A method for post-weld heat treatment of medium-carbon low-alloy rails in a low-temperature field environment
By using multi-stage heat treatment and mobile flash welding technology in low temperature environments, the problem of insufficient impact toughness and fatigue resistance of rail welded joints is solved, and the hardness and safety of rail welded joints are improved, avoiding the formation of martensite structure .
Patent Information
- Application Number
- CN202211479638.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-24
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-11-24
AI Technical Summary
In low temperature environments, the impact toughness and fatigue resistance of the welded joints of railway rails are insufficient, and the existing welding process leads to martensite structure in the heat-affected zone of the joint, affecting the service performance of the rails and the safety of railway operation.
A medium-carbon low-alloy rail post-weld heat treatment method is adopted in the field low-temperature environment. Multi-stage heating and cooling treatment is carried out through the contour temperature control device to ensure uniform temperature heating and cooling of the rail head, rail waist and rail bottom to avoid Martha The formation of body tissues and the use of mobile flash welding technology is used to control the welding heat input.
It effectively improves the hardness and impact toughness of the rail welded joints, ensures the uniformity of the mechanical properties of the joints, avoids the generation of martensite structure, and ensures the safety of railway operation.
Smart Images

Figure CN115725831B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of railway rail manufacturing, and in particular to a post-weld heat treatment construction method for a medium-carbon low-alloy rail in a field low-temperature environment. Background Art
[0002] In recent years, the development trend of domestic and foreign railway systems towards high speed and heavy load has put forward high requirements for the comprehensive performance of rail parent materials and welded joints. At present, the carbon content of railway rails is mainly concentrated in 0.7-1.1%, with full pearlite structure or structure of pearlite + a small amount of proeutectoid ferrite or proeutectoid cementite. The rail strength is usually required to be not less than 880MPa and have good wear resistance. In areas with colder winters, harsh sections with special natural conditions such as large temperature differences throughout the year and day and night temperature differences, new requirements are put forward for the impact toughness and fatigue damage resistance of rails. As the U71Mn hot-rolled rail widely used on the line, the U-shaped impact toughness of the rail head of this rail is 25-30J at room temperature (20-30℃), while the U-shaped impact value of the rail head at low temperature -40℃ is only 5-8J, and the impact toughness is greatly reduced. In this case, medium-carbon low-alloy rails with higher impact toughness and better fatigue damage resistance came into being. However, similar to other types of pearlite rails, this type of rail also has the problem of poor impact toughness of the entire section of the welded joint in welding applications. Therefore, post-weld heat treatment has become the most effective means to improve the impact toughness of rail joints and improve the service performance of joints.
[0003] Conventional rail post-weld normalizing equipment heats the entire cross-section of the joint as a whole, and the temperature collection (temperature measurement) position is the rail head tread of the rail welding joint. When conventional normalizing equipment is used to heat the rail joint, the thickness of the rail waist and rail bottom area is relatively thin, and it is easy to reach the set normalizing heating temperature first. However, the thickness of the rail head area is large, the heat conduction is relatively slow, and the heating process is obviously lagging behind the rail waist and rail bottom. It is often manifested that the joint rail waist and rail bottom area have reached the set normalizing temperature first, while the rail head area has not yet reached the set temperature. When the rail head of the rail joint reaches the set temperature, the rail waist and rail bottom have already exceeded the set temperature due to long-term heating. In this case, the impact toughness of the welding heat-affected zone at the rail waist and rail bottom of the rail joint is easily reduced due to excessive heating temperature and long high temperature residence time during the normalizing process. In addition, the difference in temperature distribution between the rail head, rail waist and rail bottom during the normalizing process will indirectly lead to differences in the microstructure, austenite grain size, residual stress, etc. at the rail head, rail waist and rail bottom, affecting the uniformity of the mechanical properties of the entire cross-section of the rail joint, which will further lead to differences in the service performance of the entire cross-section of the rail joint, which is not conducive to the safety of railway operation.
[0004] At present, with the increase in railway transportation volume, rails serving in low-temperature environments have put forward new requirements for wear resistance, low-temperature toughness, etc. When welding in such a low-temperature environment, the existing welding method is prone to low-temperature brittle fracture of the welded joint due to the low field environment temperature and limited welding process, resulting in unqualified welded joint quality.
[0005] Therefore, there is a need in the prior art for improving the post-weld heat treatment of medium carbon low alloy rails. Summary of the invention
[0006] In view of this, the purpose of the embodiment of the present invention is to propose a post-weld heat treatment construction method for medium-carbon low-alloy rails in a field low-temperature environment, to improve the tread hardness of the rails reduced by welding, and at the same time to improve the impact toughness of the rail joints, to ensure the service performance of the dissimilar rail welded joints and the safety of railway operation.
[0007] Based on the above purpose, the embodiment of the present invention provides a method for post-weld heat treatment of medium-carbon low-alloy rails in a low-temperature outdoor environment, the method comprising the following steps:
[0008] The welded rail joint is placed in a contoured temperature control device for a first cooling treatment by means of thermal compensation, and cooled to 200-300°C;
[0009] The rail joint is subjected to full-section heating treatment in the profiling temperature control device, and heated to 900-960°C. During the heating treatment, the rail head, rail waist and rail bottom of the rail joint are respectively controlled and heated;
[0010] Remove the contour temperature control device, place the rail joint in a low-temperature outdoor environment for the second cooling process, and cool it naturally to 400-450℃;
[0011] The rail joint is placed in a contoured temperature control device for a third cooling process by means of thermal compensation, and cooled to 200-250°C;
[0012] The contoured temperature control device is removed, and the rail joint is placed in a low-temperature outdoor environment for the fourth cooling treatment, and is naturally cooled to ambient temperature.
[0013] In some embodiments, during the heating treatment, the heating temperature of the rail waist and rail bottom of the contoured temperature control device is set to be 20-40° C. higher than the heating temperature of the rail head.
[0014] In some embodiments, the rail joint is welded by mobile flash welding, the upset amount is maintained at 11.9-12.9 mm during welding, and the heat input amount of 9.5-11.2 MJ is used during welding.
[0015] In some embodiments, the contoured temperature control device is a split-type contoured temperature control device, and temperature control is achieved by arranging a plurality of ceramic electric heating plates in the split-type contoured temperature control device.
[0016] In some embodiments, the cooling rate during the first cooling process is 0.5 to 1.1° C. / s.
[0017] In some embodiments, the cooling rate during the second cooling process is 4.0 to 15.0°C / s
[0018] In some embodiments, the cooling rate during the third cooling process is 0.5 to 1.1 °C / s
[0019] In some embodiments, the microstructure of the rail base material of the medium carbon low alloy rail includes 94-99% pearlite and 1-6% proeutectoid ferrite, and the rail base material contains, by weight percentage: 0.56-0.66% C, 0.40-0.70% Si, 0.55-0.8% Mn, 0.20-0.40% Cr, 0.15-0.45% Cu, 0.05-0.25% Ni, 0.02-0.12% V, and the balance is Fe and unavoidable impurities.
[0020] In some embodiments, the tensile strength of the rail base material at room temperature (20-30°C) is 1050-1200MPa, the elongation is 12.5-17.5%, the room temperature U-type impact energy of the rail head of the rail base material is 38-55J, the room temperature U-type impact energy of the rail waist and rail bottom is in the range of 18-30J, the room temperature impact energy of the rail head weld of the welded rail joint is in the range of 10-17J, and the room temperature impact energy of the rail waist and rail bottom weld is in the range of 8-13J.
[0021] Another aspect of the present invention provides a medium-carbon low-alloy rail joint for use in a field low-temperature environment, wherein the rail joint is formed by using the above method.
[0022] The present invention has at least the following beneficial technical effects:
[0023] The invention discloses a method for post-weld heat treatment of medium-carbon low-alloy rails for outdoor low-temperature environments, which can effectively improve the joint hardness and impact toughness through comprehensive control of rail welding process and post-weld heat treatment, and can avoid the appearance of harmful martensitic structure in the heat-affected zone of the joint. The average hardness of the medium-carbon low-alloy rail welded joint obtained by the welding method of the invention at room temperature (20-30°C) reaches 90-95% of the hardness of the corresponding parent material. At room temperature, the average impact energy of the normalized joint rail head weld reaches 28-40J, and the impact energy of the rail waist and rail bottom welds ranges from 16-25J; under the low-temperature test condition of -20°C, the average impact energy of the normalized joint rail head weld reaches 20-32J, and the impact energy of the rail waist and rail bottom welds ranges from 10-18J, which helps to ensure the safety of railway operation.
[0024] The rail joint of the present invention has the same beneficial effects as the above method. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other embodiments can be obtained based on these drawings without paying creative work.
[0026] Figure 1 A schematic diagram of the sampling position of the impact specimens of the rail welded joint is shown. In the embodiments and comparative examples, the impact toughness at the rail head, rail waist and rail bottom of the rail welded joint is the average value of the impact energy of the impact specimens at the rail head, rail waist and rail bottom of the rail welded joint at room temperature. Among them, the impact toughness at the rail head of the welded joint is the average impact energy of the corresponding 1# to 4# specimens, the impact toughness at the rail waist of the welded joint is the average impact energy of the corresponding 5# to 8# specimens, and the impact toughness at the rail bottom of the welded joint is the average impact energy of the corresponding 9# to 14# specimens;
[0027] Figure 2 This is a schematic diagram of the hardness test position of the rail joint longitudinal section;
[0028] Figure 3 Schematic diagram of the cutting position of metallographic samples in various embodiments and comparative examples, in which d is the heat affected zone and c is the weld;
[0029] Figure 4 Schematic diagram of the distribution of electric heaters in the rail head of the split-type contour temperature control device
[0030] Figure 5 It is an overall schematic diagram of a split-type contour temperature control device;
[0031] Figure 6 The metallographic structure diagram of the welding heat affected zone of Example 1;
[0032] Figure 7 The metallographic structure diagram of the welding heat affected zone of Comparative Example 1;
[0033] Figure 8 This is the metallographic structure diagram of the welding heat affected zone of Comparative Example 2;
[0034] Fig. 9 This is the metallographic structure diagram of the welding heat affected zone of Comparative Example 3;
[0035] Fig.10 The metallographic structure diagram of the welding heat affected zone of Comparative Example 4;
[0036] Fig.11This is the metallographic structure diagram of the welding heat affected zone of Comparative Example 5;
[0037] Fig.12 This is the metallographic structure diagram of the welding heat affected zone of comparative example 7.
[0038] In the figure:
[0039] a and c are the rail base material area, b is the weld heat affected zone of the weld joint, d is the rail head tread, e is the weld center, f is the metallographic specimen sampling position, A3 is the rail head tread heating area, B3 is the rail head side heating area, C3 is the rail head jaw heating area, D3 is the circular crawler ceramic electric heater, E3 is the rail joint rail head weld positioning line, A1 / A2 / B1 / B2 are terminal posts, C is the circular crawler ceramic electric heater at the rail waist, D is the rotating shaft, E is the fixed clamp ring, F is the device casing, and G is the asbestos insulation layer.
[0040] It should be noted that the rail post-weld heat treatment device of the present invention is fixed with the center of the rail head weld of the rail weld joint (weld positioning line) as the boundary. The A1 terminal and the A2 terminal form a loop and perform full-section controlled heating on the left half of the device (rail weld joint); the B1 terminal and the B2 terminal form a loop and perform full-section controlled heating on the right half of the device (rail weld joint).
[0041] It should be pointed out that the heating capacity (heating rate, heating temperature) of the left and right halves of the profiling device during the heat treatment process is the same. The ceramic electric heaters in the rail head area of the profiling device are densely distributed and small in size, so the heating temperature is higher. The ceramic electric heaters in the waist and bottom areas of the profiling device are large in size and sparsely distributed compared to the head of the profiling device, so the heating temperature of the waist and bottom areas of the profiling device is slightly lower than that of the head area of the profiling device. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0043] During rail welding, the brittle martensite structure produced in the weld and heat-affected zone is directly related to the service life of the rail and even endangers driving safety. In rail welding production, large-sized martensite is often formed in the heat-affected zone due to improper welding process and post-weld cooling control. The formation of large-sized martensite is inevitably accompanied by a sharp expansion of the volume of the local area, resulting in the formation of microcracks inside the martensite. These microcracks will directly affect the service life of the rail joint and even endanger the safety of railway operation. It should be noted that the reheating austenitization process accompanied by the post-weld heat treatment of the rail can eliminate the martensite formed during the welding process, but it cannot eliminate the microcracks inside the martensite. Therefore, in order to ensure the service performance of the rail welded joint, it is necessary to avoid the formation of harmful martensite structure during rail welding and post-weld heat treatment. At present, the current railway industry rail welding standard TB / T1632.2-2014 stipulates that the structure of the rail joint weld and heat-affected zone should be mainly pearlite, a small amount of ferrite may appear, and harmful structures such as martensite or bainite should not appear. Welding gray spots are another major cause of rail joint drop weight, fatigue and tensile fracture.
[0044] During rail welding, the welding heat input should be strictly controlled to avoid the joint cooling too fast after welding and the formation of martensitic structure due to too low welding heat input. Especially in the field low-temperature construction environment, the cooling rate of the rail in the environment after welding is too fast (much higher than the critical cooling rate of martensitic transformation of rail steel). If the post-weld cooling control is not performed, harmful martensitic structure will be generated inside the joint. Therefore, in the field low-temperature construction environment, it is usually necessary to use a large heat input for rail welding to avoid the formation of martensitic structure due to the fast cooling rate of the joint in the low-temperature construction environment. At the same time, the performance control of the rail welding joint also needs to be matched with an appropriate amount of upsetting to fully eliminate defects such as welding gray spots and welding slag that may be formed in the weld, so as to reduce the influence of welding defects on the mechanical properties of the rail joint. Compared with the parent material, the mechanical properties of the rail joint will inevitably decline to varying degrees due to the influence of the flash welding thermal cycle process. At present, post-weld heat treatment is the most effective means to improve the organizational state of the rail joint and enhance the mechanical properties of the joint. Heat treatment of the joint after welding will have a significant effect on the impact toughness and hardness of the joint.
[0045] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0046] A method for post-weld heat treatment of medium-carbon low-alloy rails in a low-temperature outdoor environment comprises the following steps:
[0047] Flash welding of medium carbon low alloy rails was performed using a welding upset of 11.9-12.9 mm and a welding heat input of 9.5-11.2 MJ;
[0048] The welded rail joint is placed in a contoured temperature control device for a first cooling treatment by means of thermal compensation, and cooled to 200-300°C;
[0049] The rail joint is subjected to full-section heating treatment in the profiling temperature control device, and heated to 900-960°C. During the heating treatment, the rail head, rail waist and rail bottom of the rail joint are respectively controlled and heated;
[0050] Remove the contour temperature control device, place the rail joint in a low-temperature outdoor environment for the second cooling process, and cool it naturally to 400-450℃;
[0051] The rail joint is placed in a contoured temperature control device for a third cooling process by means of thermal compensation, and cooled to 200-250°C;
[0052] The contoured temperature control device is removed, and the rail joint is placed in a low-temperature outdoor environment for the fourth cooling treatment, and is naturally cooled to ambient temperature.
[0053] Among them, the cooling rate during the first cooling treatment is 0.5-1.1°C / s, the cooling rate during the second cooling treatment is 4.0-15.0°C / s, and the cooling rate during the third cooling treatment is 0.5-1.1°C / s. The cooling rate during the second cooling treatment is between 4.0 and 15.0°C / s, and there is a situation where the cooling rate is fast in the high temperature stage and relatively slow in the low temperature stage, that is, the cooling rates in different temperature sections are different. Specifically: when the temperature is greater than 800°C, the cooling rate is 12.0-15.0°C / s; when the temperature is between 800 and 500°C, the cooling rate is 7.0-11.9°C / s; when the temperature is less than 499°C, the cooling rate is 4.0-6.9°C / s.
[0054] The present invention utilizes a rail mobile flash welder, adopts a welding upset amount of 11.9-12.9mm, and a heat input of 9.5-11.2MJ to carry out welding of medium-carbon low-alloy rails. If the upset amount is less than 11.9mm, it is easy to cause large-sized weld gray spots, welding non-metallic inclusions, etc., which cannot be discharged in time, reducing the impact toughness of the weld. If the welding upset amount is higher than 12.9mm, it is easy to cause the weld metal to be discharged excessively, forming a cold joint, and reducing the impact toughness of the weld. The welding heat input is controlled at 9.5-11.2MJ to ensure that the rail joint after welding will not cool too quickly due to the low ambient temperature in the low-temperature field construction environment, avoid the appearance of martensite in the heat-affected zone of the rail welding in the welded state, and effectively avoid the formation of large-sized gray spot defects. Under the low-temperature field construction conditions of -20 to 0°C, due to the rapid cooling of the rail joint after welding, when the welding heat input is lower than 9.2MJ, randomly distributed point martensite will appear in the heat-affected zone of the rail welding. Under low-temperature field construction conditions of -20 to 0℃, when the welding heat input is higher than 11.2MJ, large-sized gray spots and melting holes in the overheated zone may appear at the weld, affecting the impact toughness and service safety of the joint.
[0055] In order to avoid the formation of harmful martensitic structure in the heat affected zone during rail welding and post-weld heat treatment, the cooling rate during welding and post-weld heat treatment can be controlled by artificial intervention to be lower than the critical cooling rate of martensitic transformation of rail steel, or the final cooling temperature of the rapid cooling stage of welding and post-weld heat treatment can be controlled above the starting temperature of martensitic transformation Ms of rail steel at a cooling rate higher than the critical cooling rate of martensitic transformation of rail steel, and then the rail steel is cooled to ambient temperature at a cooling rate lower than the critical cooling rate of martensitic transformation of rail steel. In the process of rail welding and post-weld heat treatment, in order to improve the hardness and toughness of the welding area, accelerated cooling (such as spraying compressed air) is usually adopted to obtain pearlite structure with finer interlamellar spacing in the weld heat affected zone.
[0056] Due to the addition of alloying elements such as Si, Mn, and Cr, the critical cooling rate of martensitic transformation of the medium-carbon low-alloy rail involved in the present invention is between 1.2 and 1.8°C. In a normal temperature (20-30°C) environment, the rails cool naturally with the environment after welding (air cooling), and no harmful martensitic structure will be formed in the heat-affected zone of the rail welding due to excessive cooling speed. However, in a low-temperature (-20-0°C) field construction environment, the lower ambient temperature leads to an extremely fast cooling rate during rail welding and post-weld heat treatment (the cooling rate can reach 4.0-15.0°C / s), which creates conditions for the formation of martensite. Therefore, when performing rail welding and post-weld heat treatment in a low-temperature field environment, special attention should be paid to the generation of martensitic structure, that is, the rail welding and post-weld heat treatment process should be strictly controlled.
[0057] The present invention forms a joint by welding a medium-carbon low-alloy rail with a specification of 60kg / m through a rail mobile flash welder. The welded joint includes an area with a length of 70 to 110 mm including a weld and a heat-affected zone, and the center of the area is the weld. In the present invention, the "room temperature or normal temperature" is a temperature in the range of 20 to 30°C, and the "low-temperature field construction environment" is a temperature in the range of -20 to 0°C.
[0058] In the present invention, the critical cooling rate of martensitic transformation in the continuous cooling process of medium carbon low alloy rail steel is between 1.2 and 1.8°C / s, and the martensitic transformation starting temperature is between 251 and 280°C. For the post-weld heat treatment of medium carbon low alloy rails, in order to improve the mechanical properties of the welding heat affected zone and avoid the formation of harmful martensite due to too fast cooling during the heat treatment process, the rapid cooling stage is selected to cool at a cooling rate higher than the critical cooling rate of martensitic transformation of the rail steel, and the final cooling temperature is controlled above the martensitic transformation Ms temperature of the rail steel. Taking into account the inevitable component segregation in the alloying process of rail steel and the welding construction in the field under low temperature environment, in order to avoid the generation of martensite during the post-weld heat treatment, the final cooling temperature of the rapid cooling stage of the post-weld heat treatment of the rail steel is controlled to be above 100°C of the martensitic transformation Ms temperature of the rail steel in the present invention.
[0059] It should be pointed out that the post-weld heating treatment of the rail is a heat treatment process without insulation. The heating process ends after the rail joint is heated to the set temperature, and then enters the cooling stage. Compared with the rail waist and rail bottom, the rail head has a significant heating lag during the heat treatment process due to its large thickness. During the post-weld heat treatment of the rail welded joint using a traditional medium-frequency induction normalizing unit, when the rail waist and rail bottom are heated to the set temperature, the rail head temperature is significantly lower than the rail waist and rail bottom. In order to achieve the impact toughness matching between the rail head of the rail welded joint and the rail waist and rail bottom, it is necessary to appropriately increase the heating temperature of the rail welded joint area, while ensuring that the rail head area of the welded joint is fully austenitized, and the mechanical properties of the joint rail head area will not be reduced due to overheating of the tissue. In the present invention, by reasonably arranging the size, number and distribution distance of the ceramic electric heating plate embedded in the split device, the heating temperature difference between the rail head and the rail waist and rail bottom areas is eliminated, so that the rail head of the rail joint reaches the same heating temperature as the rail waist and rail bottom at the same time.
[0060] In the present invention, the normalizing heat treatment generally refers to a heat treatment process in which a metal workpiece is heated to 30 to 50°C above Ac3 (the final temperature at which ferrite transforms to austenite during heating) in a conventional manner, and after a period of heat preservation, the metal workpiece is taken out of the furnace and cooled naturally in the air, or sprayed, or cooled by compressed air. The post-weld normalizing heat treatment of rail joints is different from the heat treatment process usually used for small-sized workpieces, because the length of the sample after rail welding can be as high as hundreds of meters, which determines that the normalizing heat treatment of rail welded joints cannot be kept warm for a long time after reaching the target temperature (temperature above the austenitizing temperature). Therefore, a heat treatment process is generally performed in which the rail welded joint is heated to the target temperature at a temperature slightly higher than the conventional normalizing temperature, and then air-cooled or air-cooled. The preferred normalizing heating temperature of the present invention is 900 to 960°C.
[0061] In the present invention, the second cooling treatment is natural cooling in a field construction environment (-20 to 0°C). Due to the low ambient temperature, the cooling rate in the natural cooling stage is between 4.0 and 15.0°C / s, and there is a situation where the cooling rate is fast in the high temperature stage and relatively slow in the low temperature stage, that is, the cooling rates in different temperature sections are different. Specifically: when the temperature is greater than 800°C, the cooling rate is 12.0 to 15.0°C / s; when the temperature is between 800 and 500°C, the cooling rate is 7.0 to 11.9°C / s; when the temperature is less than 499°C, the cooling rate is 4.0 to 6.9°C / s. In the present invention, in order to avoid the formation of martensite after rail welding in a low-temperature field construction environment, a split device is used to cover the rail head, rail waist and rail bottom of the rail joint immediately after the rail welding is completed to slow down the cooling rate of the rail joint after welding. At the same time, the rail joint is cooled to 200-300°C at a cooling rate of 0.5-1.1°C / s in the split device by thermal compensation, and then a subsequent heat treatment is performed. It should be noted that the ceramic electric heater embedded in the split device is used for thermal compensation to regulate the cooling rate of this stage. When the cooling rate is lower than 0.5°C / s, the cooling rate is too slow and takes too long, which will affect the subsequent rail welding production. When the cooling rate is higher than 1.1°C / s, since the critical cooling rate of martensitic transformation of rail steel is 1.2°C / s, the excessively high cooling rate may cause the formation of martensitic structure in the continuous cooling process after the rail joint is welded, affecting the service safety of the rail joint. Therefore, in the present invention, in the cooling stage after the flash welding of the rail, the joint is cooled at a cooling rate of 0.5 to 1.1°C / s in a split device in a thermally compensated manner to avoid the formation of martensite in the heat-affected zone of the rail welding. In the subsequent heat treatment process, the surface of the rail head of the rail joint is heated to 900 to 960°C in the split device. After the heating of the rail joint is completed, the split device is disassembled from the middle position to allow the rail joint to cool rapidly with the environment in the field construction environment. The second cooling stage in the present invention is natural cooling in a field low-temperature construction environment, and the cooling rate is between 4.0 and 15.0°C / s, which is much higher than the critical cooling rate of martensitic transformation of rail steel of 1.2 to 1.8°C / s, so as to refine the pearlite lamellar spacing by accelerating the cooling of the supercooled austenite and improve the mechanical properties of the pearlite structure in the welding area. The final cooling temperature of the second cooling stage in the present invention is 400-450°C, which is more than 100°C higher than the martensitic transformation start temperature of the rail steel of 251-280°C, which helps to avoid the martensitic structure formed during the rapid cooling process of the heat treatment. When the surface temperature of the rail joint head drops to 400-450°C, the third cooling treatment is immediately carried out. In this stage, the rail joint is cooled to 200-250°C at a cooling rate of 0.5-1.1°C / s by means of thermal compensation of the profiling temperature control device, and then the power supply to the split device is stopped and the device is dismantled, and the fourth cooling treatment is carried out to cool the joint to an ambient temperature of -20-0°C in the field environment.
[0062] It should be pointed out that when the surface temperature of the rail joint reaches 400-450℃, the core of the rail joint is about 30-50℃ higher than the surface, that is, the core temperature is 430-500℃, at which time the surface and core of the rail joint have completed the pearlite transformation. When the rail joint is subsequently cooled at a cooling rate lower than the critical cooling rate of the martensitic transformation of rail steel, no martensitic structure will be generated.
[0063] It should be pointed out that the thermal compensation during the cooling process after the rail welding and the thermal compensation during the subsequent post-weld heat treatment cooling stage are all carried out in the split device through a contoured temperature control device. The device is internally distributed with densely arranged disc-shaped crawler-type ceramic electric heaters, which can fit closely with the surface of the rail to achieve good heat conduction. The thermal compensation process of the rail joint is achieved under the joint action of multiple rows of parallelly distributed disc-shaped crawler-type ceramic electric heaters.
[0064] Figure 7 The layout of the rail head, rail waist and rail bottom heating areas of the split-type contoured temperature control device shown is similar. Because the rail head is thicker and the heat transfer is slower, the number of disc-shaped crawler-type ceramic electric heaters covering the rail head is larger and denser than that of the crawler-type ceramic electric heaters in the rail waist and rail bottom areas, and the diameter of the electric heaters is smaller, so as to ensure that the rail head of the rail joint is fully heated. In addition, the size and density of the disc-shaped crawler-type electric heaters distributed on the left and right sides of the split-type device are the same. By reasonably arranging the size, number and distribution distance of the ceramic electric heaters embedded in the split-type device, the heating temperature difference between the rail head and the rail waist and rail bottom areas is eliminated, so that the rail head of the rail joint and the rail waist and rail bottom reach the same heating temperature at the same time.
[0065] like Figure 8The split-type contour temperature control device shown has the advantages of being small, flexible, and low-cost, and is convenient for field construction. It can be powered by a diesel generator with a voltage of 380V or 220V AC mains, and has a rated power of 10kW. The device uses a commercial LCD disc-shaped crawler ceramic electric heater as a heat source. The split-type device uses a disc-shaped crawler ceramic electric heater with a diameter of φ5mm and a thickness of 5mm in the rail head area, while the split-type device uses a disc-shaped crawler ceramic electric heater with a diameter of φ8mm and a thickness of 5mm in the rail waist and rail bottom area. With asbestos insulation material and steel structure shell, it is made into a rail contour split heater, which is easy to assemble and disassemble and is suitable for local heating of rail welding joints. The actual size of the heating device and the specifications and distribution of the heater can be adjusted and changed according to the actual profile of the rail. During the design of the device, multiple rows of parallel circular track-type ceramic electric heaters are evenly fixed on the inner side of a device with a similar rail profile, so that the heating plates are evenly coated on the surface of the rail and fully fit the surface of the rail to achieve good heat conduction during the heating process. Based on this device, thermal compensation and normalizing heating of the rail joint are realized. During the test, a temperature controller is used to control the heating temperature. The operating temperature range of the split device is 400-1000℃, and the device can rotate up to 180° around the rotation axis.
[0066] Figure 7 A3 is the rail head tread heating area, B3 is the rail head side heating area, C3 is the rail head jaw heating area, D3 is a circular crawler ceramic electric heater, E3 is the rail joint rail head weld positioning line, A1 / A2 / B1 / B2 are terminals, C is a circular crawler ceramic electric heater at the rail waist, D is a rotating shaft, E is a fixed clamp, F is a device shell, and G is an asbestos insulation layer. It should be noted that the rail post-weld heat treatment device involved in the present invention is fixed with the center of the rail head weld of the rail welding joint (weld positioning line) as the boundary. The A1 terminal and the A2 terminal form a loop and perform full-section controlled heating on the left half of the device (rail welding joint); the B1 terminal and the B2 terminal form a loop and perform full-section controlled heating on the right half of the device (rail welding joint). It should be pointed out that the heating capacity (heating rate, heating temperature) of the left and right halves of the profiling device during the heat treatment process is the same. The ceramic electric heaters in the rail head area of the profiling device are densely distributed and small in size, so the heating temperature is higher. The ceramic electric heaters in the waist and bottom areas of the profiling device are large in size and sparsely distributed compared to the rail head of the profiling device. By reasonably arranging the size, number and distribution distance of the ceramic electric heaters embedded in the split device, the heating temperature difference between the rail head and the waist and bottom areas is eliminated, so that the rail head, waist and bottom of the rail joint reach the same heating temperature at the same time.
[0067] The present invention refers to the TB / T 1632.2-2014 "Rail Welding Part 2: Flash Welding" standard to machine the rail joint into a longitudinal section hardness specimen, and perform a longitudinal section Rockwell hardness test on the joint at a position 5 mm below the tread, the measuring points are symmetrically arranged to the left and right sides with the weld as the center, the measuring point spacing is 5 mm, the Rockwell hardness method is carried out in accordance with the provisions of GB / T230.1-2009, the HRC scale is adopted, Hp represents the average hardness of the rail base material, Hj represents the average hardness of the joint, and the position where the joint hardness is lower than 0.9 Hp represents the softening area.
[0068] Example 1
[0069] The microstructure of the rail base material is controlled to be 94% pearlite and 6% proeutectoid ferrite. The tensile strength of the rail base material at room temperature (20-25°C) is 1050MPa, the elongation is 17.5%, the U-type impact energy of the base material rail head at room temperature is 55J, and the U-type impact energy of the rail waist and rail bottom at room temperature is 30J. The chemical composition of the rail steel to obtain the microstructure and mechanical properties must meet the following conditions: 0.56% C, 0.40% Si, 0.55% Mn, 0.20% Cr, 0.15% Cu, 0.05% Ni, 0.02% V, and the remainder is Fe and unavoidable impurities.
[0070] Using a rail mobile flash welder, the rail flash welding was carried out with a heat input of 9.5 MJ. The actual welding upset was maintained at 11.9 mm. After the rail welding was completed, when the surface temperature of the rail head dropped below 250 °C, the following method was used: Figure 4 The split-type profiling temperature control device shown heats the rail head, rail waist and rail bottom of the rail joint separately. Heating is stopped when the surface temperature of the rail head, rail waist and rail bottom of the rail joint is heated to 900℃. Subsequently, the rail joint is cooled in the field construction environment. When the surface temperature of the joint drops to 400℃, the rail joint is cooled to 200℃ at a cooling rate of 0.5℃ / s by thermal compensation of the profiling temperature control device, and then the joint is cooled to an ambient temperature of -20℃ with the field environment, thereby completing the welding and post-weld heat treatment process of the medium-carbon low-alloy rail.
[0071] according to Figure 1 The rail joints obtained in this embodiment after post-weld heat treatment were machined into Charpy U-shaped impact specimens at the sampling position shown in the figure, and the weld was located at the center of the specimen. The impact test of the rail joint impact specimens was carried out at room temperature (20-30°C) using a SANS ZBC2000 impact testing machine. Figure 2-3The sampling method shown is to conduct metallographic inspection on the metallographic specimens of rail joints according to GB / T13298-2015 "Methods for Examination of Metal Microstructures", use 3% nitric acid alcohol solution to etch the metallographic specimens of rail joints, and use a German Leica MeF3 optical microscope to observe the metallographic structure of the rail joints.
[0072] The results show that for the normalized joint of the medium carbon low alloy rail obtained by the post-weld heat treatment construction method of the present invention, Figure 6 As shown, at 100X observation magnification, no martensitic structure appears in the heat affected zone of the rail joint. Among them, the weld structure is pearlite and intergranular proeutectoid ferrite, and the heat affected zone structure is pearlite and a small amount of proeutectoid ferrite. The average room temperature impact energy of the rail head weld of the obtained flash welding joint air-cooled (in welded state) is 17J, and the average room temperature impact energy of the welds at the rail waist and rail bottom is 13J. The average longitudinal section hardness of the normalized joint using the present invention reaches 90% of the hardness of the parent material. At room temperature, the average impact energy of the rail head weld of the normalized joint reaches 40J, and the impact energy of the rail waist and rail bottom welds is in the range of 25J; under the low temperature test condition of -20℃, the average impact energy of the rail head weld of the normalized joint reaches 32J, and the impact energy of the rail waist and rail bottom welds is in the range of 18J, which meets the various indicators required for rail welding joints in low temperature environments and helps to ensure the safety of railway operations.
[0073] Example 2
[0074] The microstructure of the rail base material is controlled to be 99% pearlite and 1% proeutectoid ferrite. The room temperature tensile strength of the rail base material is 1200MPa, the elongation is 12.5%, the average U-type impact energy of the base material rail head at room temperature is 38J, and the average U-type impact energy of the rail waist and rail bottom at room temperature is 18J. The chemical composition of the rail steel to obtain the microstructure and mechanical properties must meet the following conditions: 0.66% C, 0.70% Si, 0.85% Mn, 0.40% Cr, 0.45% Cu, 0.25% Ni, 0.12% V, the remainder is Fe and unavoidable impurities.
[0075] Using a rail mobile flash welder, the rail flash welding was carried out with a heat input of 11.2 MJ. The actual welding upset was maintained at 12.9 mm. After the rail was welded, when the surface temperature of the rail head dropped below 200 °C, the following method was used: Figure 4The split-type profiling temperature control device shown heats the rail head, rail waist and rail bottom of the rail joint separately. Heating is stopped when the surface temperature of the rail head, rail waist and rail bottom of the rail joint is heated to 960℃. Subsequently, the rail joint is cooled in the field construction environment. When the surface temperature of the joint drops to 450℃, the rail joint is cooled to 250℃ at a cooling rate of 1.1℃ / s through thermal compensation of the profiling temperature control device, and then the joint is cooled to an ambient temperature of 0℃ with the field environment, thereby completing the welding and post-weld heat treatment process of the medium-carbon low-alloy rail.
[0076] according to Figure 1 The rail joints obtained in this embodiment after post-weld heat treatment were machined into Charpy U-shaped impact specimens at the sampling position shown in the figure, and the weld was located at the center of the specimen. The impact test of the rail joint impact specimens was carried out at room temperature (20-30°C) using a SANS ZBC2000 impact testing machine. Figure 2-3 The sampling method shown is to conduct metallographic inspection on the metallographic specimens of rail joints according to GB / T13298-2015 "Methods for Examination of Metal Microstructures", use 3% nitric acid alcohol solution to etch the metallographic specimens of rail joints, and use a German Leica MeF3 optical microscope to observe the metallographic structure of the rail joints.
[0077] The results show that the metallographic structure of the normalized joint of the medium carbon low alloy rail obtained by the post-weld heat treatment construction method of the present invention is Figure 6 Consistent. At an observation magnification of 100X, no martensitic structure appeared in the heat affected zone of the rail joint. Among them, the weld structure is pearlite and intergranular proeutectoid ferrite, and the heat affected zone structure is pearlite and a small amount of proeutectoid ferrite. The average room temperature impact energy of the rail head weld of the obtained flash welding joint air-cooled (in welded state) is 10J, and the average room temperature impact energy of the welds at the rail waist and rail bottom is 8J. The average longitudinal section hardness of the normalized joint using the present invention reaches 95% of the hardness of the parent material. At room temperature, the average impact energy of the rail head weld of the normalized joint reaches 28J, and the impact energy of the rail waist and rail bottom welds is in the range of 16J; under the low temperature test conditions of -20℃, the average impact energy of the rail head weld of the normalized joint reaches 20J, and the impact energy of the rail waist and rail bottom welds is in the range of 10J, which meets the various indicators required for rail welding joints in low temperature environments and helps to ensure the safety of railway operations.
[0078] Example 3
[0079] The microstructure of the rail base material is controlled to be 96% pearlite and 3% proeutectoid ferrite. The room temperature tensile strength of the rail base material is 1100MPa, the elongation is 15%, the average U-type impact energy of the base material rail head at room temperature is 45J, and the average U-type impact energy of the rail waist and rail bottom at room temperature is 23J. The chemical composition of the rail steel to obtain the microstructure and mechanical properties must meet the following conditions: 0.60% C, 0.53% Si, 0.65% Mn, 0.30% Cr, 0.30% Cu, 0.15% Ni, 0.04% V, the remainder is Fe and unavoidable impurities.
[0080] Using a rail mobile flash welder, the rail flash welding was carried out with a heat input of 10.5 MJ. The actual welding upset was maintained at 12.4 mm. After the rail was welded, when the surface temperature of the rail head dropped below 250 °C, the following method was used: Figure 4 The split-type profiling temperature control device shown heats the rail head, rail waist and rail bottom of the rail joint separately. Heating is stopped when the surface temperature of the rail head, rail waist and rail bottom of the rail joint is heated to 920℃. Subsequently, the rail joint is cooled in the field construction environment. When the surface temperature of the joint drops to 420℃, the rail joint is cooled to 200℃ at a cooling rate of 0.8℃ / s by thermal compensation of the profiling temperature control device, and then the joint is cooled to an ambient temperature of -20℃ with the field environment, thereby completing the welding and post-weld heat treatment process of the medium-carbon low-alloy rail.
[0081] according to Figure 1 The rail joints obtained in this embodiment after post-weld heat treatment were machined into Charpy U-shaped impact specimens at the sampling position shown in the figure, and the weld was located at the center of the specimen. The impact test of the rail joint impact specimens was carried out at room temperature (20-30°C) using a SANS ZBC2000 impact testing machine. Figure 2-3 The sampling method shown is to conduct metallographic inspection on the metallographic specimens of rail joints according to GB / T13298-2015 "Methods for Examination of Metal Microstructures", use 3% nitric acid alcohol solution to etch the metallographic specimens of rail joints, and use a German Leica MeF3 optical microscope to observe the metallographic structure of the rail joints.
[0082] The results show that the metallographic structure of the normalized joint of the medium carbon low alloy rail obtained by the post-weld heat treatment construction method of the present invention is Figure 6Consistent. At 100X observation magnification, no martensitic structure appeared in the heat affected zone of the rail joint. Among them, the weld structure is pearlite and intergranular proeutectoid ferrite, and the heat affected zone structure is pearlite and a small amount of proeutectoid ferrite. The average room temperature impact energy of the rail head weld of the obtained flash welding joint air-cooled (in welded state) is 14J, and the average room temperature impact energy of the welds at the rail waist and rail bottom is 11J. The average longitudinal section hardness of the normalized joint using the present invention reaches 92% of the hardness of the parent material. At room temperature, the average impact energy of the rail head weld of the normalized joint reaches 33J, and the impact energy of the rail waist and rail bottom welds is in the range of 21J; under the low temperature test conditions of -20℃, the average impact energy of the rail head weld of the normalized joint reaches 25J, and the impact energy of the rail waist and rail bottom welds is in the range of 13J, which meets the various indicators required for rail welding joints in low temperature environments and helps to ensure the safety of railway operations.
[0083] Example 4
[0084] The microstructure of the rail base material is controlled to be 95% pearlite and 5% proeutectoid ferrite. The room temperature tensile strength of the rail base material is 1130MPa, the elongation is 14.5%, the average U-type impact energy of the base material rail head at room temperature is 42J, and the average U-type impact energy of the rail waist and rail bottom at room temperature is 21J. The chemical composition of the rail steel to obtain the microstructure and mechanical properties must meet the following conditions: 0.63% C, 0.56% Si, 0.65% Mn, 0.30% Cr, 0.33% Cu, 0.15% Ni, 0.04% V, the remainder is Fe and unavoidable impurities.
[0085] Using a rail mobile flash welder, the rail flash welding was carried out with a heat input of 10.0 MJ. The actual welding upset was maintained at 12.5 mm. After the rail welding was completed, when the surface temperature of the rail head dropped below 250 °C, the following method was used: Figure 4 The split-type profiling temperature control device shown heats the rail head, rail waist and rail bottom of the rail joint separately. Heating is stopped when the surface temperature of the rail head, rail waist and rail bottom of the rail joint is heated to 940℃. Subsequently, the rail joint is cooled in the field construction environment. When the surface temperature of the joint drops to 400℃, the rail joint is cooled to 200℃ at a cooling rate of 1.0℃ / s by thermal compensation of the profiling temperature control device, and then the joint is cooled to an ambient temperature of -20℃ with the field environment, thereby completing the welding and post-weld heat treatment process of the medium-carbon low-alloy rail.
[0086] according to Figure 1The rail joints obtained in this embodiment after post-weld heat treatment were machined into Charpy U-shaped impact specimens at the sampling position shown in the figure, and the weld was located at the center of the specimen. The impact test of the rail joint impact specimens was carried out at room temperature (20-30°C) using a SANS ZBC2000 impact testing machine. Figure 2-3 The sampling method shown is to conduct metallographic inspection on the metallographic specimens of rail joints according to GB / T13298-2015 "Methods for Examination of Metal Microstructures", use 3% nitric acid alcohol solution to etch the metallographic specimens of rail joints, and use a German Leica MeF3 optical microscope to observe the metallographic structure of the rail joints.
[0087] The results show that the metallographic structure of the normalized joint of the medium carbon low alloy rail obtained by the post-weld heat treatment construction method of the present invention is Figure 6 Consistent. At an observation magnification of 100X, no martensitic structure appeared in the heat affected zone of the rail joint. Among them, the weld structure is pearlite and intergranular proeutectoid ferrite, and the heat affected zone structure is pearlite and a small amount of proeutectoid ferrite. The average room temperature impact energy of the rail head weld of the obtained flash welding joint after air cooling (in welded state) is 13J, and the average room temperature impact energy of the welds at the rail waist and rail bottom is 10J. The average longitudinal section hardness of the normalized joint using the present invention reaches 93% of the hardness of the parent material. At room temperature, the average impact energy of the rail head weld of the normalized joint reaches 32J, and the impact energy of the rail waist and rail bottom welds is in the range of 20J; under the low temperature test conditions of -20℃, the average impact energy of the rail head weld of the normalized joint reaches 24J, and the impact energy of the rail waist and rail bottom welds is in the range of 11J, which meets the various indicators required for rail welding joints in low temperature environments and helps to ensure the safety of railway operations.
[0088] Comparative Example 1
[0089] The microstructure of the rail base material is controlled to be 94% pearlite and 6% proeutectoid ferrite. The tensile strength of the rail base material at room temperature (20-25°C) is 1050MPa, the elongation is 17.5%, the U-type impact energy of the base material rail head at room temperature is 55J, and the U-type impact energy of the rail waist and rail bottom at room temperature is 30J. The chemical composition of the rail steel to obtain the microstructure and mechanical properties must meet the following conditions: 0.56% C, 0.40% Si, 0.55% Mn, 0.20% Cr, 0.15% Cu, 0.05% Ni, 0.02% V, and the remainder is Fe and unavoidable impurities.
[0090] A mobile rail flash welder was used to carry out rail flash welding with a heat input of 9.5 MJ. The actual welding upset was maintained at 11.9 mm. After the rails were welded, no heat treatment was performed on the joints. Instead, the joints were allowed to cool naturally to ambient temperature (-20°C) in the low-temperature outdoor construction environment.
[0091] according to Figure 1 The rail joint obtained in this comparative example without post-weld heat treatment was machined into a Charpy U-shaped impact specimen at the sampling position shown in the figure, and the weld was located at the center of the specimen. The impact test of the rail joint impact specimen was carried out at room temperature (20-30°C) using a SANS ZBC2000 impact testing machine. Figure 2-3 The sampling method shown is to conduct metallographic inspection on the metallographic specimens of rail joints according to GB / T13298-2015 "Methods for Examination of Metal Microstructures", use 3% nitric acid alcohol solution to etch the metallographic specimens of rail joints, and use a German Leica MeF3 optical microscope to observe the metallographic structure of the rail joints.
[0092] The results show that: for the rail joints obtained without the post-weld heat treatment construction method of the present invention, Figure 7 As shown in the figure, at 100X observation magnification, a large amount of martensite structure appeared in the heat affected zone of the rail joint. Due to the natural cooling of the joint in the low temperature environment in the field after welding, a large amount of martensite structure was formed in the heat affected zone of the rail welding, resulting in a significant decrease in the impact toughness of the joint. The average room temperature impact energy of the rail head weld of the flash welding joint after air cooling (welded state) was 12J, and the average room temperature impact energy of the welds at the rail waist and rail bottom was 7J; under the low temperature test condition of -20℃, the average impact energy of the rail head weld of the normalized joint reached 8J, and the impact energy of the rail waist and rail bottom welds was in the range of 4J. The poor impact toughness of the rail joint and the presence of a large amount of martensite in the heat affected zone are not conducive to the safety of railway operation.
[0093] Comparative Example 2
[0094] The microstructure of the rail base material is controlled to be 94% pearlite and 6% proeutectoid ferrite. The tensile strength of the rail base material at room temperature (20-25°C) is 1050MPa, the elongation is 17.5%, the U-type impact energy of the base material rail head at room temperature is 55J, and the U-type impact energy of the rail waist and rail bottom at room temperature is 30J. The chemical composition of the rail steel to obtain the microstructure and mechanical properties must meet the following conditions: 0.56% C, 0.40% Si, 0.55% Mn, 0.20% Cr, 0.15% Cu, 0.05% Ni, 0.02% V, and the remainder is Fe and unavoidable impurities.
[0095] Using a rail mobile flash welder, the rail flash welding was carried out with a heat input of 9.5 MJ. The actual welding upset was maintained at 11.9 mm. After the rail was welded, when the surface temperature of the rail head dropped to 250 °C, the following method was used: Figure 4The split-type profiling temperature control device shown heats the rail head, rail waist and rail bottom of the rail joint separately. Heating is stopped when the surface temperature of the rail head, rail waist and rail bottom of the rail joint is heated to 900℃. Subsequently, the rail joint is cooled in the field construction environment. When the surface temperature of the joint drops to 250℃, the rail joint is cooled to 200℃ at a cooling rate of 0.5℃ / s by thermal compensation of the profiling temperature control device, and then the joint is cooled to an ambient temperature of -20℃ with the field environment, thereby completing the welding and post-weld heat treatment process of the medium-carbon low-alloy rail.
[0096] according to Figure 1 The rail joints obtained in this comparative example after post-weld heat treatment were machined into Charpy U-shaped impact specimens at the sampling position shown in the figure, and the weld was located at the center of the specimen. The impact test of the rail joint impact specimens was carried out at room temperature (20-30°C) using a SANS ZBC2000 impact testing machine. Figure 2-3 The sampling method shown is to conduct metallographic inspection on the metallographic specimens of rail joints according to GB / T13298-2015 "Methods for Examination of Metal Microstructures", use 3% nitric acid alcohol solution to etch the metallographic specimens of rail joints, and use a German Leica MeF3 optical microscope to observe the metallographic structure of the rail joints.
[0097] The results show that for the rail normalizing joints obtained without adopting the post-weld heat treatment construction method of the present invention, Figure 8 As shown in the figure, at 100X observation magnification, a large amount of martensitic structure appeared in the heat affected zone of the rail joint. The average room temperature impact energy of the rail head weld of the air-cooled (welded) joint after flash welding is 17J, and the average room temperature impact energy of the welds at the rail waist and rail bottom is 13J. The average hardness of the longitudinal section of the normalized joint reached 96% of the hardness of the parent material. Since the final cooling temperature of the joint in the rapid cooling stage of the post-weld heat treatment is 250℃, which is lower than the martensitic transformation start temperature of the rail steel 251~280℃, a large amount of martensitic structure is formed in the heat affected zone of the rail welding, resulting in poor impact toughness of the joint. At room temperature, the average impact energy of the rail head weld of the normalized joint reaches 14J, and the impact energy of the rail waist and rail bottom welds is in the range of 8J; under the low temperature test condition of -20℃, the average impact energy of the rail head weld of the normalized joint reaches 10J, and the impact energy of the rail waist and rail bottom welds is in the range of 5J. The impact toughness of the joint is poor, which is not conducive to the safety of railway operation.
[0098] Comparative Example 3
[0099] The microstructure of the rail base material is controlled to be 94% pearlite and 6% proeutectoid ferrite. The tensile strength of the rail base material at room temperature (20-25°C) is 1050MPa, the elongation is 17.5%, the U-type impact energy of the base material rail head at room temperature is 55J, and the U-type impact energy of the rail waist and rail bottom at room temperature is 30J. The chemical composition of the rail steel to obtain the microstructure and mechanical properties must meet the following conditions: 0.56% C, 0.40% Si, 0.55% Mn, 0.20% Cr, 0.15% Cu, 0.05% Ni, 0.02% V, and the remainder is Fe and unavoidable impurities.
[0100] Using a rail mobile flash welder, the rail flash welding was carried out with a heat input of 9.5 MJ. The actual welding upset was maintained at 11.9 mm. After the rail welding was completed, when the surface temperature of the rail head dropped below 250 °C, the following method was used: Figure 4 The split-type profiling temperature control device shown heats the rail head, rail waist and rail bottom of the rail joint separately. Heating is stopped when the surface temperature of the rail head, rail waist and rail bottom of the rail joint is heated to 900℃. Subsequently, the rail joint is cooled in the field construction environment. When the surface temperature of the joint drops to 400℃, the rail joint is cooled to 200℃ at a cooling rate of 1.2℃ / s by thermal compensation of the profiling temperature control device, and then the joint is cooled to an ambient temperature of -20℃ with the field environment, thereby completing the welding and post-weld heat treatment process of the medium-carbon low-alloy rail.
[0101] according to Figure 1 The rail joints obtained in this comparative example after post-weld heat treatment were machined into Charpy U-shaped impact specimens at the sampling position shown in the figure, and the weld was located at the center of the specimen. The impact test of the rail joint impact specimens was carried out at room temperature (20-30°C) using a SANS ZBC2000 impact testing machine. Figure 2-3 The sampling method shown is to conduct metallographic inspection on the metallographic specimens of rail joints according to GB / T13298-2015 "Methods for Examination of Metal Microstructures", use 3% nitric acid alcohol solution to etch the metallographic specimens of rail joints, and use a German Leica MeF3 optical microscope to observe the metallographic structure of the rail joints.
[0102] The results show that for the rail normalizing joints obtained without adopting the post-weld heat treatment construction method of the present invention, Fig. 9As shown in the figure, at 100X observation magnification, a small amount of martensite structure appeared in the heat affected zone of the rail joint. The average room temperature impact energy of the rail head weld of the air-cooled (welded state) joint after flash welding is 17J, and the average room temperature impact energy of the welds at the rail waist and rail bottom is 13J. The average hardness of the longitudinal section of the normalized joint reached 91% of the hardness of the parent material. At room temperature, the average impact energy of the rail head weld of the normalized joint is 35J, and the impact energy of the rail waist and rail bottom welds is in the range of 21J; under the low temperature test condition of -20℃, the average impact energy of the rail head weld of the normalized joint is 24J, and the average impact energy of the rail waist and rail bottom welds is 14J. Because the cooling rate (1.2℃ / s) during the heat treatment process of the rail after welding reaches the critical cooling rate of martensitic transformation of the rail steel, brittle and hard martensite is formed in the heat affected zone of the rail welding, which is not conducive to the safety of railway operation. At the same time, it also leads to a decrease in the impact toughness of the joint.
[0103] Comparative Example 4
[0104] The microstructure of the rail base material is controlled to be 94% pearlite and 6% proeutectoid ferrite. The tensile strength of the rail base material at room temperature (20-25°C) is 1050MPa, the elongation is 17.5%, the U-type impact energy of the base material rail head at room temperature is 55J, and the U-type impact energy of the rail waist and rail bottom at room temperature is 30J. The chemical composition of the rail steel to obtain the microstructure and mechanical properties must meet the following conditions: 0.56% C, 0.40% Si, 0.55% Mn, 0.20% Cr, 0.15% Cu, 0.05% Ni, 0.02% V, and the remainder is Fe and unavoidable impurities.
[0105] Using a rail mobile flash welder, the rail flash welding was carried out with a heat input of 9.5 MJ. The actual welding upset was maintained at 11.9 mm. After the rail welding was completed, when the surface temperature of the rail head dropped below 250 °C, the following method was used: Figure 4 The split-type profiling temperature control device shown heats the rail head, rail waist and rail bottom of the rail joint separately. Heating is stopped when the surface temperature of the rail head, rail waist and rail bottom of the rail joint is heated to 900℃. Subsequently, the rail joint is cooled in the field construction environment. When the surface temperature of the joint drops to 400℃, the rail joint is cooled to 200℃ at a cooling rate of 2.0℃ / s by thermal compensation of the profiling temperature control device, and then the joint is cooled to an ambient temperature of -20℃ with the field environment, thereby completing the welding and post-weld heat treatment process of the medium-carbon low-alloy rail.
[0106] according to Figure 1 The rail joints obtained in this comparative example after post-weld heat treatment were machined into Charpy U-shaped impact specimens at the sampling position shown in the figure, and the weld was located at the center of the specimen. The impact test of the rail joint impact specimens was carried out at room temperature (20-30°C) using a SANS ZBC2000 impact testing machine. Figure 2-3 The sampling method shown is to conduct metallographic inspection on the metallographic specimens of rail joints according to GB / T13298-2015 "Methods for Examination of Metal Microstructures", use 3% nitric acid alcohol solution to etch the metallographic specimens of rail joints, and use a German Leica MeF3 optical microscope to observe the metallographic structure of the rail joints.
[0107] The results show that for the rail normalizing joints obtained without adopting the post-weld heat treatment construction method of the present invention, Fig.10 As shown in the figure, at 100X observation magnification, a small amount of martensite structure appeared in the heat affected zone of the rail joint. The average room temperature impact energy of the rail head weld of the air-cooled (welded state) joint after flash welding is 17J, and the average room temperature impact energy of the welds at the rail waist and rail bottom is 13J. The average hardness of the longitudinal section of the normalized joint reached 93% of the hardness of the parent material. At room temperature, the average impact energy of the rail head weld of the normalized joint is 24J, and the impact energy of the rail waist and rail bottom welds is in the range of 16J; under the low temperature test condition of -20℃, the average impact energy of the rail head weld of the normalized joint is 14J, and the average impact energy of the rail waist and rail bottom welds is 10J. Because the cooling rate (2.0℃ / s) during the heat treatment process of the rail after welding exceeds the critical cooling rate of martensitic transformation of rail steel (1.2~1.8℃ / s), brittle and hard martensite is formed in the heat affected zone of the rail welding, which is not conducive to the safety of railway operation. At the same time, the impact toughness of the joint has also dropped significantly.
[0108] Comparative Example 5
[0109] The microstructure of the rail base material is controlled to be 99% pearlite and 1% proeutectoid ferrite. The room temperature tensile strength of the rail base material is 1200MPa, the elongation is 12.5%, the average U-type impact energy of the base material rail head at room temperature is 38J, and the average U-type impact energy of the rail waist and rail bottom at room temperature is 18J. The chemical composition of the rail steel to obtain the microstructure and mechanical properties must meet the following conditions: 0.66% C, 0.70% Si, 0.85% Mn, 0.40% Cr, 0.45% Cu, 0.25% Ni, 0.12% V, the remainder is Fe and unavoidable impurities.
[0110] Using a rail mobile flash welder, the rail flash welding was carried out with a heat input of 11.3 MJ. The actual welding upset was maintained at 12.9 mm. After the rail was welded, when the surface temperature of the rail head dropped to 200 °C, the following method was used: Figure 4The split-type profiling temperature control device shown heats the rail head, rail waist and rail bottom of the rail joint separately. Heating is stopped when the surface temperature of the rail head, rail waist and rail bottom of the rail joint is heated to 960℃. Subsequently, the rail joint is cooled in the field construction environment. When the surface temperature of the joint drops to 450℃, the rail joint is cooled to 250℃ at a cooling rate of 1.1℃ / s through thermal compensation of the profiling temperature control device, and then the joint is cooled to an ambient temperature of 0℃ with the field environment, thereby completing the welding and post-weld heat treatment process of the medium-carbon low-alloy rail.
[0111] according to Figure 1 The rail joints obtained in this comparative example after post-weld heat treatment were machined into Charpy U-shaped impact specimens at the sampling position shown in the figure, and the weld was located at the center of the specimen. The impact test of the rail joint impact specimens was carried out at room temperature (20-30°C) using a SANS ZBC2000 impact testing machine. Figure 2-3 The sampling method shown is to conduct metallographic inspection on the metallographic specimens of rail joints according to GB / T13298-2015 "Methods for Examination of Metal Microstructures", use 3% nitric acid alcohol solution to etch the metallographic specimens of rail joints, and use a German Leica MeF3 optical microscope to observe the metallographic structure of the rail joints.
[0112] The results show that the metallographic structure type of the normalized joint of the medium carbon low alloy rail obtained by the post-weld heat treatment construction method of this comparative example is Figure 6 The results are consistent, but burn holes appear in the heat affected zone. Fig.11 . At 100X observation magnification, no martensitic structure appeared in the heat affected zone of the rail joint. Among them, the weld structure is pearlite and intergranular proeutectoid ferrite, and the heat affected zone structure is pearlite and a small amount of proeutectoid ferrite. The average room temperature impact energy of the rail head weld of the obtained flash welded joint after air cooling (in welded state) is 8J, and the average room temperature impact energy of the welds at the rail waist and rail bottom is 5J. The average longitudinal section hardness of the normalized joint using this comparative example reaches 95% of the hardness of the parent material. At room temperature, the average impact energy of the rail head weld of the normalized joint reaches 18J, and the impact energy of the rail waist and rail bottom welds is in the range of 12J; under the low temperature test condition of -20℃, the average impact energy of the rail head weld of the normalized joint reaches 12J, and the impact energy of the rail waist and rail bottom welds is in the range of 6J. Due to the excessive heat input during the flash welding process, overburned holes appeared in the heat affected zone near the weld, which further caused a significant decrease in the impact performance of the rail joint, which is not conducive to the safety of railway operation.
[0113] Comparative Example 6
[0114] The microstructure of the rail base material is controlled to be 99% pearlite and 1% proeutectoid ferrite. The room temperature tensile strength of the rail base material is 1200MPa, the elongation is 12.5%, the average U-type impact energy of the base material rail head at room temperature is 38J, and the average U-type impact energy of the rail waist and rail bottom at room temperature is 18J. The chemical composition of the rail steel to obtain the microstructure and mechanical properties must meet the following conditions: 0.66% C, 0.70% Si, 0.85% Mn, 0.40% Cr, 0.45% Cu, 0.25% Ni, 0.12% V, the remainder is Fe and unavoidable impurities.
[0115] Using a rail mobile flash welder, the rail flash welding was carried out with a heat input of 11.2 MJ. The actual welding upset was maintained at 11.8 mm. After the rail was welded, when the surface temperature of the rail head dropped to 200 °C, the following method was used: Figure 4 The split-type profiling temperature control device shown heats the rail head, rail waist and rail bottom of the rail joint separately. Heating is stopped when the surface temperature of the rail head, rail waist and rail bottom of the rail joint is heated to 960℃. Subsequently, the rail joint is cooled in the field construction environment. When the surface temperature of the joint drops to 450℃, the rail joint is cooled to 250℃ at a cooling rate of 1.1℃ / s through thermal compensation of the profiling temperature control device, and then the joint is cooled to an ambient temperature of 0℃ with the field environment, thereby completing the welding and post-weld heat treatment process of the medium-carbon low-alloy rail.
[0116] according to Figure 1 The rail joints obtained in this comparative example after post-weld heat treatment were machined into Charpy U-shaped impact specimens at the sampling position shown in the figure, and the weld was located at the center of the specimen. The impact test of the rail joint impact specimens was carried out at room temperature (20-30°C) using a SANS ZBC2000 impact testing machine. Figure 2-3 The sampling method shown is to conduct metallographic inspection on the metallographic specimens of rail joints according to GB / T13298-2015 "Methods for Examination of Metal Microstructures", use 3% nitric acid alcohol solution to etch the metallographic specimens of rail joints, and use a German Leica MeF3 optical microscope to observe the metallographic structure of the rail joints.
[0117] The results show that: for the normalized joints of the medium carbon low alloy rails obtained without the post-weld heat treatment construction method of the present invention, Figure 6Completely consistent, at 100X observation magnification, no martensitic structure appears in the heat affected zone of the rail joint. Among them, the weld structure is pearlite and proeutectoid ferrite along the grain, and the heat affected zone structure is pearlite and a small amount of proeutectoid ferrite. The average room temperature impact energy of the rail head weld of the obtained flash welding joint after air cooling (in welded state) is 9J, and the average room temperature impact energy of the welds at the rail waist and rail bottom is 6J. The average longitudinal section hardness of the normalized joint using the present invention reaches 95% of the hardness of the parent material. At room temperature, the average impact energy of the rail head weld of the normalized joint reaches 24J, and the impact energy of the rail waist and rail bottom welds is in the range of 16J; under the low temperature test conditions of -20℃, the average impact energy of the rail head weld of the normalized joint reaches 18J, and the impact energy of the rail waist and rail bottom welds is in the range of 10J. Due to the low amount of upsetting during the flash welding process, the gray spot defects in the weld cannot be removed in time and remain in the weld, which in turn affects the impact performance of the rail joint, causing a significant decrease in the impact performance of the rail joint, which is not conducive to the safety of railway operation.
[0118] Comparative Example 7
[0119] The microstructure of the rail base material is controlled to be 94% pearlite and 6% proeutectoid ferrite. The tensile strength of the rail base material at room temperature (20-25°C) is 1050MPa, the elongation is 17.5%, the U-type impact energy of the base material rail head at room temperature is 55J, and the U-type impact energy of the rail waist and rail bottom at room temperature is 30J. The chemical composition of the rail steel to obtain the microstructure and mechanical properties must meet the following conditions: 0.56% C, 0.40% Si, 0.55% Mn, 0.20% Cr, 0.15% Cu, 0.05% Ni, 0.02% V, and the remainder is Fe and unavoidable impurities.
[0120] Using a rail mobile flash welder, the rail flash welding was carried out with a heat input of 9.4MJ. The actual welding upset was maintained at 11.9mm. After the rail was welded, when the surface temperature of the rail head dropped below 250℃, the following method was used: Figure 4 The split-type profiling temperature control device shown heats the rail head, rail waist and rail bottom of the rail joint separately. Heating is stopped when the surface temperature of the rail head, rail waist and rail bottom of the rail joint is heated to 900℃. Subsequently, the rail joint is cooled in the field construction environment. When the surface temperature of the joint drops to 400℃, the rail joint is cooled to 200℃ at a cooling rate of 0.5℃ / s by thermal compensation of the profiling temperature control device, and then the joint is cooled to an ambient temperature of -20℃ with the field environment, thereby completing the welding and post-weld heat treatment process of the medium-carbon low-alloy rail.
[0121] according to Figure 1The rail joints obtained in this comparative example after post-weld heat treatment were machined into Charpy U-shaped impact specimens at the sampling position shown in the figure, and the weld was located at the center of the specimen. The impact test of the rail joint impact specimens was carried out at room temperature (20-30°C) using a SANS ZBC2000 impact testing machine. Figure 2-3 The sampling method shown is to conduct metallographic inspection on the metallographic specimens of rail joints according to GB / T13298-2015 "Methods for Examination of Metal Microstructures", use 3% nitric acid alcohol solution to etch the metallographic specimens of rail joints, and use a German Leica MeF3 optical microscope to observe the metallographic structure of the rail joints.
[0122] The results show that for the medium carbon low alloy rail joints obtained without the post-weld heat treatment construction method of the present invention, Fig.12 As shown in the figure, under the observation magnification of 100X, a significant amount of martensite structure appeared in the heat affected zone of the rail joint in the welded state. The average room temperature impact energy of the rail head weld of the air-cooled (welded state) joint after flash welding is 16J, and the average room temperature impact energy of the welds at the rail waist and rail bottom is 13J. The weld structure of the normalized joint is pearlite and intergranular proeutectoid ferrite, and the heat affected zone structure is pearlite and a small amount of proeutectoid ferrite. The average hardness of the longitudinal section of the normalized joint reaches 90% of the hardness of the parent material. At room temperature, the average impact energy of the rail head weld of the normalized joint is 38J, and the average impact energy of the rail waist and rail bottom weld is 22J; under the low temperature test condition of -20℃, the average impact energy of the rail head weld of the normalized joint is 26J, and the average impact energy of the rail waist and rail bottom weld is 15J. Due to the low heat input during the flash welding process of the joint, a significant amount of martensite structure is formed in the heat affected zone of the rail welding in the field low temperature construction environment. Considering that the martensite structure is easy to form microcracks inside due to volume expansion, even if the martensite formed in the welded state is eliminated through the subsequent heat treatment process, it is not conducive to the service of the subsequent joint. Therefore, the joint obtained in this comparative example is not conducive to the safety of railway operation.
[0123] Comparative Example 8
[0124] The microstructure of the rail base material is controlled to be 96% pearlite and 3% proeutectoid ferrite. The room temperature tensile strength of the rail base material is 1100MPa, the elongation is 15%, the average U-type impact energy of the base material rail head at room temperature is 45J, and the average U-type impact energy of the rail waist and rail bottom at room temperature is 23J. The chemical composition of the rail steel to obtain the microstructure and mechanical properties must meet the following conditions: 0.60% C, 0.53% Si, 0.65% Mn, 0.30% Cr, 0.30% Cu, 0.15% Ni, 0.04% V, the remainder is Fe and unavoidable impurities.
[0125] Using a rail mobile flash welder, the rail flash welding was carried out with a heat input of 10.5 MJ. The actual welding upset was maintained at 12.4 mm. After the rail was welded, when the surface temperature of the rail head dropped below 250 °C, the following method was used: Figure 4 The split-type profiling temperature control device shown heats the rail head, rail waist and rail bottom of the rail joint separately. Heating is stopped when the surface temperature of the rail head, rail waist and rail bottom of the rail joint is heated to 800℃. Subsequently, the rail joint is cooled in the field construction environment. When the surface temperature of the joint drops to 420℃, the rail joint is cooled to 200℃ at a cooling rate of 0.8℃ / s by thermal compensation of the profiling temperature control device, and then the joint is cooled to an ambient temperature of -20℃ with the field environment, thereby completing the welding and post-weld heat treatment process of the medium-carbon low-alloy rail.
[0126] according to Figure 1 The rail joints obtained in this comparative example after post-weld heat treatment were machined into Charpy U-shaped impact specimens at the sampling position shown in the figure, and the weld was located at the center of the specimen. The impact test of the rail joint impact specimens was carried out at room temperature (20-30°C) using a SANS ZBC2000 impact testing machine. Figure 2-3 The sampling method shown is to conduct metallographic inspection on the metallographic specimens of rail joints according to GB / T13298-2015 "Methods for Examination of Metal Microstructures", use 3% nitric acid alcohol solution to etch the metallographic specimens of rail joints, and use a German Leica MeF3 optical microscope to observe the metallographic structure of the rail joints.
[0127] The results show that the metallographic structure of the normalized joint of the medium carbon low alloy rail obtained by the post-weld heat treatment construction method of this comparative example is Figure 6 Consistent. At 100X observation magnification, no martensitic structure appeared in the heat affected zone of the rail joint. Among them, the weld structure is pearlite and intergranular proeutectoid ferrite, and the heat affected zone structure is pearlite and a small amount of proeutectoid ferrite. The average room temperature impact energy of the rail head weld of the obtained flash welding joint after air cooling (in welded state) is 14J, and the average room temperature impact energy of the welds at the rail waist and rail bottom is 11J. The average longitudinal section hardness of the normalized joint using this comparative example reaches 90% of the hardness of the parent material. At room temperature, the average impact energy of the rail head weld of the normalized joint reaches 18J, and the impact energy of the rail waist and rail bottom welds is in the range of 14J; under the low temperature test conditions of -20℃, the average impact energy of the rail head weld of the normalized joint reaches 13J, and the impact energy of the rail waist and rail bottom welds is in the range of 8J. Due to the low heating temperature during the post-weld heat treatment of the joint, the austenitization process of the joint is incomplete, and the mechanical properties of the normalized rail joint are not significantly improved compared to the welded joint. That is, the rail joint heat treated at the normalizing temperature (800℃) is not conducive to the safety of railway operation.
[0128] By comparing Examples 1-4 and Comparative Examples 1-8, it can be seen that the welding process provided by the present invention can effectively reduce the probability of welding gray spots and avoid the appearance of martensitic structure in the heat-affected zone of the rail joint. The welding method of the present invention can avoid the appearance of harmful martensitic structure in the heat-affected zone of the joint. The average hardness of the normalized rail joint at room temperature (20-30°C) reaches 90-95% of the hardness of the parent material. At room temperature, the average impact energy of the normalized joint rail head weld reaches 28-40J, and the impact energy of the rail waist and rail bottom welds ranges from 16-25J; under the low temperature test condition of -20°C, the average impact energy of the normalized joint rail head weld reaches 20-32J, and the impact energy of the rail waist and rail bottom welds ranges from 10-18J, which helps to ensure the safety of railway operation.
[0129] The above embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention.
Claims
1. A method for post-weld heat treatment of medium-carbon low-alloy rails for outdoor low-temperature environments, characterized in that: include: S1: placing the welded rail joint in a contoured temperature control device for a first cooling treatment by a thermal compensation method, cooling the rail joint to 200-300° C., wherein the cooling rate during the first cooling treatment is 0.5-1.1° C. / s; S2: performing full-section heating treatment on the rail joint in the profiling temperature control device to heat the rail joint to 900-960° C., and controlling the heating of the rail head, rail waist and rail bottom of the rail joint respectively during the heating treatment; S3: removing the contour temperature control device, placing the rail joint in a low-temperature outdoor environment for a second cooling treatment, and naturally cooling it to 400-450° C.; S4: placing the rail joint in the profiling temperature control device for a third cooling treatment by means of thermal compensation, cooling the rail joint to 200-250° C., wherein the cooling rate during the third cooling treatment is 0.5-1.1° C. / s; S5: removing the contour temperature control device, placing the rail joint in a field low temperature environment for a fourth cooling treatment, and naturally cooling it to ambient temperature, wherein the field low temperature environment is -20 to 0°C.
2. The post-weld heat treatment construction method for medium-carbon low-alloy rails used in outdoor low-temperature environments according to claim 1 is characterized in that: During the heating treatment, the heating temperature of the rail waist and rail bottom of the profiling temperature control device is set to be 20-40° C. higher than the heating temperature of the rail head.
3. The post-weld heat treatment construction method for medium-carbon low-alloy rails used in outdoor low-temperature environments according to claim 1 is characterized in that: The rail joint is welded by mobile flash welding, the upsetting amount is maintained at 11.9-12.9 mm during welding, and the heat input amount is 9.5-11.2 MJ during welding.
4. The post-weld heat treatment construction method for medium-carbon low-alloy rails used in outdoor low-temperature environments according to claim 1 is characterized in that: The contour-like temperature control device is a split-type contour-like temperature control device, and temperature control is achieved by arranging a plurality of ceramic electric heating sheets in the split-type contour-like temperature control device.
5. The post-weld heat treatment construction method for medium-carbon low-alloy rails used in outdoor low-temperature environments according to claim 1 is characterized in that: The cooling rate during the second cooling treatment is 4.0 to 15.0° C. / s.
6. The post-weld heat treatment construction method for medium-carbon low-alloy rails used in outdoor low-temperature environments according to claim 1 is characterized in that: The microstructure of the rail base material of the medium-carbon low-alloy rail includes 94-99% pearlite and 1-6% proeutectoid ferrite. In terms of weight percentage, the rail base material contains: 0.56-0.66% C, 0.40-0.70% Si, 0.55-0.8% Mn, 0.20-0.40% Cr, 0.15-0.45% Cu, 0.05-0.25% Ni, 0.02-0.12% V, and the balance is Fe and unavoidable impurities.
7. The post-weld heat treatment construction method for medium-carbon low-alloy rails used in outdoor low-temperature environments according to claim 6 is characterized in that: The tensile strength of the rail base material at room temperature (20-30°C) is 1050-1200MPa, the elongation is 12.5-17.5%, the room temperature U-shaped impact energy of the rail head of the rail base material is 38-55J, the room temperature U-shaped impact energy of the rail waist and the rail bottom is in the range of 18-30J, the room temperature impact energy of the rail head weld of the rail joint after welding is in the range of 10-17J, and the room temperature impact energy of the rail waist and rail bottom weld is in the range of 8-13J.
8. A medium-carbon low-alloy rail joint for use in a field low-temperature environment, the rail joint being formed by processing using the method according to any one of the above claims.