High temperature resistant polyurethane sheet foam material and preparation method and use thereof

By adjusting the component ratio of polyurethane sheets and adding amino acid compounds, the high-temperature dimensional stability and bearing performance of polyurethane sheets are improved, and the problem of existing polyurethane foam materials easily deformed at high temperatures is solved. It is suitable for automotive coat rack boards industrial applications.

CN115703874BActive Publication Date: 2024-12-06ZHANGJIAGANG CHANGTAI AUTO TRIM MATERIAL CO LTD
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
CN202110918241.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-11
Publication Date
2024-12-06
Estimated Expiration
2041-08-11

AI Technical Summary

Technical Problem

Existing polyurethane foam materials are prone to deform at high temperatures and have poor load-bearing performance, which cannot meet the needs of automotive coat rack plates for lightweight, high load-bearing and high temperature resistance.

Method used

Polyurethane sheet foaming material with a weight ratio of 100:100 to 150 is used. Component A includes polyether polyols, crosslinking agents, catalysts and foam stabilizers. Component B is an isocyanate, through The selection of amino acid compounds and low atomization catalysts can improve the high-temperature dimensional stability and bearing performance of the material.

Benefits of technology

The dimensional stability is maintained at a temperature of 100°C less than 0.5%, and the tensile strength and compression strength reach 187~232Kpa and 209~265Kpa, which meets the load-bearing performance requirements of automobile coat rack plates and has good high temperature resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003206419740000031
    Figure BDA0003206419740000031
  • Figure BDA0003206419740000041
    Figure BDA0003206419740000041
  • Figure BDA0003206419740000051
    Figure BDA0003206419740000051
Patent Text Reader

Abstract

The invention relates to a high-temperature resistant polyurethane sheet foam material and a preparation method and application thereof, and mainly solves the problem that polyurethane foam is easy to deform and not resistant to high temperature at high temperature in the prior art. The invention adopts a high-temperature resistant polyurethane sheet foam material, which is composed of component A and component B, and the weight ratio of component A to component B is 100:100-150, wherein component A comprises, by weight, 1-30 parts of polyether polyol I, 55-90 parts of polyether polyol II, 3-10 parts of crosslinking agent, 0.5-1 part of catalyst, 0.5-2 parts of foam stabilizer, and 1.5-2.5 parts of water; component B is isocyanate; polyether polyol I has an average molecular weight of 3000-8000 and a functionality of 2-4; polyether polyol II has an average molecular weight of 200-900 and a functionality of 3-8; and the technical solution that the crosslinking agent is an amino acid compound solves the above problems well, and can be used in industrial applications of automobile coat rack plates.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polyurethane, and particularly relates to a high-temperature resistant polyurethane sheet foam material and a preparation method and application thereof. Background Art

[0002] Polyurethane foam materials are increasingly used in the automotive industry and have become one of the most widely used plastics in automobiles. Currently, polyurethane foam materials for automobiles are developing in the direction of lightweight, safety, environmental protection and comfort. Among them, automobile coat rack boards are used to cover and isolate the trunk compartment, and need to have high load-bearing and good high temperature resistance; currently in the field of automotive interior materials, automobile coat rack boards are mostly made of PP blow molding, corrugated honeycomb paper spray molding and other materials and production processes for composite production; however, the automobile coat rack boards made by the above process have many shortcomings, such as large total mass, limited load-bearing capacity, easy deformation at high temperature, poor sound absorption and noise reduction effect, etc. As the market and consumers have higher and higher requirements for automotive product materials, the existing composite materials and processes can no longer meet the needs of the OEMs for the above-mentioned automobile coat rack boards in terms of lightweight, high load-bearing and high temperature resistance. Therefore, the automobile coat rack boards made of PU composite boards have gradually entered the public's field of vision due to their excellent characteristics such as light weight, high temperature resistance, high air permeability and good sound absorption.

[0003] In the prior art, automobile interior parts made of polyurethane foam materials are subjected to pressure and sunlight all year round, especially the high temperature in summer, and automobile coat rack panels are prone to bending and deformation to a certain extent; and in the process of preparing automobile coat rack panels from PU composite panels, in order to meet the demand for lightweight vehicles and to reflect cost advantages, the density of PU polyurethane foam is usually controlled at 50-70kg / m 3 However, this will result in a soft composite board skeleton and insufficient load-bearing capacity. When softened at a temperature of 220-230°C, it is prone to obvious curling and deformation, making subsequent composite production impossible. It can be seen that there is still a lot of room for improvement in the thermal stability of polyurethane foam boards. It is of great practical significance to develop a polyurethane foam that is resistant to high temperatures, has good dimensional stability at high temperatures, and is not easy to deform.

[0004] Chinese patent CN112574382A discloses a high temperature resistant and aging resistant polyurethane material and a preparation method thereof, which is prepared by reacting component A and component B, wherein the weight proportion of component A to component B is 100:40-80 parts, wherein component A comprises, by weight, 1-30 parts of polyether polyol I, 50-90 parts of polyether polyol II, 0-20 parts of polymer polyol, 1-5 parts of crosslinking agent, 0.5-1 part of catalyst, 0.5-2 parts of foam stabilizer, 1.5-2.5 parts of water, and 0.1-2 parts of antioxidant; component B comprises, by weight, 10-30 parts of isocyanate and 70-90 parts of modified isocyanate; an aging resistant and high temperature resistant polyurethane automotive material is provided, but the polyurethane foam obtained is a soft foam with poor bearing properties such as tensile strength and compressive strength, and cannot be used in places where hard panels are required, such as automobile coat rack panels, and the problem of whether dimensional deformation is prone to occur at high temperatures is not mentioned. Summary of the invention

[0005] One of the technical problems to be solved by the present invention is that the polyurethane foam in the prior art is easily deformed and not resistant to high temperatures. A high-temperature resistant polyurethane sheet foam material is provided, which has the advantages of good dimensional stability and high-temperature resistance at high temperatures.

[0006] The second technical problem to be solved by the present invention is to provide a method for preparing a high temperature resistant polyurethane sheet foam material corresponding to the first technical problem to be solved.

[0007] The third technical problem to be solved by the present invention is to provide an application of a high temperature resistant polyurethane sheet foam material corresponding to the first technical problem to be solved.

[0008] To solve one of the above technical problems, the technical solution provided by the present invention is as follows: a high temperature resistant polyurethane sheet foam material, composed of component A and component B, the weight ratio of component A to component B is 100:100-150, wherein component A comprises, by weight: 1-30 parts of polyether polyol I, 55-90 parts of polyether polyol II, 3-10 parts of cross-linking agent, 0.5-1 part of catalyst, 0.5-2 parts of foam stabilizer, and 1.5-2.5 parts of water; component B is isocyanate; wherein the average molecular weight of the polyether polyol I is 3000-8000, and the functionality is 2-4; the average molecular weight of the polyether polyol II is 200-900, and the functionality is 3-8; the cross-linking agent is an amino acid compound; the catalyst is selected from at least one of a low atomization catalyst, a delayed catalyst or a non-volatile catalyst; the foam stabilizer is at least one of a polysiloxane-oxidized olefin block copolymer.

[0009] In the above technical solution, preferably, the amino acid compound is selected from at least one of serine, phenylalanine, aspartic acid, arginine, glutamic acid or asparagine.

[0010] In the above technical solution, preferably, the polyether polyol I is selected from at least one of CHE-828, CHE-330N, CHE-5602, N-240 or N-430; the polyether polyol II is selected from at least one of N-403, ZS-4110, N-303, CHE-305 or CHE-306.

[0011] In the above technical solution, preferably, the catalyst is selected from at least one of TEDA, ZF-10, ZR-70, ZF-20, Dabco T, Toyocat-NP, Toyocat-RX5, Dabco DMEA or Toyocat-TRC.

[0012] In the above technical solution, preferably, the foam stabilizer is selected from at least one of L-5340, L-618, B-8715LF2, B-8734LF2, DC198, L-5440, L-580, AK-8805 or AK-8815.

[0013] In the above technical solution, preferably, the isocyanate is selected from at least one of PM-200, M20S, 44V20 or PAPI-135C.

[0014] To solve the second technical problem above, the present invention provides a technical solution as follows: a method for preparing a high temperature resistant polyurethane sheet foam material, comprising the following steps:

[0015] (1) Prepare the raw materials according to the weight proportions of the following components:

[0016] The weight ratio of component A to component B is 100:100-150, wherein component A comprises, by weight: 1-30 parts of polyether polyol I, 55-90 parts of polyether polyol II, 3-10 parts of crosslinking agent, 0.5-1 part of catalyst, 0.5-2 parts of foam stabilizer, and 1.5-2.5 parts of water; component B is isocyanate; the average molecular weight of the polyether polyol I is 3000-8000, and the functionality is 2-4; the average molecular weight of the polyether polyol II is 200-900, and the functionality is 3-8; the crosslinking agent is an amino acid compound; the catalyst is selected from at least one of a low-atomization catalyst, a delayed catalyst, or a non-volatile catalyst; the foam stabilizer is at least one of a polysiloxane-oxidized olefin block copolymer;

[0017] (2) Preparation of component A:

[0018] According to the components and weight proportions in step (1), polyether polyol I, polyether polyol II, a crosslinking agent, a catalyst, a foam stabilizer and water are sequentially added into container A, and stirred evenly at a temperature of 20 to 25° C. to obtain a mixed material I;

[0019] (3) Preparation of component B:

[0020] Add isocyanate into container B according to the components and weight proportions in step (1), and stir evenly at 20-25°C;

[0021] (4) Component A and component B are mixed and stirred at a weight ratio of 100:100-150, and then injected into a pre-prepared tooling mold. After free rising, a high temperature resistant polyurethane sheet foam material is obtained.

[0022] In the above technical solution, preferably, the amino acid compound is selected from at least one of serine, phenylalanine, aspartic acid, arginine, glutamic acid or asparagine.

[0023] In the above technical solution, preferably, the polyether polyol I is selected from at least one of CHE-828, CHE-330N, CHE-5602, N-240 or N-430; the polyether polyol II is selected from at least one of N-403, ZS-4110, N-303, CHE-305 or CHE-306; the catalyst is selected from TEDA, ZF-10, ZR-70, ZF-20, Dabco T, Toyocat-NP, Toyocat-RX5, Dabco At least one of DMEA or Toyocat-TRC; the foam stabilizer is selected from at least one of L-5340, L-618, B-8715LF2, B-8734LF2, DC198, L-5440, L-580, AK-8805 or AK-8815; the isocyanate is selected from at least one of PM-200, M20S, 44V20 or PAPI-135C.

[0024] In order to solve the third of the above technical problems, the technical solution provided by the present invention is as follows: the prepared high temperature resistant polyurethane sheet foam material is used in the industrial application of automobile coat rack panels.

[0025] In the high temperature resistant polyurethane sheet foam material of the present invention, different polyether polyols, crosslinking agents, foam stabilizers and catalysts are selected and compounded, and in particular, an amphoteric amino acid compound containing both amino groups and carboxyl groups is introduced into the reaction components, so that the dimensional stability of the prepared polyurethane sheet foam material at high temperature is improved; in the performance test, the tensile strength is 187-232 Kpa, and the compressive strength is 209-265 Kpa, which meet the internal control index requirements of the automobile coat rack plate for the polyurethane sheet foam material (bearing performance requirements: tensile strength ≥150 Kpa, compressive strength ≥200 Kpa), and the thermal dimensional stability at a temperature of 100 DEG C is 0.1-0.5%, which has the advantage of high temperature resistance while maintaining the bearing performance, and achieves good technical effects.

[0026] The present invention will be further described below by way of examples, but are not limited thereto. DETAILED DESCRIPTION

[0027] Table 1 List of raw materials

[0028]

[0029]

[0030] [Example 1]

[0031] A method for preparing a high temperature resistant polyurethane sheet foam material comprises the following steps:

[0032] (1) Prepare the following raw materials by weight:

[0033] Component A: 100 parts, including 10 parts CHE-828, 80 parts N-403, 6 parts glutamic acid, 0.5 parts TEDA, 1.5 parts L-618 and 2 parts water;

[0034] Component B: 150 parts, specifically 150 parts PM-200

[0035] (2) Preparation of component A:

[0036] According to the weight proportions in step (1), CHE-828, N-403, glutamic acid, TEDA, L-618 and water are added to container A in sequence, and stirred evenly at 20° C. to obtain a mixed material I;

[0037] (3) Preparation of component B:

[0038] Add PM-200 to container B according to the weight proportions in step (1) and stir evenly at 20°C;

[0039] (4) After the component A and the component B are quickly mixed and stirred evenly, they are quickly injected into the tooling mold prepared in advance. After free rising is completed, a high temperature resistant polyurethane sheet foam material is obtained, and physical properties are tested. The performance index data are shown in Table 3;

[0040] (5) The high temperature resistant polyurethane sheet foam material is used to prepare automobile coat rack panels.

[0041] [Examples 2 to 10]

[0042] Examples 2 to 10 are carried out according to the steps in Example 1, except that the reaction raw materials and raw material ratios in the foaming formula are different, as shown in Table 2; the performance index data of the obtained high temperature resistant polyurethane sheet foam material are shown in Table 3.

[0043] Table 2 Weight parts of each component in the formula of high temperature resistant polyurethane sheet foam material of Examples 1 to 10

[0044]

[0045]

[0046] [Comparative Example 1]

[0047] A method for preparing a polyurethane sheet foam material comprises the following steps:

[0048] (1) Prepare the following raw materials by weight:

[0049] Component A: 100 parts, specifically 15 parts CHE-330N, 75 parts ZS-4110, 0.8 parts triethanolamine, 0.3 parts ZF-10, 6.9 parts AK-8805 and 2 parts water;

[0050] Component B: 150 parts, specifically 150 parts M20S

[0051] (2) Preparation of component A:

[0052] According to the weight proportions in step (1), CHE-330N, ZS-4110, triethanolamine, ZF-10, AK-8805 and water are sequentially added into container A, and stirred evenly at 20° C. to obtain a mixed material I;

[0053] (3) Preparation of component B:

[0054] Add M20S to container B according to the weight proportions in step (1) and stir evenly at 20°C;

[0055] (4) After the component A and the component B are quickly mixed and stirred evenly, they are quickly injected into the tooling mold prepared in advance. After free rising is completed, the polyurethane sheet foam material is obtained and the physical properties are tested. The performance index data are shown in Table 3;

[0056] (5) The polyurethane sheet foam material is used to prepare automobile coat rack panels.

[0057] Table 3 Performance test data of polyurethane sheet foam materials of Examples 1 to 10 and Comparative Example 1

[0058]

[0059] It can be seen from the data results in Table 3 that: compared with Comparative Example 1, the test data of the physical properties of tensile strength, elongation at break and compressive strength of Examples 1 to 10 are similar, and the bearing performance is equivalent; after being placed under high temperature conditions of 100°C for 1 hour, the dimensional change rate of Comparative Example 1 is 0.7%, and the dimensional stability is poor, while the dimensional change rate of the polyurethane sheet foam material in Examples 1 to 10 is 0.1-0.5%, and the dimensional change rate is small, and it has the advantages of good high temperature dimensional stability and high temperature resistance.

[0060] Therefore, the high temperature resistant polyurethane sheet foam material provided by the present invention has good high temperature resistance and high temperature dimensional stability while ensuring the load-bearing performance, achieves good technical effects, and can be used in industrial applications of automobile coat rack plates.

Claims

1. A high temperature resistant polyurethane sheet foam material, consisting of component A and component B, wherein the weight ratio of component A to component B is 100:100-150. in, Component A comprises, by weight: 1 to 30 parts of polyether polyol I, 61.4 to 78 parts of polyether polyol II, 3 to 10 parts of a crosslinking agent, 0.5 to 1 part of a catalyst, 0.5 to 2 parts of a foam stabilizer, and 1.5 to 2.5 parts of water; component B is an isocyanate; wherein the average molecular weight of the polyether polyol I is 3000 to 8000, and the functionality is 2 to 4; the average molecular weight of the polyether polyol II is 200 to 900, and the functionality is 3 to 8; the crosslinking agent is an amino acid compound; the catalyst is selected from at least one of a low atomization catalyst, a delayed catalyst, or a non-volatile catalyst; the foam The foam stabilizer is at least one of polysiloxane-olefin oxide block copolymers; the amino acid compound is at least one of serine, phenylalanine, aspartic acid, arginine, glutamic acid or asparagine; the polyether polyol I is at least one of CHE-828, CHE-330N, CHE-5602, N-240 or N-430; the polyether polyol II is at least one of N-403, ZS-4110, N-303, CHE-305 or CHE-306; the catalyst is TEDA, ZF-10, ZR-70, ZF-20, Dabco T, Toyocat-NP, Toyocat-RX5, Dabco DMEA or Toyocat-TRC; the foam stabilizer is selected from at least one of L-5340, B-8715 LF2, B-8734 LF2, DC198, L-5440, AK-8805 or AK-8815; the isocyanate is selected from at least one of PM-200, M20S, 44V20 or PAPI-135C; the compressive strength of the high temperature resistant polyurethane sheet foam material is 209~265Kpa, and the tensile strength is 200~232Kpa.

2. A method for preparing the high temperature resistant polyurethane sheet foam material according to claim 1, The following steps are involved: (1) Prepare the raw materials according to the following weight proportions: The weight ratio of component A to component B is 100:100-150, wherein component A comprises, by weight: 1-30 parts of polyether polyol I, 61.4-78 parts of polyether polyol II, 3-10 parts of crosslinking agent, 0.5-1 part of catalyst, 0.5-2 parts of foam stabilizer, and 1.5-2.5 parts of water; component B is isocyanate; the average molecular weight of the polyether polyol I is 3000-8000, and the functionality is 2-4; the average molecular weight of the polyether polyol II is 200-900, and the functionality is 3-8; the crosslinking agent is an amino acid compound; the catalyst is selected from at least one of a low-atomization catalyst, a delayed catalyst, or a non-volatile catalyst; the foam stabilizer is at least one of a polysiloxane-oxidized olefin block copolymer; (2) Preparation of component A: According to the components and weight proportions in step (1), polyether polyol I, polyether polyol II, a crosslinking agent, a catalyst, a foam stabilizer and water are sequentially added into container A, and stirred evenly at a temperature of 20 to 25° C. to obtain a mixed material I; (3) Preparation of component B: Add isocyanate into container B according to the components and weight proportions in step (1), and stir evenly at 20-25°C; (4) Component A and component B are mixed and stirred quickly in a weight ratio of 100:100-150, and then injected into a pre-prepared tooling mold. After free rising, a high temperature resistant polyurethane sheet foam material is obtained.

3. Application of the high temperature resistant polyurethane sheet foam material according to claim 1 in automobile coat rack panels.

Citation Information

Patent Citations

  • High-temperature-resistant and aging-resistant polyurethane material and preparation method thereof

    CN112574382A

  • Light polyurethane plastic rubber paving material

    CN101195705A

  • Degradable foamed plastic and preparation method thereof

    CN104292784A

  • Low-VOC hydrolysis-resistant polyurethane foam and preparation method thereof

    CN108610463A

  • Karst pipeline type ultrahigh-expansion grouting material for efficient blocking of gushing water, and preparation method, use method and application thereof

    CN110835449A