Thermosetting adhesive film and cover film comprising the same

By using epoxy resin, thermoset acrylic rubber and phosphorus-based flame retardant in flexible printed circuit boards, the problems of ion migration and high dielectric constant in the adhesive are solved, and efficient signal transmission and Improved mechanical performance.

CN115803405BActive Publication Date: 2024-11-12HANWHA YISHENSHA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280005450.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-01-26
Filing Date
2022-01-25
Publication Date
2024-11-12
Estimated Expiration
2042-01-25

AI Technical Summary

Technical Problem

Existing adhesives cannot effectively prevent ion migration in flexible printed circuit boards, and at the same time, high dielectric constant leads to signal transmission delays, making it difficult to develop adhesives that can delay ion migration and have low dielectric constants.

Method used

An epoxy resin and thermosetting acrylic rubber which are solid at a temperature of 15°C to 28°C, combined with a phosphorus flame retardant, was prepared to prepare a thermosetting adhesive film with excellent ion mobility, low dielectric constant and high peel strength.

Benefits of technology

It effectively suppresses ion migration at high temperatures, reduces dielectric constant, improves signal transmission speed, and maintains excellent peel strength and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115803405B_ABST
    Figure CN115803405B_ABST
Patent Text Reader

Abstract

The present invention relates to a thermosetting adhesive film and a cover film including the same, and more particularly to a thermosetting adhesive film having excellent resistance to ion migration, a low dielectric constant and excellent peel strength and a cover film including the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a thermosetting adhesive film and a cover film including the same, and more particularly to a thermosetting adhesive film having excellent resistance to ion migration, a low dielectric constant and excellent peel strength and a cover film including the same. Background Art

[0002] Recently, due to the trend of miniaturization, lightweight, thin film and integration in the electronic industry, the use of flexible printed circuits (FPCB) has increased and the development of technology has also accelerated.

[0003] However, adhesive technologies for cover films, adhesive sheets, and metal laminates do not adapt to the rapid technological developments of electronics manufacturers and flexible circuit board manufacturers, such as the realization of large-capacity high-speed transmission and micro-fine circuits.

[0004] A representative example is the ion migration phenomenon.

[0005] The ion migration phenomenon is a phenomenon that occurs in adhesives used in cover films, adhesive sheets, and metal laminates, and occurs when a dielectric or moisture is present or a voltage is applied between conductors.

[0006] In a general flexible printed circuit board, an adhesive is used as a medium, and the ion migration phenomenon is accelerated due to ion residues and moisture contained in the adhesive.

[0007] In the prior art, adhesive compositions applied to coverlay films, adhesive sheets, and metal laminates can maintain high resistance to solder bath heat and stable peel strength, etc., but cannot prevent the ion migration phenomenon.

[0008] Even in the case of advanced technology in Japan and other countries, the only way to delay ion migration is to increase the purity of nitrile rubber. In this case, although the ion migration phenomenon can be partially suppressed and delayed by removing impurities in the rubber, this is not a complete solution, and there is also the problem that the cost of raw materials has increased by more than 10 times compared to the past, and it cannot cope with the problem of discoloration at high temperatures.

[0009] On the other hand, since the data transmission speed of the 5G generation is expected to be faster than that of 4G mobile communications, it is necessary to develop materials that correspond to higher speeds and higher frequencies to meet the requirements for higher performance and higher functionality of information and communication equipment. Therefore, if the dielectric constant of the adhesive constituting the cover film, adhesive sheet, and metal laminate used in digital home appliances such as mobile phones, digital cameras, notebook computers, and liquid crystal displays is large, signal transmission will be delayed, resulting in a delay in transmission speed, so materials with low dielectric constants should be used.

[0010] However, among adhesives used for cover films, adhesive sheets, and metal laminates, it is difficult to develop an adhesive that can retard ion migration and has a low dielectric constant. Summary of the invention

[0011] Technical issues

[0012] The present invention is developed to solve the above problems, and an object of the present invention is to provide a thermosetting adhesive film having excellent resistance to ion migration, low dielectric constant and good peel strength.

[0013] Furthermore, by using the thermosetting adhesive film of the present invention, it is possible to provide a cover film, a bonding sheet, or a metal laminate that is excellent in resistance to ion migration and has a low dielectric constant.

[0014] Solutions to the problem

[0015] In order to solve the above technical problems, the thermosetting adhesive film of the present invention includes an epoxy resin that is solid at a temperature of 15° C. to 28° C., a thermosetting acrylic rubber that is solid at a temperature of 15° C. to 28° C., and a phosphorus-based flame retardant.

[0016] In a preferred embodiment of the present invention, the thermosetting acrylic rubber may include a hydroxyl group and a carboxyl group as functional groups.

[0017] In a preferred embodiment of the present invention, the weight average molecular weight (Mw) of the thermosetting acrylic rubber may be 400,000 to 1,500,000.

[0018] In a preferred embodiment of the present invention, the glass transition temperature (Tg) of the thermosetting acrylic rubber may be -10°C to 15°C.

[0019] In a preferred embodiment of the present invention, the thermosetting adhesive film of the present invention may satisfy condition (1).

[0020] (1) A ≥ 100 MΩ

[0021] In the above condition (1), A is the insulation resistance measured under the conditions of 85° C., 85% relative humidity and 50 V DC voltage for 500 to 1000 hours according to the IPC-TM 650 test standard.

[0022] In a preferred embodiment of the present invention, the thermosetting adhesive film of the present invention may satisfy condition (2).

[0023] (2) B1≤3.3, B2≤3.1

[0024] In the above condition (2), B1 represents a dielectric constant at 1 GHz, and B2 represents a dielectric constant at 10 GHz.

[0025] In a preferred embodiment of the present invention, the thermosetting adhesive film of the present invention may satisfy condition (3).

[0026] (3) C ≥ 0.7 kgf / cm

[0027] In the above condition (3), C represents the peel strength measured when peeling at a speed of 50 mm / min and a peeling direction of 90°.

[0028] In a preferred embodiment of the present invention, the thermosetting adhesive film of the present invention may satisfy condition (4).

[0029] (4) D≤0.5%

[0030] In the above condition (4), D represents moisture absorption measured according to the following relational expression 1 according to the IPC TM-650 test standard.

[0031] [Equation 1]

[0032] Moisture absorption rate (%) = (D1-D0) / D0×100

[0033] In the above-mentioned Relational Formula 1, D0 represents the weight of the dry thermosetting adhesive film, and D1 represents the weight of the dry thermosetting adhesive film after immersing it in distilled water for 24 hours.

[0034] In a preferred embodiment of the present invention, the thermosetting adhesive film of the present invention may satisfy condition (5).

[0035] (5)65℃≤E≤85℃

[0036] In the above condition (5), E represents the glass transition temperature.

[0037] In a preferred embodiment of the present invention, the thermosetting adhesive film of the present invention may satisfy condition (6).

[0038] (6)65ppm / ℃≤F1≤95ppm / ℃, 200ppm / ℃≤F2≤280ppm / ℃

[0039] In the above condition (6), F1 represents the thermal expansion coefficient before reaching the glass transition temperature when the temperature is increased at a rate of 10°C / min, and F2 represents the thermal expansion coefficient after reaching the glass transition temperature when the temperature is increased at a rate of 10°C / min.

[0040] In a preferred embodiment of the present invention, the thermosetting adhesive film of the present invention may satisfy condition (7).

[0041] (7)20MPa≤G≤50MPa

[0042] In the above condition (7), G represents the tensile strength measured according to the IPC TM-650 test standard.

[0043] In a preferred embodiment of the present invention, the thermosetting adhesive film of the present invention may satisfy condition (8).

[0044] (8)0.3GPa≤H≤1.0GPa

[0045] In the above condition (8), H represents Young's modulus measured according to the IPC TM-650 test standard.

[0046] In a preferred embodiment of the present invention, the thermosetting adhesive film of the present invention may satisfy condition (9).

[0047] (9) 30% ≤ I ≤ 130%

[0048] In the above condition (9), I represents the elongation measured according to the IPC TM-650 test standard.

[0049] In a preferred embodiment of the present invention, the epoxy resin may include at least two selected from bisphenol-A type epoxy resin, o-cresol novolac type epoxy resin, phenol novolac type epoxy resin, low-chlorine type epoxy resin, dicycolpentadiene type epoxy resin, biphenyl type epoxy resin and multi-functional novolac type epoxy resin.

[0050] In a preferred embodiment of the present invention, the epoxy resin may have a softening point of 60° C. to 80° C. and an epoxy equivalent weight of 200 g / eq to 350 g / eq.

[0051] In a preferred embodiment of the present invention, the thermosetting acrylic rubber may be a polymer obtained by polymerizing a monomer mixture, wherein the monomer mixture includes at least three selected from the group consisting of butyl acrylate monomer, 2-ethylhexyl acrylate monomer, 2-methoxyethyl acrylate monomer, 4-hydroxybutyl acrylate monomer, ethyl acrylate monomer, 2-hydroxyethyl acrylate monomer, 2-hydroxypropyl acrylate monomer, pentylmethacrylate monomer, 2-hydroxymethyl acrylate monomer, ethylmethacrylate monomer, methylmethacrylate monomer, acrylic acid monomer, and acrylonitrile monomer.

[0052] In a preferred embodiment of the present invention, the thermosetting acrylic rubber may have an acid value of 30 to 45 and a viscosity of 500 cps to 8,000 cps.

[0053] In a preferred embodiment of the present invention, the phosphorus-based flame retardant may include at least one selected from the group consisting of a phosphate-based flame retardant, a phosphazene-based flame retardant, and a phosphinate-based flame retardant.

[0054] In a preferred embodiment of the present invention, the thermosetting adhesive film of the present invention may include 120 to 180 parts by weight of epoxy resin and 10 to 40 parts by weight of phosphorus-based flame retardant relative to 100 parts by weight of thermosetting acrylic rubber.

[0055] In a preferred embodiment of the present invention, the thermosetting adhesive film of the present invention may further include at least one selected from a curing agent and an inorganic filler.

[0056] In a preferred embodiment of the present invention, the thermosetting adhesive film of the present invention may include 8 to 18 parts by weight of a curing agent and 20 to 40 parts by weight of an inorganic filler relative to 100 parts by weight of the thermosetting acrylic rubber.

[0057] In a preferred embodiment of the present invention, the curing agent may include at least one selected from an amine curing agent, an imidazole curing agent and an acid anhydride curing agent.

[0058] In a preferred embodiment of the present invention, the inorganic filler may include at least one selected from aluminum hydroxide, magnesium hydroxide, silicon dioxide, aluminum oxide, zinc oxide, magnesium oxide, zirconium oxide, titanium oxide, iron oxide, cobalt oxide and chromium oxide.

[0059] On the other hand, the cover film of the present invention may include: an electrically insulating substrate; the thermosetting adhesive film of the present invention formed on one side of the electrically insulating substrate; and a release film formed on one side of the thermosetting adhesive film.

[0060] Effects of the Invention

[0061] The thermosetting adhesive film and the cover film including the same of the present invention have not only excellent ion migration resistance and a low dielectric constant but also excellent peel strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 FIG. 4 is a cross-sectional view of a cover film according to a preferred embodiment of the present invention.

[0063] Figure 2 A diagram showing an electrode pattern for measuring the insulation resistance of a thermosetting adhesive film. DETAILED DESCRIPTION

[0064] Best Mode for Carrying Out the Invention

[0065] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings so that a person skilled in the art can easily implement the present invention. The present invention can be implemented in a variety of different embodiments and is not limited to the embodiments described in this specification. In order to clearly illustrate the present invention, parts not related to the description are omitted in the accompanying drawings, and the same reference numerals are given to the same or similar structural elements throughout the specification.

[0066] The thermosetting adhesive film of the present invention may include an epoxy resin which is solid at 15°C to 28°C, preferably at 20°C to 26°C, a thermosetting acrylic rubber which is solid at 15°C to 28°C, preferably at 20°C to 26°C, and a phosphorus-based flame retardant.

[0067] First, the epoxy resin of the present invention can improve the crosslinking density and reduce the moisture absorption rate and the chlorine content reduction effect, and the above-mentioned epoxy resin can include at least two selected from bisphenol A type epoxy resin, o-cresol novolac type epoxy resin, phenol novolac type epoxy resin, low chlorine type epoxy resin, dicyclopentadiene type epoxy resin, biphenyl type epoxy resin and multifunctional novolac type epoxy resin, preferably, can include two to four. If only one of the above-mentioned epoxy resins is used as the epoxy resin of the present invention, there may be a problem that not only the bonding force is reduced but also the odor resistance is reduced.

[0068] Specifically, the softening point of the epoxy resin of the present invention may be 60° C. to 80° C., preferably 66° C. to 75° C., and the epoxy equivalent of the epoxy resin of the present invention may be 200 g / eq to 350 g / eq, preferably 240 g / eq to 300 g / eq. If the epoxy equivalent is less than 200 g / eq, it may be difficult to adjust the resin fluidity, and if the epoxy equivalent exceeds 350 g / eq, the chemical resistance may deteriorate.

[0069] Secondly, the thermosetting acrylic rubber of the present invention can not only control resin flow, but also improve odor resistance, and the above-mentioned thermosetting acrylic rubber can be a polymer formed by polymerizing various monomer mixtures. Specifically, the thermosetting acrylic rubber can be a polymer formed by polymerizing a monomer mixture, and the above-mentioned monomer mixture includes at least three selected from butyl acrylate monomer, 2-ethylhexyl acrylate monomer, 2-methoxyethyl acrylate monomer, 4-hydroxybutyl acrylate monomer, ethyl acrylate monomer, 2-hydroxyethyl acrylate monomer, 2-hydroxypropyl acrylate monomer, pentyl methacrylate monomer, 2-hydroxymethyl acrylate monomer, ethyl methacrylate monomer, methyl methacrylate monomer, acrylic acid monomer and acrylonitrile monomer, preferably, including three to five kinds. If the thermosetting acrylic rubber of the present invention is a polymer formed by polymerizing the above-mentioned monomers including less than three kinds, there may be a problem of mechanical strength (tensile strength, Young's modulus, etc.) reduction.

[0070] In addition, the thermosetting acrylic rubber of the present invention may include a hydroxyl group and a carboxyl group as functional groups. If the thermosetting acrylic rubber does not include any of the hydroxyl group and the carboxyl group as functional groups, there may be problems that compatibility with epoxy resins is deteriorated and adhesion is reduced.

[0071] In addition, the weight average molecular weight of the thermosetting acrylic rubber of the present invention can be 400,000 to 1,500,000, preferably 800,000 to 1,100,000. If the weight average molecular weight is less than 400,000, excessive resin flow will occur and there will be a problem of reduced odor resistance. If the weight average molecular weight exceeds 1,500,000, there may be a problem of deterioration in workability due to increased viscosity.

[0072] In addition, the glass transition temperature of the thermosetting acrylic rubber of the present invention can be -10°C to 15°C, preferably, -5°C to 10°C. If the glass transition temperature is less than -10°C, the adhesive surface tackiness (Tacky) may increase. If the glass transition temperature exceeds 15°C, the adhesive odor resistance may deteriorate, especially at low temperatures below 10°C.

[0073] In addition, the acid value of the thermosetting acrylic rubber of the present invention may be 30 to 45, preferably 35 to 41. If the acid value is less than 30, there may be a problem of decreased adhesion, and if the acid value exceeds 45, there may be a problem of decreased stability of the mixture.

[0074] In addition, the viscosity of the thermosetting acrylic rubber of the present invention can be 500cps to 8,000cps, preferably, 4,000cps to 6,000cps. If the viscosity is less than 500cps, there may be a problem of reduced mixing stability (such as flame retardant sedimentation and aggregation). If the viscosity exceeds 8,000cps, there may be a problem of reduced coordination and mixing workability.

[0075] Secondly, the phosphorus-based flame retardant of the present invention is not only used to impart flame retardant effect, but also to ensure heat resistance. The above-mentioned phosphorus-based flame retardant may include at least one selected from phosphate-based flame retardants, phosphazene-based flame retardants and phosphinate-based flame retardants. Preferably, it may include at least one selected from phosphate-based flame retardants and phosphazene-based flame retardants.

[0076] On the other hand, the thermosetting adhesive film of the present invention may include 120 to 180 parts by weight of epoxy resin, preferably 140 to 160 parts by weight of epoxy resin, relative to 100 parts by weight of thermosetting acrylic rubber. If the content of epoxy resin is less than 120 parts by weight, there is a problem of deterioration of adhesion and heat resistance. If the content of epoxy resin exceeds 180 parts by weight, there is a problem of excessive resin flow.

[0077] In addition, the thermosetting adhesive film of the present invention may include 10 to 40 parts by weight of a phosphorus-based flame retardant, preferably 15 to 30 parts by weight of a phosphorus-based flame retardant, relative to 100 parts by weight of the thermosetting acrylic rubber. If the content of the phosphorus-based flame retardant is less than 10 parts by weight, the flame retardancy may not be ensured, and if the content of the phosphorus-based flame retardant exceeds 40 parts by weight, the heat resistance may be reduced.

[0078] In addition, the thermosetting adhesive film of the present invention may further include at least one selected from a curing agent and an inorganic filler, and preferably, may further include a curing agent and an inorganic filler.

[0079] The curing agent of the present invention can form crosslinks of epoxy resin, and the curing agent can include at least one selected from amine curing agents, imidazole curing agents and acid anhydride curing agents.

[0080] Furthermore, the inorganic filler of the present invention is a substance that can not only impart flame retardant effect but also improve mechanical strength. The inorganic filler can include at least one selected from aluminum hydroxide, magnesium hydroxide, silicon dioxide, aluminum oxide, zinc oxide, magnesium oxide, zirconium oxide, titanium oxide, iron oxide, cobalt oxide and chromium oxide.

[0081] On the other hand, the thermosetting adhesive film of the present invention may include 8 to 18 parts by weight of a curing agent, preferably 10 to 16 parts by weight of a curing agent, relative to 100 parts by weight of a thermosetting acrylic rubber. If the content of the curing agent is less than 8 parts by weight, there may be a problem of deterioration in heat resistance due to uncured adhesive components. If the content of the curing agent exceeds 18 parts by weight, there may be a problem of decreased adhesion and decreased long-term storage workability (rapid changes over time) due to excessive curing of the adhesive components.

[0082] On the other hand, the thermosetting adhesive film of the present invention may include 20 to 40 parts by weight of inorganic filler, preferably 25 to 35 parts by weight of inorganic filler, relative to 100 parts by weight of thermosetting acrylic rubber. If the content of the inorganic filler is less than 20 parts by weight, there may be a problem of reduced mechanical strength. If the content of the inorganic filler exceeds 40 parts by weight, there may be problems of sedimentation and aggregation of the inorganic filler.

[0083] Furthermore, the thermosetting adhesive film of the present invention may further contain an organic solvent in order to promote workability by adjusting the viscosity, and may contain methyl ethyl ketone as the organic solvent.

[0084] In addition, the thermosetting adhesive film of the present invention may further include various additives to improve physical properties, and preferably, may further include at least one selected from polyester raw materials, silane coupling agents and surfactants.

[0085] On the other hand, the thermosetting adhesive film of the present invention may satisfy all of the conditions (1) to (3).

[0086] (1) A ≥ 100 MΩ, preferably, 500 MΩ ≤ A ≤ 11,000 MΩ, more preferably, 1,000 MΩ ≤ A ≤ 5,000 MΩ.

[0087] In the above condition (1), A is the insulation resistance measured under the conditions of 85° C., 85% relative humidity and 50 V DC voltage for 500 to 1000 hours according to the IPC-TM 650 test standard.

[0088] (2) B1≤3.3, B2≤3.1, preferably, 2.9≤B1≤3.3, 2.8≤B2≤3.1, more preferably, 3.1≤B1≤3.25, 3.0≤B2≤3.1.

[0089] In the above condition (2), B1 represents the dielectric constant at 1 GHz, and B2 represents the dielectric constant at 10 GHz.

[0090] (3) C ≥ 0.7 kgf / cm, preferably, 1.2 kgf / cm ≤ C ≤ 2.2 kgf / cm, more preferably, 1.7 kgf / cm ≤ C ≤ 2.0 kgf / cm.

[0091] In the above condition (3), C represents the peel strength measured when peeling at a speed of 50 mm / min and a peeling direction of 90°.

[0092] Furthermore, the thermosetting adhesive film of the present invention may also satisfy condition (4).

[0093] (4) D≤0.5%, preferably, 0.1%≤D≤0.4%, more preferably, 0.2%≤D≤0.3%.

[0094] In the above condition (4), D represents the moisture absorption rate measured according to the following relational expression 1 according to the IPC TM-650 test standard.

[0095] [Equation 1]

[0096] Moisture absorption rate (%) = (D1-D0) / D0×100

[0097] In the above-mentioned Relational Formula 1, D0 represents the weight of the dry thermosetting adhesive film, and D1 represents the weight of the dry thermosetting adhesive film after immersing it in distilled water for 24 hours.

[0098] Furthermore, the thermosetting adhesive film of the present invention may also satisfy condition (5).

[0099] (5) 65°C≤E≤85°C, preferably, 68°C≤E≤80°C, more preferably, 70°C≤E≤75°C.

[0100] In the above condition (5), E represents the glass transition temperature. If the glass transition temperature is lower than 65°C, the adhesive film surface may become sticky. If the glass transition temperature exceeds 85°C, the odor resistance may decrease and the adhesive force may decrease.

[0101] Furthermore, the thermosetting adhesive film of the present invention may also satisfy condition (6).

[0102] (6) 65ppm / ℃≤F1≤95ppm / ℃, 200ppm / ℃≤F2≤280ppm / ℃, preferably, 75ppm / ℃≤F1≤90ppm / ℃, 220ppm / ℃≤F2≤260ppm / ℃, more preferably, 80ppm / ℃≤F1≤85ppm / ℃, 240ppm / ℃≤F2≤250ppm / ℃.

[0103] In the above condition (6), F1 represents the thermal expansion coefficient before reaching the glass transition temperature when the temperature is increased at a rate of 10°C / min, and F2 represents the thermal expansion coefficient after reaching the glass transition temperature when the temperature is increased at a rate of 10°C / min.

[0104] Furthermore, the thermosetting adhesive film of the present invention may also satisfy condition (7).

[0105] (7) 20 MPa≤G≤50 MPa, preferably, 22 MPa≤G≤40 MPa, more preferably, 25 MPa≤G≤33 MPa.

[0106] In the above condition (7), G represents the tensile strength measured according to the IPC TM-650 test standard.

[0107] Furthermore, the thermosetting adhesive film of the present invention may also satisfy condition (8).

[0108] (8) 0.3 GPa ≤ H ≤ 1.0 GPa, preferably, 0.4 GPa ≤ H ≤ 0.8 GPa, more preferably, 0.5 GPa ≤ H ≤ 0.7 GPa.

[0109] In the above condition (8), H represents the Young's modulus measured according to the IPC TM-650 test standard.

[0110] Furthermore, the thermosetting adhesive film of the present invention may also satisfy condition (9).

[0111] (9) 30%≤I≤130%, preferably, 40%≤I≤120%, more preferably, 60%≤I≤120%, further preferably, 100%≤I≤120%

[0112] In the above condition (9), I represents the elongation measured according to the IPC TM-650 test standard.

[0113] Furthermore, refer to Figure 1 The cover film of the present invention may include an electrical insulating substrate 20, a thermosetting adhesive film 10 formed on one side of the electrical insulating substrate, and a release film 30 formed on one side of the thermosetting adhesive film 10. At this time, the thermosetting adhesive film 10 may include the above-mentioned thermosetting adhesive film of the present invention.

[0114] In addition, although the cover film including the thermosetting adhesive film of the present invention is used as a representative example, the thermosetting adhesive film of the present invention is not limited thereto, and can also be applied to an adhesive sheet, a metal laminate, and the like.

[0115] In addition, the electrically insulating substrate 10 and the release film 30 are not particularly limited, but can generally be polyimide (PI), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), liquid crystal polymer (LCP) film, aramid film, fluorine-based film, etc. Preferably, when high-temperature dimensional stability is required at a temperature above 240°C, the electrically insulating substrate can be a polyimide film, and the release film can be a polyethylene terephthalate film.

[0116] Hereinafter, the present invention will be described by the following examples. At this time, the following examples are only used to illustrate the present invention, and the scope of the present invention is not limited by the following examples.

[0117] Modes for Carrying Out the Invention

[0118] Example 1: Preparation of thermosetting adhesive film

[0119] A mixture was prepared by mixing a thermosetting acrylic rubber which was solid at a temperature of 20°C to 26°C and included a hydroxyl group and a carboxyl group as functional groups, an epoxy resin which was solid at a temperature of 20°C to 26°C, a phosphorus-based flame retardant, a curing agent, and an inorganic filler in methyl ethyl ketone as an organic solvent, and the prepared mixture was dried in an oven at 150°C for 2 minutes to prepare a thermosetting adhesive film having a thickness of 20 μm and a glass transition temperature of 73°C.

[0120] At this time, 150 parts by weight of epoxy resin, 20 parts by weight of phosphorus flame retardant, 13 parts by weight of curing agent and 30 parts by weight of inorganic filler are mixed with respect to 100 parts by weight of thermosetting acrylic rubber, and a polymer prepared by polymerizing ethyl acrylate monomer, acrylonitrile monomer, 2-hydroxyethyl acrylate monomer and ethyl methacrylate monomer in a weight ratio of 1:6:1:2 is used as the thermosetting acrylic rubber (solid content: 20 weight %), and the above-mentioned thermosetting acrylic rubber has a weight average molecular weight of 850,000, a glass transition temperature of 5.85°C, an acid value of 37.5 and a viscosity of 5,000 cps.

[0121] In addition, as the epoxy resin, an epoxy resin with a softening point of 71°C and an epoxy equivalent of 270 g / eq is used. The above-mentioned epoxy resin is a mixture formed by mixing 30 parts by weight of a bisphenol A type epoxy resin that is liquid at a temperature of 20°C to 26°C and 20 parts by weight of a phenol novolac type epoxy resin with respect to 100 parts by weight of a bisphenol A type epoxy resin that is solid at a temperature of 20°C to 26°C.

[0122] A phosphazene-based flame retardant was used as the phosphorus-based flame retardant, a mixture of 10 parts by weight of an amine-based curing agent and 3 parts by weight of an imidazole-based curing agent was used as the curing agent, and aluminum hydroxide was used as the inorganic filler.

[0123] Example 2: Preparation of thermosetting adhesive film

[0124] A thermosetting adhesive film was prepared in the same manner as in Example 1. However, the difference from Example 1 is that 110 parts by weight of epoxy resin was mixed with respect to 100 parts by weight of thermosetting acrylic rubber to finally prepare the thermosetting adhesive film. At this time, as the epoxy resin, an epoxy resin having a softening point of 71° C. and an epoxy equivalent of 270 g / eq was used, and the 110 parts by weight of epoxy resin was a mixture of 73 parts by weight of a bisphenol A type epoxy resin that was solid at a temperature of 20° C. to 26° C., 22 parts by weight of a bisphenol A type epoxy resin that was liquid at a temperature of 20° C. to 26° C., and 15 parts by weight of a phenol novolac type epoxy resin.

[0125] Example 3: Preparation of thermosetting adhesive film

[0126] A thermosetting adhesive film was prepared in the same manner as in Example 1. However, the difference from Example 1 is that 190 parts by weight of epoxy resin was mixed with respect to 100 parts by weight of thermosetting acrylic rubber to finally prepare the thermosetting adhesive film. At this time, as the epoxy resin, an epoxy resin having a softening point of 71° C. and an epoxy equivalent of 270 g / eq was used, and the 190 parts by weight of epoxy resin was a mixture of 127 parts by weight of a bisphenol A type epoxy resin that was solid at a temperature of 20° C. to 26° C., 38 parts by weight of a bisphenol A type epoxy resin that was liquid at a temperature of 20° C. to 26° C., and 25 parts by weight of a phenol novolac type epoxy resin.

[0127] Example 4: Preparation of thermosetting adhesive film

[0128] A thermosetting adhesive film was prepared in the same manner as in Example 1. However, unlike Example 1, a mixture of 30 parts by weight of a bisphenol A type epoxy resin that is liquid at a temperature of 20° C. to 26° C. was used as the epoxy resin to finally prepare the thermosetting adhesive film with respect to 100 parts by weight of a bisphenol A type epoxy resin that is solid at a temperature of 20° C. to 26° C. The epoxy resin had a softening point of 67° C. and an epoxy equivalent of 285 g / eq.

[0129] Example 5: Preparation of thermosetting adhesive film

[0130] A thermosetting adhesive film was prepared in the same manner as in Example 1. However, unlike Example 1, a mixture of 20 parts by weight of a phenol novolac type epoxy resin with respect to 100 parts by weight of a bisphenol A type epoxy resin that is solid at a temperature of 20° C. to 26° C. was used as the epoxy resin to finally prepare the thermosetting adhesive film. At this time, the epoxy resin had a softening point of 77° C. and an epoxy equivalent of 291 g / eq.

[0131] Example 6: Preparation of thermosetting adhesive film

[0132] A thermosetting adhesive film was prepared in the same manner as in Example 1. However, unlike Example 1, a mixture of 30 parts by weight of a bisphenol A type epoxy resin that is solid at a temperature of 20° C. to 26° C. was used as the epoxy resin to finally prepare the thermosetting adhesive film with respect to 100 parts by weight of a bisphenol A type epoxy resin that is liquid at a temperature of 20° C. to 26° C. The epoxy resin had a softening point of 52° C. and an epoxy equivalent of 190 g / eq.

[0133] Example 7: Preparation of thermosetting adhesive film

[0134] A thermosetting adhesive film was prepared in the same manner as in Example 1. However, unlike Example 1, a mixture of 30 parts by weight of a bisphenol F type epoxy resin that is liquid at a temperature of 20° C. to 26° C. was used as the epoxy resin to finally prepare the thermosetting adhesive film with respect to 100 parts by weight of a bisphenol F type epoxy resin that is solid at a temperature of 20° C. to 26° C. The epoxy resin had a softening point of 85° C. and an epoxy equivalent of 364 g / eq.

[0135] Example 8: Preparation of thermosetting adhesive film

[0136] A thermosetting adhesive film was prepared in the same manner as in Example 1. However, the difference from Example 1 was that a polymer obtained by polymerizing ethyl acrylate monomer, acrylonitrile monomer, 2-hydroxyethyl acrylate monomer, and ethyl methacrylate monomer at a weight ratio of 1:6:1:2 was used as a thermosetting acrylic rubber (solid content: 20 wt %) to finally prepare a thermosetting adhesive film. At this time, a thermosetting acrylic rubber having a weight average molecular weight of 830,000, a glass transition temperature of 5.6° C., an acid value of 19.7, and a viscosity of 4,900 cps was used.

[0137] Example 9: Preparation of thermosetting adhesive film

[0138] A thermosetting adhesive film was prepared in the same manner as in Example 1. However, the difference from Example 1 was that a polymer obtained by polymerizing ethyl acrylate monomer, acrylonitrile monomer, 2-hydroxyethyl acrylate monomer, and ethyl methacrylate monomer at a weight ratio of 1:6:1:2 was used as a thermosetting acrylic rubber (solid content: 20 wt %) to finally prepare a thermosetting adhesive film. At this time, a thermosetting acrylic rubber having a weight average molecular weight of 350,000, a glass transition temperature of 4.3° C., an acid value of 35.6, and a viscosity of 2,100 cps was used.

[0139] Example 10: Preparation of thermosetting adhesive film

[0140] A thermosetting adhesive film was prepared in the same manner as in Example 1. However, unlike Example 1, a phosphate-based flame retardant was used as the phosphorus-based flame retardant instead of the phosphazene-based flame retardant to finally prepare a thermosetting adhesive film.

[0141] Example 11: Preparation of thermosetting adhesive film

[0142] A thermosetting adhesive film was prepared in the same manner as in Example 1. However, unlike Example 1, a nitrogen-based melamine compound flame retardant was used as a phosphorus-based flame retardant instead of the phosphazene-based flame retardant to finally prepare a thermosetting adhesive film.

[0143] Example 12: Preparation of thermosetting adhesive film

[0144] A thermosetting adhesive film was prepared in the same manner as in Example 1. However, unlike Example 1, 5 parts by weight of a phosphorus-based flame retardant was mixed with respect to 100 parts by weight of the thermosetting acrylic rubber to finally prepare the thermosetting adhesive film.

[0145] Example 13: Preparation of thermosetting adhesive film

[0146] A thermosetting adhesive film was prepared in the same manner as in Example 1. However, unlike Example 1, 45 parts by weight of a phosphorus-based flame retardant was mixed with respect to 100 parts by weight of the thermosetting acrylic rubber to finally prepare the thermosetting adhesive film.

[0147] Comparative Example 1: Preparation of Thermosetting Adhesive Film

[0148] A thermosetting adhesive film was prepared in the same manner as in Example 1. However, unlike Example 1, a polymer obtained by polymerizing ethyl acrylate monomer, acrylonitrile monomer, 2-hydroxyethyl acrylate monomer, and ethyl methacrylate monomer at a weight ratio of 1:5:1:1 was used as a thermosetting acrylic rubber (solid content: 20 wt %) to finally prepare a thermosetting adhesive film. At this time, a thermosetting acrylic rubber having a weight average molecular weight of 830,000, a glass transition temperature of -16°C, an acid value of 35.0, and a viscosity of 4,000 cps was used.

[0149] Comparative Example 2: Preparation of Thermosetting Adhesive Film

[0150] A thermosetting adhesive film was prepared in the same manner as in Example 1. However, the difference from Example 1 was that a polymer obtained by polymerizing ethyl acrylate monomer, acrylonitrile monomer, 2-hydroxyethyl acrylate monomer, and ethyl methacrylate monomer at a weight ratio of 1:4.5:1:2 was used as a thermosetting acrylic rubber (solid content: 20 wt %) to finally prepare a thermosetting adhesive film. At this time, a thermosetting acrylic rubber having a weight average molecular weight of 790,000, a glass transition temperature of 20° C., an acid value of 36.3, and a viscosity of 4,200 cps was used.

[0151] Example 14: Preparation of thermosetting adhesive film

[0152] A mixture was prepared by mixing a thermosetting acrylic rubber which was solid at a temperature of 20° C. to 26° C. and included a hydroxyl group and a carboxyl group as functional groups, an epoxy resin which was solid at a temperature of 20° C. to 26° C., a phosphorus-based flame retardant, a curing agent, and an inorganic filler in methyl ethyl ketone as an organic solvent, and the prepared mixture was dried in an oven at 150° C. for 2 minutes to prepare a thermosetting adhesive film having a thickness of 20 μm and a glass transition temperature of 64° C.

[0153] At this time, 150 parts by weight of epoxy resin, 20 parts by weight of phosphorus flame retardant, 13 parts by weight of curing agent and 30 parts by weight of inorganic filler were mixed with respect to 100 parts by weight of thermosetting acrylic rubber, and a polymer obtained by polymerizing ethyl acrylate monomer, acrylonitrile monomer, 2-hydroxyethyl acrylate monomer and ethyl methacrylate monomer at a weight ratio of 1:5.2:1:0.5 was used as the thermosetting acrylic rubber (solid content: 20% by weight), and the thermosetting acrylic rubber had a weight average molecular weight of 790,000, a glass transition temperature of -8°C, an acid value of 36.2 and a viscosity of 3,900 cps. In addition, a mixture obtained by mixing 50 parts by weight of bisphenol A type epoxy resin which is solid at a temperature of 20°C to 26°C with respect to 100 parts by weight of bisphenol A type epoxy resin which is liquid at a temperature of 20°C to 26°C was used as the epoxy resin. A phosphazene-based flame retardant was used as the phosphorus-based flame retardant, a mixture of 10 parts by weight of an amine-based curing agent and 3 parts by weight of an imidazole-based curing agent was used as the curing agent, and aluminum hydroxide was used as the inorganic filler.

[0154] Example 15: Preparation of thermosetting adhesive film

[0155] A mixture was prepared by mixing a thermosetting acrylic rubber which was solid at a temperature of 20° C. to 26° C. and included a hydroxyl group and a carboxyl group as functional groups, an epoxy resin which was solid at a temperature of 20° C. to 26° C., a phosphorus-based flame retardant, a curing agent, and an inorganic filler in methyl ethyl ketone as an organic solvent, and the prepared mixture was dried in an oven at 150° C. for 2 minutes to prepare a thermosetting adhesive film having a thickness of 20 μm and a glass transition temperature of 83° C. At this time, 150 parts by weight of epoxy resin, 20 parts by weight of phosphorus flame retardant, 13 parts by weight of curing agent and 30 parts by weight of inorganic filler were mixed with respect to 100 parts by weight of thermosetting acrylic rubber, and a polymer obtained by polymerizing ethyl acrylate monomer, acrylonitrile monomer, 2-hydroxyethyl acrylate monomer and ethyl methacrylate monomer in a weight ratio of 1:4.8:1:2 was used as the thermosetting acrylic rubber (solid content: 20% by weight), and the thermosetting acrylic rubber had a weight average molecular weight of 820,000, a glass transition temperature of 13°C, an acid value of 37.1 and a viscosity of 4,000 cps. In addition, a mixture obtained by mixing 50 parts by weight of phenol novolac type epoxy resin which was liquid at a temperature of 20°C to 26°C with respect to 100 parts by weight of bisphenol A type epoxy resin which was solid at a temperature of 20°C to 26°C was used as the epoxy resin. A phosphazene-based flame retardant was used as the phosphorus-based flame retardant, a mixture of 10 parts by weight of an amine-based curing agent and 3 parts by weight of an imidazole-based curing agent was used as the curing agent, and aluminum hydroxide was used as the inorganic filler.

[0156] Experimental Example 1

[0157] The following physical properties of the thermosetting adhesive films prepared by the above Examples 1 to 15 and Comparative Examples 1 to 2 were measured, and the results are shown in Tables 1 to 5 below.

[0158] 1. Insulation resistance (migration evaluation)

[0159] According to the IPC-TM 650 test standard, the insulation resistance (MΩ) of the thermosetting adhesive films prepared by Examples 1 to 15 and Comparative Examples 1 to 2 was measured.

[0160] Specifically, if Figure 2 As shown, a polyimide (PI) film (thickness: 25 μm) having a comb-like structure pattern in which positive and negative electrodes are crossed on one side was prepared, and a sample was prepared by laminating the thermosetting adhesive films prepared in Examples 1 to 15 and Comparative Examples 1 to 2 on the polyimide film having the pattern. AMI-025-U-5 (Espec Corp., Japan) was used as an insulation resistance measuring device. The insulation resistance of the sample was measured for 1000 hours under the conditions of 85°C, 85% relative humidity and 50V DC voltage (using water: ultrapure water of 10 MΩ.cm or more). The average insulation resistance measured within 500 to 1000 hours during the measurement time is as shown in Tables 1 to 5 below.

[0161] 2. Dielectric constant

[0162] After placing each of the thermosetting adhesive films prepared by Examples 1 to 15 and Comparative Examples 1 to 2 between a first release film for hot press and a second release film for hot press, heat curing was performed by hot press to prepare a sample. At this time, at a temperature of 160° C. and 45 kgf / cm 2 The heat curing was carried out under pressure for 60 minutes.

[0163] The prepared sample was cut into a size of 150 mm in width, 160 mm in length, and 20 μm in thickness, and the dielectric constant at 1 GHz was measured using an LCR meter (Key sight E5041C). The results are shown in Tables 1 to 5 below.

[0164] Furthermore, the prepared sample was cut into a size of 40 mm in width, 40 mm in length, and 20 μm in thickness, and the dielectric constant at 10 GHz was measured using an LCR meter (Key sight E5041C). The results are shown in Tables 1 to 5 below.

[0165] 3. Peel strength

[0166] Two flexible copper clad laminates (FCCL, HGLS-S211EM) were prepared by sequentially laminating electrolytic copper foil (thickness: 1 oz), adhesive (thickness: 10 μm), and polyimide film (thickness: 25 μm). After positioning the two FCCLs in a relative manner, each of the thermosetting adhesive films prepared by Examples 1 to 15 and Comparative Examples 1 to 2 was placed therebetween, and then thermally cured by hot pressing to prepare a sample. At this time, the temperature was 160°C and the pressure was 45 kgf / cm 2 The heat curing was carried out under pressure for 60 minutes.

[0167] The prepared sample was cut into a size of 150 mm in width and 150 mm in length, and a piece of FCCL was peeled off at a speed of 50 mm / min and a peeling direction of 90° to measure the peel strength (when measuring the peel strength, the initial value of 5 mm was excluded, and the average value after repeated measurement 3 times is shown in the following Tables 1 to 5).

[0168] 4. Moisture absorption rate

[0169] According to the IPC-TM 650 test standard, the moisture absorption rates (%) of the thermosetting adhesive films prepared by Examples 1 to 15 and Comparative Examples 1 to 2 were measured.

[0170] Specifically, after placing each of the thermosetting adhesive films prepared by Examples 1 to 15 and Comparative Examples 1 to 2 between a first release film for hot press and a second release film for hot press, heat curing was performed by hot press to prepare a sample. At this time, at a temperature of 160° C. and 45 kgf / cm 2 The heat curing was carried out under pressure for 60 minutes.

[0171] The prepared sample was cut into a size of 50 mm in width, 50 mm in length, and 20 μm in thickness, and the sample was dried at 105° C. for 1 hour, and the weight of the dried sample was measured.

[0172] Soak the dried sample in distilled water for 24 hours at room temperature (23±1°C). After soaking, wipe off the moisture on the surface of the sample with a dry cloth, and then measure the weight of the sample after moisture absorption.

[0173] The moisture absorption rate was calculated by the following equation 1, and the calculated values ​​are shown in Tables 1 to 5 below.

[0174] [Equation 1]

[0175] Moisture absorption rate (%) = (sample after moisture absorption - sample after drying) / sample after drying × 100

[0176] 5. Thermal expansion coefficient

[0177] After placing each of the thermosetting adhesive films prepared by Examples 1 to 15 and Comparative Examples 1 to 2 between a first release film for hot press and a second release film for hot press, heat curing was performed by hot press to prepare a sample. At this time, at a temperature of 160° C. and 45 kgf / cm 2 The heat curing was performed for 60 minutes under the condition of a pressure of . In addition, in order to prevent oxidation, the prepared sample was purged with nitrogen at 50 cc / min.

[0178] The prepared sample was cut into a size of 5 mm in width and 16 mm in length, and the thermal expansion coefficient (F1) of the sample before reaching the glass transition temperature and the thermal expansion coefficient (F2) after reaching the glass transition temperature were measured using a TMA Q 400 apparatus while heating the sample from room temperature (23±1°C) to 200°C at a heating rate of 10°C / min. The results are shown in Tables 1 to 5 below.

[0179] 6.Tensile strength, Young's modulus, elongation

[0180] According to the IPC-TM 650 test standard, the tensile strength, Young's modulus, and elongation of each of the thermosetting adhesive films prepared by Examples 1 to 15 and Comparative Examples 1 to 2 were measured.

[0181] Specifically, after placing each of the thermosetting adhesive films prepared by Examples 1 to 15 and Comparative Examples 1 to 2 between a first release film for hot press and a second release film for hot press, heat curing was performed by hot press to prepare a sample. At this time, at a temperature of 160° C. and 45 kgf / cm 2 The heat curing was carried out under pressure for 60 minutes.

[0182] The prepared sample was cut into a size of 100 mm in width, 100 mm in length, and 20 μm in thickness, and a middle portion of the prepared sample was punched. The punched portion of the sample had a length of 20 mm and a thickness of 5 mm.

[0183] The sample was placed in a tensile tester with a span of 10 mm, and the sample was stretched at a speed of 50 mm / min to calculate the tensile strength, Young's modulus and elongation at break. The results are shown in Tables 1 to 5 below.

[0184] 7. Resin fluidity

[0185] The samples were prepared by flat-head welding each of the thermosetting adhesive films prepared by Examples 1 to 15 and Comparative Examples 1 to 2 on one side of a polyimide film (thickness: 25 μm). At this time, flat-head welding was performed at a temperature of 110° C. and a speed of 1.0 m / min. One side of the prepared sample was punched, and the thermosetting adhesive film layer of the sample was laminated on the polyimide film of the FCCL, and then thermally cured by hot pressing. At this time, the temperature was 160° C. and the speed was 45 kgf / cm 2 The heat curing was performed for 60 minutes under the condition of a pressure of . FCCL (HGLS-S211EM) was used, in which electrolytic copper foil (thickness: 1 oz), adhesive (thickness: 10 μm), and polyimide film (thickness: 25 μm) were laminated in this order.

[0186] Thereafter, the resin fluidity (the length of the adhesive flowing out during the heat pressing process) of the punched portion of the sample was measured using a microscope. The results are shown in Tables 1 to 5 below.

[0187] 8. Flame retardancy

[0188] Two polyimide films (thickness: 25 μm) were prepared. After the two polyimide films were positioned in an opposing manner, each of the thermosetting adhesive films prepared by Examples 1 to 15 and Comparative Examples 1 to 2 was placed therebetween, and then heat cured by hot pressing to prepare a sample. At this time, at a temperature of 160° C. and 45 kgf / cm 2 The heat curing was carried out under pressure for 60 minutes.

[0189] The prepared samples were subjected to a flame retardancy test according to the UL94 flame retardancy standard. When the flame retardancy standard was met, it was evaluated as OK, and when the flame retardancy standard was not met, it was evaluated as NG. The results are shown in Tables 1 to 5 below.

[0190] Table 1

[0191]

[0192] It can be confirmed from Table 1 that the thermosetting adhesive film prepared by Example 1 has excellent resistance to ion migration, exhibits a low dielectric constant not only at 1 GHz but also at 10 GHz, has low moisture absorption, excellent mechanical properties, and is flame retardant.

[0193] However, it can be confirmed that the tensile strength and Young's modulus of the thermosetting adhesive film prepared in Example 2 are decreased compared with the thermosetting adhesive film prepared in Example 1.

[0194] In addition, it can be confirmed that the thermal expansion coefficient and elongation of the thermosetting adhesive film prepared in Example 3 are significantly increased compared with the thermosetting adhesive film prepared in Example 1.

[0195] Furthermore, it can be confirmed that the peel strength of the thermosetting adhesive film prepared in Example 4 is reduced, and the thermal expansion coefficient and elongation are increased, compared with the thermosetting adhesive film prepared in Example 1.

[0196] Also, it can be confirmed that the peel strength and resin fluidity of the thermosetting adhesive film prepared in Example 5 are reduced compared to the thermosetting adhesive film prepared in Example 1.

[0197] Table 2

[0198]

[0199] As can be seen from Table 2, compared with the thermosetting adhesive film prepared in Example 1, the thermosetting adhesive film prepared in Example 6 has lower peel strength and elongation and increased resin fluidity.

[0200] Also, it was confirmed that the thermosetting adhesive film prepared in Example 7 had lower insulation resistance, peel strength, elongation, and resin fluidity, and increased moisture absorption and thermal expansion coefficient, compared to the thermosetting adhesive film prepared in Example 1.

[0201] Also, it can be confirmed that the peel strength of the thermosetting adhesive film prepared in Example 8 is reduced and the resin fluidity is increased compared to the thermosetting adhesive film prepared in Example 1.

[0202] Furthermore, it can be confirmed that the peel strength, tensile strength, Young's modulus and elongation of the thermosetting adhesive film prepared in Example 9 are decreased, and the thermal expansion coefficient and resin fluidity are increased compared with the thermosetting adhesive film prepared in Example 1.

[0203] Table 3

[0204]

[0205] As can be seen from Table 3, compared with the thermosetting adhesive film prepared in Example 1, the dielectric constant of the thermosetting adhesive film prepared in Example 10 increases, and the moisture absorption rate also increases.

[0206] Also, it can be confirmed that the dielectric constant and flame retardancy of the thermosetting adhesive film prepared in Example 11 are lowered compared to the thermosetting adhesive film prepared in Example 1.

[0207] In addition, it can be confirmed that the flame retardancy of the thermosetting adhesive film prepared in Example 12 is reduced compared with the thermosetting adhesive film prepared in Example 1.

[0208] Also, it can be confirmed that the insulation resistance and peel strength of the thermosetting adhesive film prepared in Example 13 are reduced compared to the thermosetting adhesive film prepared in Example 1.

[0209] Table 4

[0210]

[0211] It can be seen from Table 4 that, compared with the thermosetting adhesive film prepared in Example 1, the tensile strength and Young's modulus of the thermosetting adhesive film prepared in Comparative Example 1 are reduced, while the thermal expansion coefficient and elongation are increased.

[0212] Furthermore, it can be confirmed that the peel strength of the thermosetting adhesive film prepared in Comparative Example 2 is reduced, while the resin fluidity is increased, compared with the thermosetting adhesive film prepared in Example 1.

[0213] Table 5

[0214]

[0215] It can be seen from Table 5 that, compared with the thermosetting adhesive film prepared in Example 1, the thermal expansion coefficient and elongation of the thermosetting adhesive film prepared in Example 14 increased, while the tensile strength and Young's modulus decreased.

[0216] In addition, it can be confirmed that the peel strength of the thermosetting adhesive film prepared in Example 15 is decreased compared with the thermosetting adhesive film prepared in Example 1.

[0217] Those skilled in the art can easily implement simple modifications or changes of the present invention, and such modifications or changes all belong to the protection scope of the present invention.

[0218] Industrial Applicability

[0219] The present invention relates to a thermosetting adhesive film and a cover film including the same, and more particularly to a thermosetting adhesive film having excellent resistance to ion migration, a low dielectric constant and excellent peel strength and a cover film including the same.

Claims

1. A thermosetting adhesive film, characterized in that: The invention comprises an epoxy resin which is solid at a temperature of 15°C to 28°C, a thermosetting acrylic rubber which is solid at a temperature of 15°C to 28°C, and a phosphorus-based flame retardant, The thermosetting acrylic rubber contains a hydroxyl group and a carboxyl group as functional groups, and has a weight average molecular weight of 400,000 to 1,500,000 and a glass transition temperature of -10°C to 15°C. The above-mentioned thermosetting adhesive films all satisfy conditions (1) to (3) and (5): (1) A ≥ 100 MΩ (2) B1≤3.3, B2≤3.1 (3) C ≥ 0.7 kgf / cm (5)68℃≤E≤80℃ In the above condition (1), A is the insulation resistance measured under the conditions of 85°C, 85% relative humidity and 50V DC voltage for 500 hours to 1000 hours according to the IPC-TM 650 test standard, In the above condition (2), B1 represents the dielectric constant at 1 GHz, B2 represents the dielectric constant at 10 GHz, In the above condition (3), C represents the peel strength measured when peeling at a speed of 50 mm / min and a peeling direction of 90°. In the above condition (5), E represents the glass transition temperature Tg.

2. The thermosetting adhesive film according to claim 1, characterized in that The above-mentioned thermosetting adhesive film further satisfies conditions (4) and (6): (4)D≤0.5% (6)65ppm / ℃≤F1≤95ppm / ℃, 200ppm / ℃≤F2≤280ppm / ℃ In the above condition (4), D represents the moisture absorption rate measured according to the following relationship 1 according to the IPC TM-650 test standard, In the above condition (6), F1 represents the thermal expansion coefficient before reaching the glass transition temperature when the temperature is increased at a rate of 10°C / min, and F2 represents the thermal expansion coefficient after reaching the glass transition temperature when the temperature is increased at a rate of 10°C / min. [Equation 1] Moisture absorption rate (%) = (D1-D0) / D0×100 In the above-mentioned Relational Formula 1, D0 represents the weight of the dry thermosetting adhesive film, and D1 represents the weight of the dry thermosetting adhesive film after immersing it in distilled water for 24 hours.

3. The thermosetting adhesive film according to claim 1, characterized in that: The above-mentioned thermosetting adhesive film further satisfies conditions (7) to (9): (7)20MPa≤G≤50MPa (8)0.3GPa≤H≤1.0GPa (9)30%≤I≤130% In the above condition (7), G represents the tensile strength measured according to the IPC TM-650 test standard, In the above condition (8), H represents the Young's modulus measured according to the IPC TM-650 test standard, In the above condition (9), I represents the elongation measured according to the IPC TM-650 test standard.

4. The thermosetting adhesive film according to claim 1, characterized in that: The epoxy resin includes at least two selected from bisphenol A epoxy resin, o-cresol novolac epoxy resin, phenol novolac epoxy resin, dicyclopentadiene epoxy resin and biphenyl epoxy resin.

5. The thermosetting adhesive film according to claim 1, characterized in that: The epoxy resin has a softening point of 60° C. to 80° C. and an epoxy equivalent of 200 g / eq to 350 g / eq.

6. The thermosetting adhesive film according to claim 1, characterized in that: The above-mentioned thermosetting acrylic rubber is a polymer formed by polymerizing a monomer mixture, and the above-mentioned monomer mixture includes at least three selected from butyl acrylate monomer, 2-ethylhexyl acrylate monomer, 2-methoxyethyl acrylate monomer, 4-hydroxybutyl acrylate monomer, ethyl acrylate monomer, 2-hydroxyethyl acrylate monomer, 2-hydroxypropyl acrylate monomer, amyl methacrylate monomer, 2-hydroxymethyl acrylate monomer, ethyl methacrylate monomer, methyl methacrylate monomer, acrylic acid monomer and acrylonitrile monomer.

7. The thermosetting adhesive film according to claim 6, characterized in that: The above-mentioned thermosetting acrylic rubber has an acid value of 30 to 45 and a viscosity of 500 cps to 8,000 cps.

8. The thermosetting adhesive film according to claim 1, characterized in that: The phosphorus-based flame retardant includes at least one selected from phosphate-based flame retardants, phosphazene-based flame retardants and phosphinate-based flame retardants.

9. The thermosetting adhesive film according to claim 1, characterized in that: The thermosetting adhesive film includes 120 to 180 parts by weight of epoxy resin and 10 to 40 parts by weight of phosphorus-based flame retardant relative to 100 parts by weight of thermosetting acrylic rubber.

10. The thermosetting adhesive film according to claim 1, characterized in that The thermosetting adhesive film further includes at least one selected from a curing agent and an inorganic filler.

11. The thermosetting adhesive film according to claim 10, characterized in that: The thermosetting adhesive film includes 8 to 18 parts by weight of a curing agent and 20 to 40 parts by weight of an inorganic filler relative to 100 parts by weight of the thermosetting acrylic rubber.

12. The thermosetting adhesive film according to claim 11, characterized in that: The curing agent includes at least one selected from an amine curing agent, an imidazole curing agent and an acid anhydride curing agent. The inorganic filler includes at least one selected from aluminum hydroxide, magnesium hydroxide, silicon dioxide, aluminum oxide, zinc oxide, magnesium oxide, zirconium oxide, titanium oxide, iron oxide, cobalt oxide and chromium oxide.

13. A covering film, characterized in that: include: Electrically insulating substrates; The thermosetting adhesive film according to claim 1, formed on one surface of the electrical insulating substrate; and The release film is formed on one side of the thermosetting adhesive film.