Nucleating agent and preparation method thereof, and preparation method of polymer rod-shaped ultrafine powder
By adding nucleating agent to the polymer solution and using high-speed crushing equipment, the problems of uneven particle size of special polymer powder and equipment blockage are solved, and rod-shaped powder preparation with high bulk density and small particle size are achieved, which improves material performance and Production efficiency.
Patent Information
- Application Number
- CN202211583084.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-12-09
AI Technical Summary
The prior art is difficult to effectively crush the polymer materials in special polymer solutions, resulting in uneven powder particle size, affecting material performance and mixing uniformity, and easily clogging the equipment during the crushing process.
The nucleating agent is mixed with polymer solution for precipitation and pulverization, and the nucleating agent is prepared by reaction of halogenated aromatic anhydride and aliphatic hydrocarbon diol. During the pulverization process, high-speed crushing equipment and inert solvent circulation system are used to form a rod-shaped ultrafine Powder improves the packing density and particle size uniformity of the powder.
Continuous feeding and crushing of polymers is achieved, forming rod-shaped powder with high bulk density and small particle size, reducing impurities residues after crushing, and improving product quality and mixing uniformity.
Smart Images

Figure CN115819240B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer material preparation, in particular to the morphology of polymers, and more particularly to a method for preparing polymer powders. Background Art
[0002] Special polymer ultrafine powder is a kind of basic raw material that can be used for material modification, coating preparation and other applications, and has special uses. For example, polyethersulfone ultrafine powder can be used for heat-resistant coatings. For example, the interior coatings of Civil Aviation Technology are all polyethersulfone materials; non-stick pan coatings can also use polyethersulfone or polyetheretherketone coatings. For some special polymers, due to the rigid structures such as benzene rings in their structures and the excellent mechanical properties of the materials themselves, they are not easy to be broken, so it is very difficult to prepare ultrafine powders. In some special fields, special polymer materials need to be used to modify them.
[0003] Solution polymerization is a method for synthesizing polymers. It is a polymerization reaction of one or more monomers in a solution to produce a special polymer solution. Some polymer solutions are relatively easy to remove by devolatilization (such as polyoxymethylene, polyolefin elastomers, etc.), and polymer particles are obtained by pelletizing. Some special polymerizations need to be synthesized in strong polar solvents, and this series of strong polar solvents often have the characteristics of high boiling point, easy decomposition at high temperature, and difficult to remove, so it is difficult to remove by devolatilization. Therefore, it is necessary to mix the solution with an inert solvent (miscible with the strong polar solvent and not miscible with the polymer) to make the polymer in the solution undergo phase change and precipitate to obtain the polymer. The precipitated polymer is in block form, so it is necessary to use a crushing equipment to break it into small pieces, flakes, particles or powders, and wash the crushed material with the corresponding inert solvent to wash away the residual solvent or other impurities, and then obtain the final product through drying, granulation and other steps. The polymers produced by this method include soluble polyimide (Ultem, Aurumn), sulfone polymers (PSU, PPSU, PES), ketone polymers (PEEK), polyphenylene sulfide (PPS), aromatic polyamide pulp (1313 or 1414), organic acid cellulose (cellulose acetate butyrate), PVDF, etc.
[0004] At present, in addition to the precipitation and crushing method, there are some other methods that can make the polymer in the special polymer solution precipitate, such as adding stirring to the solution and adding an inert solvent during stirring, such as the method for precipitating a sulfone polymer solution introduced in patent CN102888003A. However, the time for adding the inert solution to this method needs to be slow, because after the inert solvent is accelerated, the sulfone polymer will be precipitated into blocks. Moreover, the salt in the reaction process is dissolved by water and cannot be separated. Patent CN105330840A process introduces a method of crushing after cooling with a cooling belt, but does not mention a specific method.
[0005] Special polymers such as imide polymers, sulfone polymers, polyphenylene sulfide, polyetheretherketone, etc. have strong toughness and need to be crushed in a continuous cycle in the crushing equipment to achieve the expected crushing effect. Otherwise, if the crushed particles are too large, some impurities will be wrapped in them and cannot be removed, which will affect the product quality after drying and granulation. However, since the solution of such materials will immediately precipitate into strips after contacting the mutually soluble inert solvent, the solution will block the pipeline and equipment. Therefore, how to feed the material so that it can precipitate smoothly and can be crushed quickly without clogging the pipeline and equipment is the first step to solve this problem. However, if the particle size of the material after crushing is too large, the expected particle size effect cannot be achieved.
[0006] For wet grinding of materials, the morphology after grinding also affects the performance of the product. Usually, the bulk density of special polymers such as polysulfone and polyetherimide after grinding is relatively small, but the particles are large and the state is not uniform. In addition, the powder of special polymers is usually spherical after grinding. When this spherical powder is used to modify other materials, it is often unevenly mixed due to the deviation of its bulk density, especially when adding glass fiber and carbon fiber modification, the surface of the special polymer powder after adding glass fiber and carbon fiber can be clearly seen after granulation. The uneven traces on the surface. If the special polymer is crushed into a rod-like structure, the possibility of mutual connection will increase, so that the glass fiber, carbon fiber and the special polymer itself form good entanglement, which is beneficial to the uniformity after mixing. The traditional method of separating polymers from polar solvents is usually to first precipitate the solution through an inert solvent or roll it into a block object, then separate the solid by solid-liquid separation, and then use a wet grinder to grind it again, which is inefficient. Therefore, the problem we need to solve is how to solve the uneven size of the special polymer after crushing and prepare rod-shaped powder. Summary of the invention
[0007] The present invention provides a nucleating agent and a preparation method thereof and a preparation method of polymer rod-shaped ultrafine powder. Due to the use of the nucleating agent, a rod-shaped form can be easily formed during pulverization, and the particle size is small, so that the bulk density is higher than the bulk density of powder obtained by precipitation pulverization in other ways.
[0008] In order to achieve the above technical objectives, the technical solution adopted by the present invention is as follows:
[0009] The present invention provides a nucleating agent, the structural formula of which is as follows:
[0010]
[0011] Wherein, R' or R" are independently benzene ring, biphenyl, benzophenone or polyphenyl, polybenzophenone and their derivatives, preferably benzene ring; R represents an aliphatic hydrocarbon group of 2 to 4 carbon atoms, such as: -CH 2 -、-(CH2 ) 2 -、-(CH 2 ) 3 - etc.; X or Y represents halogen, preferably Cl, Br, X and Y may be the same or different.
[0012] The preparation method of the nucleating agent of the present invention comprises the following steps: reacting halogenated aromatic anhydride with aliphatic hydrocarbon diol.
[0013] As a preferred solution, the preparation method of the nucleating agent comprises the following steps: reflux halogenated aromatic anhydride and aliphatic hydrocarbon diol in a hydrocarbon solvent to generate water, azeotropically remove the water, evaporate the solvent, obtain a solid, and recrystallize.
[0014] In the preparation method of the nucleating agent of the present invention, the molar ratio of the halogenated aromatic anhydride to the aliphatic hydrocarbon diol is 2:1.
[0015] The halogenated aromatic anhydride of the present invention includes but is not limited to one or more of 4-chlorophthalic anhydride, 3-chlorophthalic anhydride, 3-bromophthalic anhydride, and 4-bromophthalic anhydride.
[0016] The aliphatic hydrocarbon diols of the present invention include, but are not limited to, one or more of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, and 1,4-butanediol.
[0017] The hydrocarbon solvent described in the present invention is one or more of aromatic hydrocarbons, aliphatic hydrocarbons or halogenated hydrocarbons with a boiling point above 170°C, including but not limited to n-decane, chloro-o-xylene (including 3-chloro-o-xylene and / or 4-chloro-o-xylene), dichlorobenzene, etc.
[0018] In the method for preparing the nucleating agent of the present invention, the reaction temperature is the reflux temperature of the solvent and the reaction time is 2 to 5 hours.
[0019] In the preparation method of the nucleating agent of the present invention, the mass ratio of the halogenated aromatic anhydride and the aliphatic hydrocarbon diol to the mass ratio of the hydrocarbon solvent is 1:2 to 1:20, preferably 1:3 to 1:8.
[0020] As a preferred scheme, the recrystallization of the present invention comprises the following steps: the solid is recrystallized with methanol or ethanol, and the alcohol mass to solid mass ratio is 5:1 to 20:1; the recrystallization time is 1 to 5 hours, and the temperature is 60 to 75°C; after recrystallization, it is filtered and vacuum dried to obtain a nucleating agent.
[0021] A method for preparing polymer rod-shaped ultrafine powder comprises the following steps: mixing a polymer, a nucleating agent and a solvent, precipitating and crushing.
[0022] As a preferred solution, the method for preparing the polymer rod-shaped ultrafine powder comprises the following steps: mixing a polymer solution of a polymer, a nucleating agent and a solvent with an inert solvent, precipitating the polymer, and then crushing it into a slurry to obtain the polymer rod-shaped ultrafine powder.
[0023] As a preferred solution, the preparation method of the polymer rod-shaped ultrafine powder comprises the following steps: a precipitation tank with stirring, a polymer solution feeding pipe and a high-speed pulverizing device are connected to form a circulating pulverizing system. An inert solvent is added to the precipitation tank. When the high-speed pulverizing device is turned on, the inert solvent circulates in the system, and a polymer solution of a polymer, a nucleating agent and a solvent is added to the inert solvent. When the polymer solution encounters the inert solvent, the polymer precipitates into a solid strip, enters the high-speed pulverizing device and is pulverized into a slurry; after the polymer solution is fed, the pulverizing is maintained in circulation.
[0024] When the bulk density of the powder wet material reaches 0.35 g / ml, the discharge valve and the solid-liquid separation equipment are opened during the continuous crushing process of the high-speed crushing equipment, and a part of the slurry is collected for solid-liquid separation to obtain polymer rod-shaped ultrafine powder, and the remaining slurry continues to be circulated and crushed.
[0025] In the method for preparing the polymer rod-shaped ultrafine powder of the present invention, the ratio of the extraction amount to the circulation amount is 1:49 to 1:3, preferably 1:20 to 1:10.
[0026] The polymers described in the present invention include but are not limited to imide polymers, sulfone polymers, ketone polymers, polyurethanes, aromatic polyamides, cellulose, fluoropolymers, etc., preferably polyetherimide, polysulfone, polyphenylsulfone, polyethersulfone, polyphenylene sulfide, polyetheretherketone, etc.
[0027] The solvent of the polymer solution of the present invention includes one or more of N,N-dimethylacetamide, N-methylpyrrolidone, sulfolane, dimethyl sulfoxide, N,N-dimethylformamide, acetic acid and butyric acid.
[0028] The mass ratio of the nucleating agent to the polymer of the present invention is 1:1000 to 5:1000.
[0029] The amount of the polymer solution and the inert solvent used in the present invention is based on the principle that the solid content of the pulverized slurry in the solid-liquid mixed system can make the solid-liquid mixed slurry flow smoothly, and the mass ratio is usually 1:2 to 1:20, preferably 1:3 to 1:8.
[0030] The inert solvent of the present invention is a solvent that can only be miscible with the solvent in the polymer solution but cannot dissolve the polymer, including but not limited to one or more of water, ethanol, methanol, isopropanol, toluene, and xylene, preferably water.
[0031] The equipment used in the high-speed pulverizing equipment of the present invention includes but is not limited to continuous wet pulverizing equipment such as a pulverizing pump, a colloid mill, a marine pulverizing pump, and a grinder.
[0032] After the nucleating agent with the above structure is added to the polymer solution of the present invention, the secondary structure of the polymer during precipitation can be changed, and the shape of the polymer after crushing can be changed into a rod shape.
[0033] In the present invention, the type and amount of the nucleating agent are the main factors affecting the morphology of the polymer after crushing.
[0034] The beneficial effects of the present invention are:
[0035] (1) This method uses a nucleating agent to achieve regular precipitation of the polymer and can realize continuous feeding and crushing. The precipitation and crushing processes can be solved by using one crushing equipment.
[0036] (2) The nucleating agent described in the present invention is dissolved in a solvent to form a uniform solution with the polymer, which can increase the softness of the precipitate and make it easier to form a rod-like shape when crushed.
[0037] (3) Due to the use of nucleating agents, the polymer is in an aggregated state during the precipitation process, making its bulk density higher than the bulk density of powders obtained by precipitation and crushing in other ways, making the obtained material powder convenient for subsequent washing and processing, and greatly reducing the volume. The powder particle size is also much smaller than the particle size obtained by other crushing methods. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 The rod-shaped powder of Example 1;
[0039] Figure 2 This is the state after crushing in Comparative Example 1;
[0040] Figure 3 This is the crushed state of Comparative Example 3;
[0041] Figure 4 This is the process flow chart of Example 1. DETAILED DESCRIPTION
[0042] Example 1
[0043] 1. Preparation of nucleating agent:
[0044] Add 182.5g of 4-chlorophthalic anhydride, 31g of ethylene glycol, and 427g of n-decane to a 5L reactor, heat to 175°C and reflux for 5 hours, and separate the water generated by the reaction during reflux. Turn on the vacuum, gradually reduce the vacuum degree to close to -0.1MPa, and evaporate the solvent. Cool to room temperature, add 888g of methanol to the reactor, recrystallize at 60°C for 5 hours, filter and vacuum dry to obtain a nucleating agent.
[0045]
[0046] Table 1 shows the absorption wavenumbers of characteristic groups of the infrared spectrum of the nucleating agent in Example 1.
[0047] Table 1
[0048]
[0049]
[0050] 2. Crushing process:
[0051] The mass ratio of nucleating agent to polysulfone particles with a diameter of 2 to 3 mm is 1:1000, which are dissolved in DMAC solution to obtain a 30 wt% polymer solution. Water is added to the precipitation tank and stirring is started. The high-speed crushing equipment (crushing pump) is turned on to circulate water, and the polymer solution is added for crushing. The ratio of the polymer solution feed flow rate to the water flow rate is 1:4, and the water flow rate is 5m 3 / h. When the polysulfone solution is added, the average particle size of the crushed powder is 10-50μm, and the bulk density of the wet material is 0.30g / ml. Close the feed valve b, and continue to circulate and crush for 30 minutes. The bulk density reaches 0.35g / ml, the average particle size is 5-35μm, and the product shape is rod-shaped. Open valve d, control the ratio of extraction volume to circulation volume to 1:49, and stop the crushing pump when all the crushed materials are discharged from the filtration equipment.
[0052] Example 2
[0053] 1. Preparation of nucleating agent:
[0054] In a 5L reactor, add 182.5g of 4-chlorophthalic anhydride, 38g of 1,2-propylene glycol, and 662g of a mixture of 3-chloro-o-xylene and 4-chloro-o-xylene (mass ratio 55:45), heat to 187°C and reflux for 2 hours, and separate the water generated by the reaction during reflux. Turn on the vacuum, gradually draw the vacuum degree to a state close to absolute pressure, and evaporate the solvent. Cool to room temperature, add 1476g of methanol to the reactor, recrystallize at 65°C for 4 hours, filter and vacuum dry to prepare a nucleating agent.
[0055]
[0056] 2. Crushing process:
[0057] The nucleating agent and polyamide-imide particles with a diameter of 2 to 3 mm were dissolved in NMP at a mass ratio of 2:1000 to obtain a 26 wt% polymer solution. Water was added to the precipitation tank and stirring was started. The crushing pump was turned on to circulate the water, and the polymer solution was added for crushing. The ratio of the polymer solution feed flow rate to the water flow rate was 1:3, and the water flow rate was 3m 3 / h. When all the polyamide-imide solution is added, the average particle size of the crushed powder is 12-53μm, and the bulk density of the wet material is 0.31g / ml. Close the feed valve b, and continue to crush for 30 minutes. The bulk density is 0.36g / ml, the average particle size is 5-35μm, and the product is in the shape of a rod. Open valve d, control the ratio of the extraction volume to the circulation volume to be 1:20, and stop the crushing pump when all the crushed materials are discharged from the filter equipment.
[0058] Example 3
[0059] 1. Preparation of nucleating agent:
[0060] Add 182.5g of 4-chlorophthalic anhydride, 38g of 1,3-propylene glycol, and 1103g of dichlorobenzene to a 5L reactor, heat to 180°C and reflux for 4 hours, and separate the water generated by the reaction during reflux. Turn on the vacuum, gradually reduce the vacuum degree to a state close to absolute pressure, and evaporate the solvent. Cool to room temperature, add 1845g of ethanol to the reactor, recrystallize at 70°C for 3 hours, filter and vacuum dry to obtain a nucleating agent.
[0061]
[0062] 2. Crushing process:
[0063] The nucleating agent and polyphenylsulfone particles with a diameter of 2 to 3 mm were dissolved in cyclopentane sulfone at a mass ratio of 3:1000 to prepare a 33 wt% polyphenylsulfone solution. Water was added to the precipitation tank and stirring was started. The crushing pump was turned on to circulate the water, and the polymer solution was added for crushing. The ratio of the polyphenylsulfone solution feed flow rate to the water flow rate was 1:8, and the water flow rate was 30m 3 / h. When all the polyphenylsulfone solution is added, the average particle size of the crushed powder is 15-55μm, and the bulk density of the wet material is 0.33g / ml. Close valve b, and continue to crush for 30 minutes. The bulk density is 0.37g / ml, the average particle size is 5-35μm, and the product state is rod-shaped. Open valve d, control the ratio of extraction volume to circulation volume to 1:15, and stop the crushing pump when all the crushed materials are discharged from the filtration equipment.
[0064] Example 4
[0065] 1. Preparation of nucleating agent:
[0066] Add 227g of 4-bromophthalic anhydride, 45g of 1,4-butanediol, and 2176g of a mixture of 3-chloro-o-xylene and 4-chloro-o-xylene (mass ratio 55:45) to a 10L reactor, heat to 187°C and reflux for 3 hours, and separate the water generated by the reaction during reflux. Turn on the vacuum, gradually reduce the vacuum degree to a state close to absolute pressure, and evaporate the solvent. Cool to room temperature, add 3450g of ethanol to the reactor, recrystallize at 70°C for 4 hours, filter and vacuum dry to prepare a nucleating agent.
[0067]
[0068] 2. Crushing process:
[0069] The nucleating agent and polyphenylene sulfide particles with a diameter of 2 to 3 mm were dissolved in cyclopentane sulfone at a mass ratio of 4:1000 to obtain a 33 wt% polyphenylene sulfide solution. Water was added to the precipitation tank and stirring was started. The wet grinder was started to circulate the water, and the polyphenylene sulfide solution was added for crushing. The feed flow rate of the polyphenylene sulfide solution and the water flow rate ratio were 1:2, and the water flow rate was 50m 3 / h. When all the polyphenylene sulfide solution is added, the average particle size of the crushed powder is 10-30μm, and the bulk density of the wet material is 0.40g / ml. Close the feed valve b, and continue to crush for 30 minutes. The bulk density is 0.55g / ml, the average particle size is 5-35μm, and the product state is rod-shaped. Open valve d, control the ratio of extraction volume to circulation volume to 1:15, and stop the grinder when all the crushed materials are released from the filtering equipment.
[0070] Example 5
[0071] 1. Preparation of nucleating agent:
[0072] In a 10L reactor, add 182.5g of 4-chlorophthalic anhydride, 38g of 1,2-propylene glycol, and 4410g of a mixture of 3-chloro-o-xylene and 4-chloro-o-xylene (mass ratio 55:45), heat to 187°C and reflux for 3 hours, and separate the water generated by the reaction during reflux. Turn on the vacuum, gradually draw the vacuum degree to a state close to absolute pressure, and evaporate the solvent. Cool to room temperature, add 3690g of ethanol to the reactor, recrystallize at 75°C for 4 hours, filter and vacuum dry to prepare a nucleating agent.
[0073]
[0074] 2. Crushing process:
[0075] The nucleating agent and polyethersulfone particles with a diameter of 2 to 3 mm were dissolved in NMP solution at a mass ratio of 5:1000 to obtain a 40 wt% polymer solution. Water was added to the precipitation tank and stirring was started. The grinder was turned on to circulate the water, and the polymer solution was added for crushing. The ratio of the polyethersulfone solution feed flow rate to the water flow rate was 1:20, and the water flow rate was 100m 3 / h. When all the polymer solution is added, the average particle size of the crushed powder is 10-30μm, and the bulk density of the wet material is 0.23g / ml. Close the feed valve b, and continue to crush for 30 minutes. The bulk density is 0.39g / ml, the average particle size is 8-45μm, and the product state is rod-shaped. Open valve d, control the ratio of extraction volume to circulation volume to 1:3, and stop the grinder when all the crushed materials are discharged from the filtering equipment.
[0076] Comparative Example 1: Non-circulating crushing
[0077] The nucleating agent of Example 1 and polysulfone resin particles with a diameter of 2 to 3 mm were dissolved in DMAC at a mass ratio of 1:1000 to obtain a 30 wt% polysulfone solution. Water was added to the precipitation tank and stirring was started. The crushing pump was turned on. The ratio of the polysulfone solution feed flow rate to the water flow rate was 1:4, and the water flow rate was 5m 3 / h. When the polysulfone solution precipitates and changes phase, the pulverized slurry directly enters the solid-liquid separation equipment. After all the polysulfone solution is added and pulverized, the solid-liquid separation equipment and the pulverizing pump are stopped to complete the entire pulverizing process.
[0078] The tested bulk density of the wet material is 0.050 g / ml and the average particle size is 2-5 mm.
[0079] This comparative example shows that the effect of one-time crushing is far inferior to that of multiple-cycle crushing.
[0080] Comparative Example 2: No nucleating agent added
[0081] The mass ratio of polysulfone particles with a diameter of 2 to 3 mm was 1:1000 and dissolved in DMAC solution to obtain a 30 wt% polymer solution. Water was added to the precipitation tank and stirring was started. The crushing pump was turned on to circulate water, and the polymer solution was added for crushing. The ratio of the polymer solution feed flow rate to the water flow rate was 1:4, and the water flow rate was 5m 3 / h. When the polysulfone solution is added, the average particle size of the crushed powder is 10-50μm, and the bulk density of the wet material is 0.09g / ml. Close the feed valve b, and continue to circulate and crush for 30 minutes. The bulk density reaches 0.10g / ml, the average particle size is 5-330μm, and the product shape is irregular. Open valve d, control the ratio of extraction volume to circulation volume to 1:49, and stop the crushing pump when all the crushed materials are discharged from the filtration equipment.
[0082] This comparative example shows that not adding a nucleating agent will change the pulverized morphology of the material and broaden the particle size distribution after pulverization.
[0083] Comparative Example 3: No enhancement effect with more nucleating agent
[0084] The nucleating agent of Example 1 and the polysulfone resin particles were dissolved in DMAC at a mass ratio of 20:1000 to obtain a 30 wt% polysulfone solution. Water was added to the precipitation tank and stirring was started. The crushing pump was turned on to circulate water, and the polysulfone solution was added for crushing. The ratio of the polysulfone solution feed flow rate to the water flow rate was 1:4, and the water flow rate was 5m 3 / h.
[0085] When the polysulfone solution is added, the average particle size of the powder after crushing is 10-50 μm, and the bulk density of the wet material is 0.30 g / ml. After closing the feed valve b and continuing the circulation crushing for 30 minutes, the bulk density reaches 0.35 g / ml, the average particle size is 5-35 μm, and the product shape is rod-shaped. Open valve d, control the ratio of the extraction amount and the circulation amount to 1:49, and stop the crushing pump when all the crushed materials are discharged from the filtering equipment. The results of this comparative example are consistent with those of Example 1, indicating that the addition of nucleating agent no longer has the effect of improving the crushing.
Claims
1. A nucleating agent, the structural formula of which is as follows: in, R' or R" is a benzene ring; R represents -CH 2 -、-(CH 2 ) 2 -、-(CH 2 ) 3 -; X or Y represents halogen, and X and Y are the same or different.
2. The nucleating agent according to claim 1, It is characterized in that X or Y represents Cl or Br, and X and Y may be the same or different.
3. A nucleating agent, the structural formula of which is as follows:
4. The method for preparing the nucleating agent according to claim 1 or 2, The following steps are involved: Reaction of halogenated aromatic anhydride and aliphatic chain hydrocarbon diol.
5. The method according to claim 4, It is characterized in that The molar ratio of the halogenated aromatic anhydride to the aliphatic chain hydrocarbon diol is 2:
1.
6. The method according to claim 4, It is characterized in that The halogenated aromatic anhydride is selected from one or more of 4-chlorophthalic anhydride, 3-chlorophthalic anhydride, 3-bromophthalic anhydride, and 4-bromophthalic anhydride; the aliphatic chain hydrocarbon diol is selected from one or more of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, and 1,4-butanediol.
7. A method for preparing polymer rod-shaped ultrafine powder, The following steps are involved: A polymer, a nucleating agent as claimed in claim 1 or 2 and a solvent are mixed, precipitated and crushed; the polymer comprises one or more of imide polymer, sulfone polymer, ketone polymer, polyurethane, aromatic polyamide, cellulose and fluoropolymer.
8. The method according to claim 7, It is characterized in that The following steps are involved: A polymer solution of a polymer, a nucleating agent and a solvent is mixed with an inert solvent, the polymer is precipitated, and then crushed into a slurry to obtain a polymer rod-shaped ultrafine powder.
9. The method according to claim 8, It is characterized in that The method comprises the following steps: a precipitation tank with stirring, a polymer solution feeding pipe and a high-speed pulverizing device are connected to form a circulating pulverizing system; an inert solvent is added into the precipitation tank, and when the high-speed pulverizing device is turned on, the inert solvent circulates in the system, a polymer solution of a polymer, a nucleating agent and a solvent is added into the inert solvent, and enters the high-speed pulverizing device to be pulverized into a slurry; after the polymer solution is fed, the circulating pulverizing is maintained.
10. The method according to claim 7, It is characterized in that The mass ratio of the nucleating agent to the polymer is 1:1000 to 5:1000.
11. The method according to claim 8, It is characterized in that The solvent includes one or more of N,N-dimethylacetamide, N-methylpyrrolidone, cyclopentane, dimethyl sulfoxide, N,N-dimethylformamide, acetic acid, butyric acid; the inert solvent includes one or more of water, ethanol, methanol isopropanol, toluene, and xylene.