A method for preparing hexamethylenediamine by hydrogenating 6-aminocapronitrile
Hexadiene is prepared by directly hydrogenating the hydrotreating method using porous molecular sieve-supported copper-nickel-based catalyst in 6-aminocapronitrile catalytic hydrogenation, which solves the problems of alkali liquid pollution and equipment corrosion in the existing processes, and achieves high efficiency and low cost industrial production, and the catalyst has a long service life.
Patent Information
- Application Number
- CN202211192204.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-09-28
AI Technical Summary
The existing 6-aminocapronitrile catalytic hydrogenation process requires the addition of alkali or ammonia water to prepare hexanediamine, which leads to environmental pollution, equipment corrosion and catalyst recovery difficulties, high production costs, and is not suitable for industrial production.
Using porous molecular sieve-supported copper-nickel-based catalyst, the hydrogen-activated catalyst is used to perform batch kettle-type or fixed-bed reactions through hydrogen-activated catalysts, and directly hydrogenate to prepare hexanediamine, simplify the process, improve the service life and production of the catalyst. efficiency.
The production of high-purity hexanediamine is achieved, which reduces production costs and environmental impacts, is suitable for large-scale industrial production, has low catalyst costs and a long service life.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic chemical industry, and specifically relates to a method for preparing hexamethylenediamine by hydrogenating 6-aminocapronitrile. Background Art
[0002] Hexamethylenediamine is an important chemical raw material. The main use of hexamethylenediamine is to synthesize important industrial products such as nylon 66 and nylon 610, and then make various nylon resins, nylon fibers and polyamide resin inks and other important civilian materials. In addition, hexamethylenediamine is also widely used in mineral oil field demulsifiers, agricultural pesticides, building concrete additives, etc. In addition, hexamethylenediamine can react with carbon phthalate to prepare 6-aminocapronitrile isocyanate, and then continue to polymerize to produce polyurethane materials, which are widely used in the aerospace field. The application scope of hexamethylenediamine is constantly expanding, and the demand for downstream products is increasing, so realizing large-scale industrial production of hexamethylenediamine is now the primary task.
[0003] At present, the production process of hexamethylenediamine mainly includes caprolactam method, butadiene method and adiponitrile catalytic hydrogenation method. The adiponitrile catalytic hydrogenation method for preparing hexamethylenediamine is widely used because of its simple process, high product quality and low production cost. The industrial production method of hexamethylenediamine is mainly adiponitrile catalytic hydrogenation method. 6-aminocapronitrile is an important chemical intermediate, but in the production process of preparing hexamethylenediamine by 6-aminocapronitrile catalytic hydrogenation method, alkali or ammonia water needs to be added to suppress the generation of secondary amine and tertiary amine to improve the selectivity of hexamethylenediamine, so as to maintain the activity and selectivity of the catalyst. A large amount of alkali liquid is discharged in the preparation process, which pollutes the environment, and the alkali or ammonia water corrodes the equipment seriously, and the catalyst is difficult to recover, which reduces the service life of the catalyst. The production cost is too high and is not suitable for industrial production. Therefore, it is of great significance to develop a green synthesis process of hexamethylenediamine. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a method for preparing hexamethylenediamine by hydrogenating 6-aminocapronitrile. Under the condition of no need to add alkali or ammonia water, 6-aminocapronitrile is used as a raw material and hexamethylenediamine is directly hydrogenated to prepare hexamethylenediamine. The production process is simple, the process safety is high, the service life of the catalyst is improved, the production cost is low, the reaction conversion rate and yield are high, the hexamethylenediamine has high purity, and is suitable for large-scale production.
[0005] The present invention solves the above technical problems through the following technical solutions.
[0006] A method for preparing hexamethylenediamine by hydrogenating 6-aminocapronitrile comprises the following steps:
[0007] Add 6-aminocapronitrile solution into a reactor, activate the catalyst with hydrogen, transfer the activated catalyst into the reactor under nitrogen protection, seal the reactor, replace the air in the reactor with hydrogen, pressurize it to 1.5-8.0Mpa, and then stir to react; after the reaction is completed, cool to room temperature, take the reaction mixture, and obtain hexamethylenediamine after reduced pressure distillation;
[0008] The catalyst is a copper-nickel based catalyst supported by a porous molecular sieve.
[0009] Preferably, the solvent of the 6-aminocapronitrile solution is ethanol, methanol or water, and the mass concentration of the 6-aminocapronitrile is 5-75%.
[0010] Preferably, the added amount of the catalyst is 1-5% of the total mass of the 6-aminocapronitrile solution.
[0011] Preferably, the reaction is an intermittent reaction or a fixed bed reaction; in the intermittent reaction or the fixed bed reaction, the catalyst activation temperature is 300-450°C, and the activation hydrogen space velocity is 2000-3500h -1 , activation time 5-10h; intermittent reaction temperature 120-500℃; fixed bed reaction temperature 120-500℃, reaction space velocity 0.3-3h -1 .
[0012] Preferably, the content of copper oxide and nickel oxide in the catalyst is 15-55% of the total mass of the catalyst, and the mass ratio of copper oxide to nickel oxide in the catalyst is 1:1-1.5.
[0013] Preferably, the porous molecular sieve is ZSM-5 or MCM-41, with a pore size of 1-10 nm, and the content of the porous molecular sieve is 25-65% of the total mass of the catalyst.
[0014] Preferably, the porous molecular sieve is also loaded with a transition metal oxide, the content of the transition metal oxide is 15-45% of the total mass of the catalyst, and the transition metal oxide is one or more of manganese oxide, cobalt oxide, and zinc oxide.
[0015] Preferably, the porous molecular sieve-supported copper-nickel based catalyst is prepared by coprecipitation method, comprising the following steps:
[0016] S1. dissolving nickel nitrate, copper nitrate and transition metal oxide in water to prepare a mixed solution;
[0017] S2. Place the molecular sieve in a reactor, add water to mix, then drop the precipitant and the mixed solution obtained in S1 into the reactor at the same time, stir to react, adjust the pH of the mixture to 8 after the dropwise addition, and then perform an aging reaction. After the aging reaction, filter, wash, and dry to obtain a precipitate, which is then calcined to obtain a catalyst.
[0018] Preferably, in S1, the metal ion concentration in the mixed solution is 0.5-2.5 mol / L.
[0019] Preferably, in S2, the molar ratio of the precipitant to the metal ions in the mixed solution is 1-3:1, and the precipitant is ammonia water, sodium carbonate solution or sodium bicarbonate solution with a pH of 11;
[0020] The reaction temperature is 35-55°C; the aging reaction time is 3-8h, and the temperature is 35-55°C; the calcination temperature is 250-750°C, and the time is 2.5-5.5h.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention uses 6-aminocapronitrile as a raw material and directly hydrogenates hexamethylenediamine without adding alkali or ammonia water, thereby reducing the impact of alkali solution on the environment and equipment during the preparation of hexamethylenediamine. The production process is simple, the process safety is high, the production cost is low, the reaction conversion rate and yield are high, the hexamethylenediamine is high in purity, there is no three wastes discharged, the equipment investment is low, and it is suitable for large-scale production.
[0023] 2. The present invention adopts a copper-nickel-based catalyst supported by a porous molecular sieve for the reaction of hydrogenating 6-aminocapronitrile to synthesize hexamethylenediamine. Compared with the preparation of a Raney nickel catalyst, the catalyst cost is low, and the components have different chemical potentials. Under the action of the catalyst, the components exist in the form of ions in the solution and can be mixed in a more orderly manner, with good stability, simple production process and low production cost.
[0024] 3. The porous molecular sieve-supported copper-nickel-based catalyst prepared by the present invention can reduce copper at low temperatures, and the reduced copper can activate hydrogen atoms to help reduce nickel oxide, thereby reducing the reduction temperature of nickel. At the same time, the addition of transition metals improves the dispersion of metal copper and nickel, promotes the synergistic effect between copper and nickel, and improves the overall hydrogenation effect of the catalyst. The supported metal copper-nickel catalyst used is cheap, easy to obtain, and has a long service life. The catalyst after reduction and regeneration still maintains a higher reaction activity than the fresh catalyst. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] It should be noted that the professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, the various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.
[0027] Example 1
[0028] The catalyst NiCuCo / MCM-41 prepared by coprecipitation method comprises the following steps:
[0029] S1, dissolving copper nitrate, nickel nitrate and cobalt nitrate in a molar ratio of 2:2:1 in deionized water to prepare a mixed solution with a metal ion concentration of about 1 mol / L;
[0030] S2, dissolving anhydrous sodium carbonate in water to prepare an anhydrous sodium carbonate solution with a pH of 11, and simultaneously dropping the anhydrous sodium carbonate solution and the mixed solution obtained in S1 into a 250mL three-necked flask containing 5-10mL deionized water and 50% MCM-41 molecular sieves of the total mass of the catalyst for reaction, the dripping rate is 1mL / min, and the molar ratio of anhydrous sodium carbonate to metal ions in the anhydrous sodium carbonate solution is 1:1.2; the reaction temperature is 45°C, and the stirring is vigorous, and precipitation will gradually appear at this time. After the addition is completed, the pH of the test mixture is 6-7, and the pH of the mixture is adjusted to 8 with sodium carbonate solution;
[0031] Then, an aging reaction was carried out for 6 hours, and a constant temperature of 50°C and vigorous stirring were maintained. After the aging reaction, suction filtration was carried out, and the precipitate was first washed with more than 400 mL of 75°C deionized water until the washing liquid was neutral, and then washed with more than 100 mL of methanol at room temperature in order to remove the sodium ions in the precipitate as much as possible. The precipitate was then placed in an electric blast drying oven and dried at 110°C for 12 hours to obtain a precipitate. After the precipitate was cooled to room temperature, it was ground into a powder without a particle feel with a mortar, and then calcined at 450°C for 4 hours to obtain a NiCuCo / / MCM-41 catalyst.
[0032] Example 2
[0033] The catalyst NiCuZn / MCM-41 prepared by coprecipitation method comprises the following steps:
[0034] S1. Weigh nickel nitrate, aluminum nitrate and zinc nitrate in a molar ratio of 2:2:1 and dissolve them in deionized water to prepare a mixed solution with an aluminum ion concentration of 2 mol / L;
[0035] S2, dissolving anhydrous sodium carbonate in water to prepare an anhydrous sodium carbonate solution with a pH of 11, and simultaneously dropping the anhydrous sodium carbonate solution and the mixed solution obtained in S1 into a 250mL three-necked flask containing 5-10mL deionized water and 50% MCM-41 molecular sieves of the total mass of the catalyst for reaction, the dripping rate is 1mL / min, and the molar ratio of anhydrous sodium carbonate to metal ions in the anhydrous sodium carbonate solution is 1:1.2; the reaction temperature is 45°C, and the stirring is vigorous, and precipitation will gradually appear at this time. After the addition is completed, the pH of the test mixture is 6-7, and the pH of the mixture is adjusted to 8 with sodium carbonate solution;
[0036] Then, an aging reaction was carried out for 6 hours, and a constant temperature of 50°C and vigorous stirring were maintained. After the aging reaction, suction filtration was carried out, and the precipitate was first washed with more than 400 mL of 75°C deionized water until the washing liquid was neutral, and then washed with more than 100 mL of methanol at room temperature in order to remove the sodium ions in the precipitate as much as possible. The precipitate was then placed in an electric blast drying oven and dried at 110°C for 12 hours to obtain a precipitate. After the precipitate was cooled to room temperature, it was ground into a powder without a particle feel with a mortar, and then calcined at 350°C for 4.5 hours to obtain a NiCuZn / MCM-41 catalyst.
[0037] The pore structure properties of the catalysts in Examples 1-2 were calculated using the BET method. The specific surface areas of the NiCuCo / / MCM-41 and NiCuZn / MCM-41 catalysts prepared in Examples 1-2 were in the range of 230-340 m 2 / g, the pore volume and pore diameter are between 0.65-1.43cm 3 / g and between 4.2-5.7nm.
[0038] Example 3
[0039] A method for preparing hexamethylenediamine by hydrogenating 6-aminocapronitrile comprises the following steps:
[0040] A 30% mass fraction of 6-aminocapronitrile ethanol solution was added to an intermittent reactor, and 20 g (about 25 mL) of the NiCuCo / MCM-41 catalyst prepared in Example 1 was heated and activated with hydrogen on a fixed bed. The catalyst activation temperature was 320° C. and the activation hydrogen space velocity was 2200 h / min. -1, activation time 8h; then transferred to an intermittent kettle reactor under nitrogen protection, sealed, replaced the air in the kettle with hydrogen, set the reaction temperature of the reactor to 220℃, filled with hydrogen to the set reaction pressure of 6MPa; when the reaction temperature reaches 220℃, start stirring and start timing, the stirring speed is maintained at 600r / min, after 4h of reaction, turn off the stirring and heating device, cool the reactor to room temperature, release the pressure to normal pressure, take the reaction mixture, the conversion rate is 97% according to chromatographic analysis, and the selectivity of hexamethylenediamine is 99.5%. After vacuum distillation and refining, high-purity hexamethylenediamine is obtained.
[0041] Example 4
[0042] A method for preparing hexamethylenediamine by hydrogenating 6-aminocapronitrile comprises the following steps:
[0043] A 5% 6-aminocapronitrile ethanol solution was added to an intermittent reactor, and 20 g (about 25 mL) of the NiCuCo / MCM-41 catalyst prepared in Example 1 was heated and activated with hydrogen on a fixed bed. The catalyst activation temperature was 320° C. and the activation hydrogen space velocity was 2200 h / min. -1 , activation time 8h; then transferred to an intermittent reactor under nitrogen protection, sealed, replaced the air in the reactor with hydrogen, set the reaction temperature of the reactor to 220℃, filled with hydrogen to the set reaction pressure of 6MPa; when the reaction temperature reaches 220℃, start stirring and start timing, keep the stirring speed at 600r / min, after 4h of reaction, turn off the stirring and heating device, cool the reactor to room temperature, release the pressure to normal pressure, take the reaction mixture, the conversion rate is 98% according to chromatographic analysis, and the selectivity of hexamethylenediamine is 99.5%. After vacuum distillation and refining, high-purity hexamethylenediamine is obtained.
[0044] Example 5
[0045] A method for preparing hexamethylenediamine by hydrogenating 6-aminocapronitrile comprises the following steps:
[0046] A 75% mass fraction of 6-aminocapronitrile ethanol solution was added to an intermittent reactor, and 20 g (about 25 mL) of the NiCuZn / MCM-41 catalyst prepared in Example 2 was heated and activated with hydrogen on a fixed bed. The catalyst activation temperature was 320° C. and the activation hydrogen space velocity was 2200 h / min. -1, activation time 8h; then transferred to an intermittent reactor under nitrogen protection, sealed, replaced the air in the reactor with hydrogen, set the reaction temperature of the reactor to 240℃, filled with hydrogen to the set reaction pressure of 6MPa; when the reaction temperature reaches 240℃, start stirring and start timing, keep the stirring speed at 600r / min, react for 4h, turn off the stirring and heating device, cool the reactor to room temperature, release the pressure to normal pressure, take the reaction mixture, the conversion rate is 98% according to chromatographic analysis, and the selectivity of hexamethylenediamine is 99.5%. High-purity hexamethylenediamine is obtained after vacuum distillation and refining.
[0047] Example 6
[0048] 20 g (about 24 ml) of the NiCuCo / MCM-41 catalyst prepared in Example 1 was loaded into a fixed bed reactor. The catalyst was activated with hydrogen at 320°C. The temperature was programmed to reach the activation temperature from room temperature for 1 h. The activation hydrogen hourly velocity was 2200 h -1 , activated for 8h; after the catalyst was activated, the bed temperature dropped to the reaction temperature of 220℃, the system pressure was increased to 6MPa, and a 20% mass fraction of 6-aminocapronitrile ethanol solution was pumped into the reaction system at an air velocity of 1h -1 The reaction mixture was taken, and the conversion rate was 98% and the selectivity of hexamethylenediamine was 99.5% after chromatographic analysis. High-purity hexamethylenediamine was obtained after vacuum distillation and purification.
[0049] Comparative Example 1
[0050] The method for preparing hexamethylenediamine by hydrogenation of 6-aminocapronitrile is the same as that in Example 1, except that a Raney nickel catalyst is used as the catalyst. The reaction mixture is taken, and the conversion rate is 92% and the selectivity of hexamethylenediamine is 95.3% after chromatographic analysis. High-purity hexamethylenediamine is obtained after refining by vacuum distillation.
[0051] In summary, the present invention uses 6-aminocapronitrile as a raw material and adopts a supported metal nickel catalyst for the reaction of hydrogenating 6-aminocapronitrile to synthesize hexamethylenediamine without adding alkali or ammonia water, and directly hydrogenates to prepare hexamethylenediamine. The production process is simple, the process safety is high, the production cost is low, the reaction conversion rate and yield are high, the hexamethylenediamine has high purity, no three wastes are discharged, the equipment investment is low, and it is suitable for large-scale production. Compared with the preparation of the Raney nickel catalyst, the catalyst cost of the method is low, and the components have different chemical potentials. Under the action of the Raney nickel catalyst, the components exist in the form of ions in the solution and can be mixed in a more orderly manner. The supported metal copper-nickel catalyst used is cheap, easy to obtain and has a long service life. Compared with the fresh catalyst, the catalyst after reduction and regeneration still maintains a higher reaction activity.
[0052] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundancy, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they know the basic creative concept. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0053] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for preparing hexamethylenediamine by hydrogenating 6-aminocapronitrile, It is characterized in that The following steps are involved: Add 6-aminocapronitrile solution into a reactor, activate the catalyst with hydrogen, transfer the activated catalyst into the reactor under nitrogen protection, seal the reactor, replace the air in the reactor with hydrogen, pressurize it to 1.5-8.0Mpa, and then stir to react; after the reaction is completed, cool to room temperature, take the reaction mixture, and obtain hexamethylenediamine after reduced pressure distillation; The catalyst is a copper-nickel based catalyst supported by a porous molecular sieve; The content of copper oxide and nickel oxide in the catalyst is 15-55% of the total mass of the catalyst, and the mass ratio of copper oxide to nickel oxide in the catalyst is 1:1-1.5; The porous molecular sieve is ZSM-5 or MCM-41, with a pore size of 1-10 nm, and the content of the porous molecular sieve is 25-65% of the total mass of the catalyst; The porous molecular sieve is also loaded with transition metal oxide, the content of which is 15-45% of the total mass of the catalyst, and the transition metal oxide is cobalt oxide or zinc oxide.
2. The method for preparing hexamethylenediamine by hydrogenating 6-aminocapronitrile according to claim 1, It is characterized in that The solvent of the 6-aminocapronitrile solution is ethanol, methanol or water, and the mass concentration of the 6-aminocapronitrile is 5-75%.
3. The method for preparing hexamethylenediamine by hydrogenating 6-aminocapronitrile according to claim 1, It is characterized in that The added amount of the catalyst is 1-5% of the total mass of the 6-aminocapronitrile solution.
4. The method for preparing hexamethylenediamine by hydrogenating 6-aminocapronitrile according to claim 1, It is characterized in that The reaction is an intermittent reaction or a fixed bed reaction; in the intermittent reaction or the fixed bed reaction, the catalyst activation temperature is 300-450°C, and the activation hydrogen space velocity is 2000-3500h -1 , activation time 5-10h; intermittent reaction temperature 120-500℃; fixed bed reaction temperature 120-500℃, reaction space velocity 0.3-3h -1 .
5. The method for preparing hexamethylenediamine by hydrogenating 6-aminocapronitrile according to claim 1, It is characterized in that The method of preparing a porous molecular sieve-supported copper-nickel based catalyst by a coprecipitation method comprises the following steps: S1. dissolving nickel nitrate, copper nitrate and transition metal oxide in water to prepare a mixed solution; S2. Place the molecular sieve in a reactor, add water to mix, then drop the precipitant and the mixed solution obtained in S1 into the reactor at the same time, stir to react, adjust the pH of the mixture to 8 after the dropwise addition, and then perform an aging reaction. After the aging reaction, filter, wash, and dry to obtain a precipitate, which is then calcined to obtain a catalyst.
6. The method for preparing hexamethylenediamine by hydrogenating 6-aminocapronitrile according to claim 5, It is characterized in that In S1, the metal ion concentration in the mixed solution is 0.5-2.5 mol / L.
7. The method for preparing hexamethylenediamine by hydrogenating 6-aminocapronitrile according to claim 5, It is characterized in that In S2, the molar ratio of the precipitant to the metal ions in the mixed solution is 1-3:1, and the precipitant is ammonia water, sodium carbonate solution or sodium bicarbonate solution with a pH of 11; The reaction temperature is 35-55°C; the aging reaction time is 3-8h, and the temperature is 35-55°C; the calcination temperature is 250-750°C, and the time is 2.5-5.5h.