1 is characterized in that: The length of the long punch is 2 / 3 of the height of the forging; the length of the short punch is 1 / 3 of the height of the forging.

3. The short-process manufacturing process of a hollow main shaft of a super-high-power giant wind power generator according to claim 1 is characterized in that: In S2, the temperature of the hot-delivered steel ingot is 650~780℃.

4. The short-process manufacturing process of a hollow main shaft of a super-high-power giant wind power generator according to claim 1 is characterized in that: The grain size of the cast structure of the steel ingot is large, ranging from 50 to 150 microns; the grain size of the finished steel ingot is small, ranging from 10 to 20 microns, with ultrafine black precipitates dispersed.

5. A large wind turbine generator set with an ultra-high power giant wind turbine hollow main shaft manufactured using the short-process manufacturing process for an ultra-high power giant wind turbine hollow main shaft as described in any one of claims 1 to 4.

6. Application of the ultra-high power giant wind power hollow main shaft manufactured by the short-process manufacturing process of the ultra-high power giant wind power hollow main shaft as claimed in any one of claims 1 to 4 in large wind turbine generator sets.