A method for preparing graphene composite film at ultrafast speed

By growing graphyyne materials in situ on the porous base film, the problems of peeling and low flux in the synthesis of traditional graphyyne films are solved, and a high-throughput and stable graphyyne composite film is achieved, which is suitable for a variety of organic small molecules Efficient separation.

CN115869785BActive Publication Date: 2024-11-26BEIJING UNIV OF CHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211559923.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-06
Publication Date
2024-11-26
Estimated Expiration
2042-12-06

AI Technical Summary

Technical Problem

The synthesis method of traditional graphyne films requires peeling from the substrate, affecting performance, and the prepared film has a small lateral size, which limits its application, and has low flux and poor stability, making it difficult to meet the needs of efficient separation.

Method used

Chemical modification is performed using porous base film, and the surface of the base film is made of amino active groups by terminal aminosilane coupling agent or dopamine, and small alkynyl molecules are grafted, and graphiteyne materials are grown in situ on the surface of the porous base film to form Selective separation of the layers, using alkynyl monomer and catalyst to react at a specific temperature, and quickly grow graphyyne thin films.

Benefits of technology

A high-throughput, stable graphyne composite film has high retention and permeability. It is suitable for the separation of various organic small molecules in water, and has a short growth time, which is suitable for molecular screening of different molecular weights.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003984255510000011
    Figure HDA0003984255510000011
  • Figure HDA0003984255510000012
    Figure HDA0003984255510000012
  • Figure HDA0003984255510000013
    Figure HDA0003984255510000013
Patent Text Reader

Abstract

The invention discloses an ultrafast preparation method of a graphene composite membrane, belonging to the field of membrane separation technology. The method ultrafast synthesizes a graphene membrane on the surface of an alkyne-modified porous substrate, wherein the graphene composite membrane comprises a porous base membrane and a graphene material selective separation layer in situ grown on the surface of the porous base membrane; the graphene material is graphdiyne generated by coupling an alkyne monomer on an alkyne-modified substrate. The surface of the porous base membrane is chemically modified by using an amino-terminated silane coupling agent or dopamine, and then grafted with an alkyne-containing small molecule organic substance that can react with an amino group to obtain an alkyne-deposited porous base membrane; the alkyne-deposited porous base membrane is immersed in a monomer and catalyst mixed solution of the synthetic graphene material, reacted, and a high-throughput graphene composite membrane is obtained at high temperature for 15 minutes. The composite membrane prepared by the invention has a high rejection rate for a variety of organic small molecules in water and good molecular sieving performance of molecules with different molecular weights (molecular weight <400 and molecular weight >700), and has a high permeation flux.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of membrane separation, and in particular relates to a high-throughput graphyne composite membrane and an ultrafast preparation method thereof. Background Art

[0002] As a new type of efficient separation technology, membrane separation technology has shown superior performance in seawater desalination, wastewater treatment, drug separation, domestic water softening, etc. with its energy-saving and environmentally friendly characteristics. The separation performance of the membrane mainly depends on the properties of the membrane material itself and the structural morphology of the membrane. In view of the shortcomings of traditional nanofiltration membranes such as low flux, poor stability and short service life, the development of new membrane materials is still a key issue that needs to be solved.

[0003] As a new type of porous nanomaterial, graphyne has intrinsically uniform and easily controllable pores. These pores are usually formed by acetylene bonds of a certain length connecting benzene rings or acetylene groups in graphyne units. The shape and size of the pores vary due to the different arrangements of acetylene and phenyl groups and the number of acetylene bonds. These structural features make graphyne an ideal material for preparing high-precision molecular separation membranes, and it has broad application prospects in water treatment, drug separation, and gas separation. At present, most graphyne synthesized by in-situ polymerization uses copper foil as a substrate and catalyst. The graphyne synthesized by this method needs to be peeled off from the substrate. The peeling process will have a great impact on the performance of graphyne, and the lateral size of the obtained graphyne film is small, only at the micron level, which greatly limits the application of graphyne products. Summary of the invention

[0004] The key technical problem to be solved by the present invention is to provide an ultrafast preparation method for a large-area graphyne composite membrane. The prepared graphyne membrane does not need to be peeled off from a substrate, has a high retention rate for a variety of small organic molecules in water, and has good molecular sieving performance with different molecular weights (molecular weight <400 and molecular weight >700), and has a very high permeability flux.

[0005] The specific technical solutions are as follows:

[0006] In a first aspect, the present invention provides a high-throughput graphyne composite membrane, comprising a porous base membrane and a graphyne material selective separation layer in-situ grown on the surface of the porous base membrane;

[0007] The Graphdiyne material is graphene diyne, which has extremely strong stability in water, acid, alkali, salt and organic solvent.

[0008] Preferably, the graphyne monomer includes one or more of 1,3,5-triethynylbenzene, hexaethynylbenzene, 1,3,5-tri-(4-ethynylphenyl)benzene, triethynyl boron, tri(4-ethynylphenyl)amine, tetra(4-ethynylphenyl)ethylene, 1,3,5-trichloro-2,4,6-triethynylbenzene, 2,4,6-triethynyl-1,3,5-triazine or 3,4-diethynylhexa-3-ene-1,5-diyne.

[0009] Specifically, the thickness of the graphyne material selective separation layer is 100nm to 400nm.

[0010] Specifically, the porous base membrane is selected from an organic polymer membrane, an inorganic membrane or an organic / inorganic hybrid membrane, and has an average pore size of 0.01-100 μm.

[0011] Specifically, the porous base membrane may be in the form of a flat plate, a tube or a hollow fiber.

[0012] In a second aspect, the present invention provides an ultrafast preparation method of a Graphene Oxide Composite Film, comprising:

[0013] Step a, chemically modifying the surface of the porous base film with an amino-terminated silane coupling agent or dopamine to provide the base film with amino-active groups, and then grafting small molecules with alkynyl groups that can react with amino groups to obtain a functional porous base film with an alkynyl-based layer deposited;

[0014] Step b, dissolving a certain amount of acetylene monomer in a solvent, and adding a certain amount of catalyst powder, stirring and ultrasonically treating, to prepare a mixed solution of graphene monomer and catalyst; immersing the porous base film on which the acetylene layer is deposited in step a in the above mixed solution, and reacting at a certain temperature for 15 minutes to 6 hours, so that the graphene diacetylene material can fully grow on the surface of the porous base film.

[0015] Specifically, the method of chemically modifying the surface of the porous base film using a terminal amino silane coupling agent in step a is preferably as follows: immersing the porous base film in a toluene solution of a terminal amino silane coupling agent having a concentration of 0.1-1 mM, reacting at 100-150° C. for 1-3 hours after passing nitrogen or argon protection; the terminal amino silane coupling agent is selected from γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, N-β (aminoethyl)-γ-aminopropylmethoxydimethoxysilane, N-β (aminoethyl) )-γ-aminopropyltriethoxysilane, N-β (aminoethyl)-γ-aminopropylmethoxydiethoxysilane, anilinomethyltriethoxysilane, anilinomethyltrimethoxysilane, aminoethylaminoethylaminopropyltrimethoxysilane, and polyaminoalkyltrialkylsilane; the use of dopamine to treat the surface of the porous base membrane is preferably: the porous base membrane is immersed in a 0.1-0.5wt.% dopamine aqueous solution, and the pH value is adjusted to 8.5 with Tris-HCl (trihydroxymethylaminomethane), and the reaction is carried out at room temperature for 4-24h.

[0016] Specifically, the grafted alkynyl small molecule that reacts with the amino group in step a is selected from one or more of 4-ethynylbenzaldehyde, 3-ethynylbenzaldehyde, 2-ethynylbenzaldehyde, 5-ethynylisophthalic acid, 4-ethynylbenzoic acid, 3,5-diethynylbenzoic acid, 3-ethynylbenzoic acid, 2-ethynylbenzoic acid, 3-ethynyl-4-methylbenzoic acid, and 2-chloro-4-ethynylbenzoic acid. The porous base film after surface amination is immersed in a toluene solution of the alkynyl small molecule that reacts with the amino group at a concentration of 5-50 mg / 10 ml, and reacted at 100-150° C. for 1-3 hours.

[0017] Specifically, in the monomer solution of the graphyne material described in step b, the acetylenic monomer is selected from one or more of 1,3,5-triethynylbenzene, hexaethynylbenzene, 1,3,5-tri-(4-ethynylphenyl)benzene, triethynyl boron, tri(4-ethynylphenyl)amine or tetra(4-ethynylphenyl)ethylene.

[0018] Specifically, the concentration of the acetylenic monomer is 0.4-5 mg / ml; the solvent is selected from one of methanol, ethanol, n-propanol, isopropanol, n-octanol, isooctyl alcohol, n-hexane, n-heptane, N,N-dimethylformamide, and N-methylpyrrolidone.

[0019] Specifically, the catalyst in step b is selected from one or more of cupric acetate and cupric chloride.

[0020] Preferably, the reaction temperature of the acetylenic monomer in the solvent in step b is 25°C-150°C.

[0021] The application of the graphene composite membrane of the present invention is used for nanofiltration of pollutants, or for separation and screening of molecular sieves with different molecular weights, i.e., molecular weight <400 and molecular weight >700.

[0022] The technical solution provided by the present invention has the following beneficial effects: the method provided by the present invention rapidly grows graphene material in situ on an alkyne-modified porous base film and forms a dense separation layer. Since the structure of the graphene material is stable and the two-dimensional sheet itself has a regular pore structure, the separation layer formed is ultra-thin (about 100nm) and has a uniform pore size (0.6-1.7nm). The pore size in this range can selectively separate many small organic molecules in water, such as dye molecules, drug molecules, etc., and the permeation flux of the membrane is 5-6 times higher than that of a traditional polyamide nanofiltration membrane. In addition, the method of the present invention is extremely time-consuming, and only 15 minutes are needed at high temperature for the graphene film to be uniformly grown on a variety of substrate surfaces. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 . Surface scanning electron microscopy image of the high-throughput tubular Graphene Dyne (GDY) composite membrane prepared in Example 1 of the present invention (ethanol as solvent, reaction at 110°C for 15 minutes).

[0024] Figure 2 . Surface scanning electron microscopy image of the high-throughput tubular Graphene Dyne (GDY) composite membrane prepared in Example 2 of the present invention (ethanol as solvent, reaction at 110°C for 30 minutes).

[0025] Figure 3 . Surface scanning electron microscopy image of the high-throughput tubular Graphene Dyne (GDY) composite membrane prepared in Example 3 of the present invention (ethanol as solvent, reaction at 110°C for 1h).

[0026] Figure 4 .Scanning electron microscope image of the cross section of the high-throughput tubular Graphene Dyne (GDY) composite membrane prepared in Example 1 of the present invention (ethanol as solvent, reaction at 110°C for 15 minutes). DETAILED DESCRIPTION

[0027] To make the purpose, technical solution and advantages of the present invention clearer, the embodiments of the present invention will be described in further detail below in conjunction with the accompanying drawings, but the present invention is not limited to the following embodiments. The scanning electron microscope images were observed and measured using a ZEISS 300 scanning electron microscope (SEM).

[0028] In a first aspect, an embodiment of the present invention provides a high-throughput graphyne composite membrane, comprising a porous base membrane and a graphyne material selective separation layer grown on the surface of the porous base membrane;

[0029] The Graphdiyne material is graphene diyne, which has extremely strong stability in water, acid, alkali, salt and organic solvent.

[0030] Preferably, the graphyne monomer includes one or more of 1,3,5-triethynylbenzene, hexaethynylbenzene, 1,3,5-tri-(4-ethynylphenyl)benzene, triethynyl boron, tri(4-ethynylphenyl)amine, tetra(4-ethynylphenyl)ethylene, 1,3,5-trichloro-2,4,6-triethynylbenzene, 2,4,6-triethynyl-1,3,5-triazine or 3,4-diethynylhexa-3-ene-1,5-diyne.

[0031] Specifically, the thickness of the graphyne material selective separation layer is 100nm to 400nm.

[0032] Specifically, in the embodiment of the present invention,

[0033] In a second aspect, the present invention provides an ultrafast preparation method of a Graphene Oxide Composite Film, comprising:

[0034] Step 101, chemically modifying the surface of the porous base film with an amino-terminated silane coupling agent or dopamine to make the surface of the base film have amino-active groups, and then grafting small molecules with alkynyl groups that can react with amino groups to obtain a functional porous base film with an alkynyl-based layer deposited;

[0035] Step 102, dissolving a certain amount of acetylene monomer in a solvent, and adding a certain amount of catalyst powder, stirring and ultrasonically treating, to prepare a mixed solution of graphene monomer and catalyst; immersing the porous base membrane on which the acetylene layer is deposited in step a in the monomer catalyst solution, and reacting at a certain temperature for 15 minutes to 6 hours, so that the graphene diacetylene material can fully grow on the surface of the porous base membrane.

[0036] Specifically, in step 101, chemically modifying the surface of the porous base membrane using an amino-terminated silane coupling agent means: immersing the porous base membrane in a toluene solution of the amino-terminated silane coupling agent at a concentration of 0.1-1 mM, reacting at 100-150° C. for 1-3 hours under nitrogen or argon protection; wherein the concentration of the amino-terminated silane coupling agent can be 0.1 mM, 0.3 mM, 0.5 mM, 0.7 mM, 1 mM, the reaction temperature can be 100° C., 110° C., 120° C., 130° C., 140° C., 150° C., and the reaction time can be 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours; such a setting can ensure that the aminosilane coupling agent fully reacts with the base membrane, and a layer of amino groups is uniformly grafted on the surface of the base membrane, which is beneficial to the subsequent growth of the covalent organic skeleton separation layer.

[0037] Specifically, the terminal amino silane coupling agent includes γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, N-β (aminoethyl)-γ-aminopropylmethoxydimethoxysilane, N-β (aminoethyl)-γ-aminopropyltriethoxysilane, N-β (aminoethyl)-γ-aminopropylmethoxydiethoxysilane, anilinomethyltriethoxysilane, anilinomethyltrimethoxysilane, aminoethylaminoethylaminopropyltrimethoxysilane, and polyaminoalkyltrialkylsilane.

[0038] Specifically, in step 101, treating the surface of the porous base membrane with dopamine means: immersing the porous base membrane in a 0.1-0.5wt.% dopamine aqueous solution, adjusting the pH value to 8.5 with Tris-HCl (trishydroxymethylaminomethane), and reacting at room temperature for 4-24h; wherein the dopamine concentration can be 0.1wt.%, 0.2wt.%, 0.3wt.%, 0.4wt.%, 0.5wt.%, and the reaction time at room temperature can be 4h, 8h, 12h, 16h, 20h, 24h. Under these conditions, the polymerized dopamine can be evenly distributed on the surface of the base membrane, which is conducive to the subsequent growth of the graphyne separation layer.

[0039] Specifically, the grafting of alkynyl-containing small molecule organic matter in step 101 refers to: immersing the porous base membrane after surface amination in a toluene solution containing alkynyl small molecules that react with amino groups at a concentration of 10-50 mg / 10 ml, and reacting at 100-150° C. for 1-3 hours; wherein the concentration of the alkynyl small molecule organic matter can be 5 mg / 10 ml, 15 mg / 10 ml, 25 mg / 10 ml, 35 mg / 10 ml, 50 mg / 10 ml, the reaction temperature can be 100° C., 110° C., 120° C., 130° C., 140° C., 150° C., and the reaction time can be 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours; such an arrangement can make the alkynyl small molecule organic matter uniformly grafted to the surface of the base membrane, so that the subsequent graphene material can grow uniformly on the surface of the base membrane.

[0040] Preferably, the small molecule containing an alkynyl group that reacts with an amino group includes one or more of 4-ethynylbenzaldehyde, 3-ethynylbenzaldehyde, 2-ethynylbenzaldehyde, 5-ethynylisophthalic acid, 4-ethynylbenzoic acid, 3,5-diethynylbenzoic acid, 3-ethynylbenzoic acid, 2-ethynylbenzoic acid, 3-ethynyl-4-methylbenzoic acid, and 2-chloro-4-ethynylbenzoic acid.

[0041] Specifically, in the monomer solution of the graphyne material described in step 102, the acetylene monomer is selected from one or more of 1,3,5-triethynylbenzene, hexaethynylbenzene, 1,3,5-tri-(4-ethynylphenyl)benzene, triethynyl boron, tri(4-ethynylphenyl)amine, tetra(4-ethynylphenyl)ethylene, 1,3,5-trichloro-2,4,6-triethynylbenzene, 2,4,6-triethynyl-1,3,5-triazine or 3,4-diethynylhexa-3-ene-1,5-diyne; the concentration of the acetylene monomer is 0.4-5 mg / ml, and the specific concentration can be 0.4 mg / ml, 0.8 mg / ml. ml, 1mg / ml, 2mg / ml, 3mg / ml, etc., to ensure that the graphene film grows fully on the surface of the base film to form a dense and defect-free selective separation layer; the solvent is selected from one of methanol, ethanol, n-propanol, isopropanol, n-octanol, isooctyl alcohol, n-hexane, n-heptane, N,N-dimethylformamide, and N-methylpyrrolidone; the catalyst is selected from one of copper acetate and copper chloride, and the concentration of the catalyst is 0.2-1g / L, and the specific concentration can be 0.2g / L, 0.4g / L, 0.6g / L, 0.8g / L, 1g / L, so that the acetylenic monomer has a suitable reaction rate in the solvent.

[0042] Preferably, the reaction temperature of the acetylenic monomer in the solvent in step 102 is 25°C-150°C, specifically 40°C, 60°C, 80°C, 100°C, 120°C, 140°C.

[0043] The present invention will be further described below through specific examples.

[0044] In the following specific examples, the operations involved, if the conditions are not specified, are all carried out under conventional conditions or conditions recommended by the manufacturer. The raw materials used, if the manufacturers and specifications are not specified, are all conventional products that can be obtained from the market.

[0045] Example 1

[0046] A tubular ceramic (Al2O3) porous base membrane is used, and the average pore size and porosity of the base membrane are 0.1 μm and 40% respectively; and terminal amino silane coupling agent γ-aminopropyltriethoxysilane is selected to chemically modify the base membrane.

[0047] Step a, immersing the tubular ceramic base membrane in a toluene solution of an amino-terminated silane coupling agent with a concentration of 1 mM, reacting at 110° C. for 2 hours under argon protection, so that the base membrane surface has amino active groups; then immersing the amination-treated porous base membrane in a toluene solution of 4-ethynylbenzaldehyde with a concentration of 1 mg / ml, and reacting at 110° C. for 2 hours to obtain a porous base membrane with alkynyl deposition;

[0048] Step b, dissolving 10 mg of triacetylene benzene and 15 mg of cupric acetate in 25 ml of ethanol, stirring and ultrasonically treating to prepare a monomer-catalyst mixed solution; vertically immersing the functionalized tubular ceramic base membrane in step a in the prepared monomer-catalyst solution, and reacting at 110° C. for 15 min, and naturally cooling to room temperature to allow graphyne to fully grow on the surface of the porous base membrane.

[0049] SEM photos ( Figure 1 ) shows that the surface of the tubular Graphene Oxide composite membrane is dense, without pinholes and intercrystalline defects, and the thickness of the selective separation layer is about 100nm ( Figure 4 ).

[0050] The prepared composite membrane was placed in a dye removal device for performance testing. The test conditions were as follows: (1) the stock solution composition was 0.1 g / L chrome black T water system, (2) the stock solution composition was 0.1 g / L acid fuchsin water system, (3) the stock solution composition was 0.1 g / L Congo red water system, (4) the stock solution composition was 0.1 g / L methyl blue water system, (5) the stock solution composition was 0.1 g / L Bengal rose red water system, (6) the stock solution composition was 0.1 g / L / L Coomassie Brilliant Blue water system, (7) the stock solution composition is 0.1g / L direct black system, (8) the stock solution composition is 0.1g / L active black water system, (9) the stock solution composition is 0.1g / L Alcin blue water system, (10) the stock solution composition is 0.1g / L methyl orange and 0.1g / L methyl blue water system, (11) the stock solution composition is 0.1g / L methyl orange and 0.1g / L Alcin blue water system, and the operating pressure is 0.2MPa.

[0051] The performance of the composite membrane was measured as follows: (1) the retention rate of chrome black T was 98.68%, and the permeation flux was 602 L / (m 2 h MPa); (2) The acid fuchsin rejection rate was 95.75%, and the permeation flux was 465 L / (m 2 h MPa); (3) Congo red rejection rate is 99.82%, and the flux is 780L / (m 2 h MPa); (4) the retention rate of methyl blue is 99.52%, and the flux is 650L / (m 2 hMPa); (5) The retention rate of Bengal rose red is 99.63%, and the flux is 455L / (m 2 h MPa); (6) Coomassie brilliant blue rejection rate is 99.78%, and the flux is 690L / (m 2 h MPa); (7) the direct black rejection rate is 98.17%, and the permeation flux is 635L / (m 2 h MPa); (8) The active black retention rate is 98.61%, and the permeation flux is 658L / (m 2h MPa); (9) The retention rate of Alcian Blue is 99.42%, and the flux is 1100 L / (m 2 h MPa); (10) the methyl orange retention rate is 18.53%, the methyl blue retention rate is 98.87%, and the permeation flux is 675 L / (m 2 h MPa), the separation ratio was 72.1; (11) the methyl orange retention rate was 17.75%, the alician blue retention rate was 99.33%, and the permeation flux was 1050 L / (m 2 h MPa), the separation ratio is 122.8.

[0052] Example 2

[0053] A tubular ceramic (Al2O3) porous base membrane is used, and the average pore size and porosity of the base membrane are 0.1 μm and 40% respectively; and terminal amino silane coupling agent γ-aminopropyltriethoxysilane is selected to chemically modify the base membrane.

[0054] Step a, immersing the tubular ceramic base membrane in a toluene solution of an amino-terminated silane coupling agent with a concentration of 1 mM, reacting at 110° C. for 2 hours under argon protection, so that the base membrane surface has amino active groups; then immersing the amination-treated porous base membrane in a toluene solution of 4-ethynylbenzaldehyde with a concentration of 3 mg / ml, and reacting at 110° C. for 2 hours to obtain a porous base membrane with alkynyl deposition;

[0055] Step b, dissolving 15 mg of copper acetate and 10 mg of triacetin in 25 ml of ethanol, stirring and ultrasonically treating to prepare a monomer catalyst solution; vertically immersing the functionalized tubular ceramic base membrane in step a in the prepared monomer catalyst solution, reacting at 110° C. for 30 minutes, and naturally cooling to room temperature to allow graphyne to fully grow on the surface of the porous base membrane.

[0056] The prepared composite membrane was placed in a dye removal device for performance testing. The test conditions were: (1) the stock solution composition was 0.1 g / L chrome black T water system, (2) the stock solution composition was 0.1 g / L Congo red water system, (3) the stock solution composition was 0.1 g / L methyl blue water system, and the operating pressure was 0.2 MPa.

[0057] The performance of the composite membrane was measured as follows: (1) the retention rate of chrome black T was 98.92% and the permeation flux was 535 L / (m 2 h MPa); (2) Congo red rejection rate is 98.92%, and the flux is 604L / (m 2 h MPa); (3) the retention rate of methyl blue was 99.45%, and the flux was 540 L / (m 2 h MPa).

[0058] Example 3

[0059] A tubular ceramic (Al2O3) porous base membrane is used, and the average pore size and porosity of the base membrane are 0.1 μm and 40% respectively; and terminal amino silane coupling agent γ-aminopropyltriethoxysilane is selected to chemically modify the base membrane.

[0060] Step a, immersing the tubular ceramic base membrane in a toluene solution of an amino-terminated silane coupling agent with a concentration of 1 mM, reacting at 110° C. for 2 hours under argon protection, so that the base membrane surface has amino active groups; then immersing the amination-treated porous base membrane in a toluene solution of 4-ethynylbenzaldehyde with a concentration of 3 mg / ml, and reacting at 110° C. for 2 hours to obtain a porous base membrane with alkynyl deposition;

[0061] Step b, dissolving 15 mg of copper acetate and 10 mg of triacetin in 25 ml of ethanol, stirring and ultrasonically treating to prepare a monomer catalyst solution; vertically immersing the functionalized tubular ceramic base membrane in step a in the prepared monomer catalyst solution, reacting at 110° C. for 1 hour, and naturally cooling to room temperature to allow graphyne to fully grow on the surface of the porous base membrane.

[0062] The prepared composite membrane was placed in a dye removal device for performance testing. The test conditions were: the stock solution composition was a 0.1 g / L methyl blue water system, and the operating pressure was 0.2 MPa.

[0063] The performance of the composite membrane was measured as follows: the methyl blue rejection rate was 99.53%, and the permeation flux was 158 L / (m 2 h MPa).

[0064] Example 4

[0065] A tubular ceramic (Al2O3) porous base membrane is used, and the average pore size and porosity of the base membrane are 0.1 μm and 40% respectively; and terminal amino silane coupling agent γ-aminopropyltriethoxysilane is selected to chemically modify the base membrane.

[0066] Step a, immersing the tubular ceramic base membrane in a toluene solution of an amino-terminated silane coupling agent with a concentration of 1 mM, reacting at 110° C. for 2 hours under argon protection, so that the base membrane surface has amino active groups; then immersing the amination-treated porous base membrane in a toluene solution of 4-ethynylbenzaldehyde with a concentration of 3 mg / ml, and reacting at 110° C. for 2 hours to obtain a porous base membrane with alkynyl deposition;

[0067] Step b, dissolving 15 mg of copper acetate and 10 mg of triacetin in 25 ml of ethanol, stirring and ultrasonically treating to prepare a monomer catalyst solution; vertically immersing the functionalized tubular ceramic base membrane in step a in the prepared monomer catalyst solution, and reacting at 60° C. for 3 hours, and naturally cooling to room temperature to allow graphyne to fully grow on the surface of the porous base membrane.

[0068] The prepared composite membrane was placed in a dye removal device for performance testing. The test conditions were: the stock solution composition was a 0.1 g / L methyl blue water system, and the operating pressure was 0.2 MPa.

[0069] The performance of the composite membrane was measured as follows: the methyl blue rejection rate was 99.42%, and the permeation flux was 638 L / (m 2 h MPa).

[0070] The above description is only a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. An ultrafast preparation method of a Graphene Oxide Composite Film, characterized in that: A method for ultrafast synthesis of a graphene film on the surface of an alkyne-treated porous substrate, wherein the graphene composite membrane comprises a porous substrate membrane and a graphene material selective separation layer in situ grown on the surface of the porous substrate membrane; the graphene material is graphdiyne; The specific steps include: Step a, chemically modifying the surface of the porous base film with an amino-terminated silane coupling agent or dopamine to provide the base film with amino-active groups, and then grafting small molecules with alkynyl groups that can react with amino groups to obtain a functional porous base film with an alkynyl-based layer deposited; Step b, dissolving a certain amount of acetylene monomer in a solvent, adding a certain amount of catalyst powder, stirring and ultrasonically treating, to prepare a mixed solution of graphene monomer and catalyst; immersing the porous base film on which the acetylene layer is deposited in step a in the mixed solution, and reacting at a certain temperature for 15 min-6 h, so that the graphene material is fully grown on the surface of the porous base film; The method of chemically modifying the surface of the porous base film by using an amino-terminated silane coupling agent as described in step a is as follows: immersing the porous base film in a toluene solution of an amino-terminated silane coupling agent having a concentration of 0.1-1 mM, reacting at 100-150° C. for 1-3 hours after passing nitrogen or argon protection; the amino-terminated silane coupling agent is selected from one or more of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, N-β (aminoethyl)-γ-aminopropylmethoxydimethoxysilane, N-β (aminoethyl)-γ-aminopropyltriethoxysilane, N-β (aminoethyl)-γ-aminopropylmethoxydiethoxysilane, anilinomethyltriethoxysilane, anilinomethyltrimethoxysilane, aminoethylaminoethylaminopropyltrimethoxysilane, and polyaminoalkyltrialkylsilane; The dopamine is used to treat the surface of the porous base membrane: the porous base membrane is immersed in a 0.1-0.5wt.% dopamine aqueous solution, and the pH value is adjusted to 8.5 with Tris-HCl (trishydroxymethylaminomethane), and the reaction is carried out at room temperature for 4-24 hours; The small molecule with alkynyl group that is grafted and reacts with amino group in step a is selected from one or more of 4-ethynylbenzaldehyde, 3-ethynylbenzaldehyde, 2-ethynylbenzaldehyde, 5-ethynylisophthalic acid, 4-ethynylbenzoic acid, 3,5-diethynylbenzoic acid, 3-ethynylbenzoic acid, 2-ethynylbenzoic acid, 3-ethynyl-4-methylbenzoic acid, and 2-chloro-4-ethynylbenzoic acid; the porous base film after surface amination is immersed in a toluene solution of the small molecule with alkynyl group that reacts with amino group at a concentration of 5-50 mg / 10 ml, and reacted at 100-150° C. for 1-3 hours; In step b, the reaction temperature of the acetylenic monomer in the solvent is 25°C-150°C.

2. The method according to claim 1, characterized in that The thickness of the graphyne material selective separation layer is 5nm to 500nm.

3. The method according to claim 1, characterized in that The porous base membrane is selected from an organic polymer membrane, an inorganic membrane or an organic / inorganic hybrid membrane, and has an average pore size of 0.01-100 μm.

4. The method according to claim 1, characterized in that The porous base membrane is in the shape of a flat plate, a tube or a hollow fiber.

5. The method according to claim 1, characterized in that In the alkynyl monomer solution of the graphene material described in step b, the alkynyl monomer is selected from one or more of 1,3,5-triethynylbenzene, hexaethynylbenzene, 1,3,5-tri-(4-ethynylphenyl)benzene, triethynyl boron, tri(4-ethynylphenyl)amine, tetra(4-ethynylphenyl)ethylene, 1,3,5-trichloro-2,4,6-triethynylbenzene, 2,4,6-triethynyl-1,3,5-triazine or 3,4-diethynylhexa-3-ene-1,5-diyne; the concentration of the alkynyl monomer is 0.4-5 mg / ml; the solvent is selected from one of methanol, ethanol, n-propanol, isopropanol, n-octanol, isooctyl alcohol, n-hexane, n-heptane, N,N-dimethylformamide and N-methylpyrrolidone.

6. A graphene composite film prepared according to the method according to any one of claims 1 to 5.