A method for granulating gas adsorption material particles at room temperature and its application

By mixing solvents with binders and gas adsorbent powder at room temperature, granulation forms high porosity and high-strength gas adsorbent material particles, solving the problems of material instability and performance changes caused by high-temperature sintering, and broadening adsorption The application range of materials and improves oxygen absorption capacity.

CN115869910BActive Publication Date: 2024-11-12EXTREME PURE MATERIALS TECHNOLOGY (JIANGSU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211695378.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-28
Publication Date
2024-11-12
Estimated Expiration
2042-12-28

AI Technical Summary

Technical Problem

The granulation method of existing gas adsorption materials requires high-temperature sintering, which leads to unstable materials at high temperatures and cannot be suitable for certain adsorbed materials. The volatility of the adhesive during granulation process leads to changes in the material properties.

Method used

The solvent and the binder are mixed at room temperature, stir evenly and merged with the gas adsorbent material powder, and granulated through the particle forming equipment to avoid high temperature treatment, forming gas adsorbent material particles with porosity and mechanical high strength.

Benefits of technology

The high porosity and mechanical strength of granulated gas adsorbent materials at room temperature are achieved, the scope of use of unstable adsorbent materials is broadened, the performance changes caused by high temperature treatment are avoided, and the oxygen absorption capacity and convenience of adsorbent materials are improved. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115869910B_ABST
    Figure CN115869910B_ABST
Patent Text Reader

Abstract

The present invention provides a method for granulating gas adsorbent material particles at room temperature, comprising the following steps: first, mixing a solvent with a binder to fully dissolve the binder to form a mixed solution 1; combining the mixed solution 1 and gas adsorbent material powder, stirring evenly, and granulating at room temperature through a particle forming device, and obtaining the gas adsorbent material particles after the solvent in the particles is completely volatilized. The present invention can complete granulation at room temperature, the method is simple and easy to operate, the granulation conditions are mild, and the temperature in ordinary granulation methods is avoided to be too high, and the particles obtained by granulation are formed and not easy to pulverize. The present invention also provides an application of a method for granulating gas adsorbent material particles at room temperature. The present invention is suitable for the granulation of gas adsorbent materials that are unstable at high temperatures, and is also suitable for the molding preparation of multi-component gas adsorbent material particles. The present invention also provides gas adsorbent material particles obtained by granulation by this method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of gas adsorption materials, and relates to a room-temperature granulation method for gas adsorption material particles and application thereof, as well as gas adsorption material particles obtained by granulation. Background Art

[0002] The raw materials of gas adsorption materials are usually in powder form. Since the gas passing through the powder will generate great resistance, it cannot be used directly. The powder needs to be made into granules so that the gas can pass through the gaps between the particles, greatly reducing wind resistance. Adsorption materials are used to adsorb gas. In order to make full use of the adsorption materials, the gas needs to be able to diffuse quickly into the particles. Therefore, the particles of gas adsorption materials need to contain many evenly distributed micropores so that the gas can diffuse into the entire particle. However, these micropores will reduce the strength of the particles. Therefore, the current granulation process of gas adsorption materials is to sinter the powder and the binding material at high temperature. The high-temperature sintering allows chemical bonds to be formed between the adsorption material particles and the binding material. The sintering process is used for granulation of molecular sieves, activated carbon, alumina, etc.

[0003] In patent CN 114849646 A "A modified gasification ash activated carbon adsorption material", the granulated material is pyrolyzed and carbonized in an internal heating rotary kiln at a pyrolysis temperature of 400°C, and then water vapor and carbon dioxide are used as activation media to activate the carbonized material in a multi-stage rake furnace. The activation temperature is controlled between 800-850°C to obtain activated carbon particles. In patent CN 102319557 A "An activated alumina / activated carbon composite material and its preparation method", the prepared material can also be used as a gas adsorption material. After granulation, it needs to be aged, formed, dried, sintered, rinsed, and dried. The spherical molecular sieve particles prepared in patent CN 110237771 A "A method for preparing a spherical molecular sieve" need to be screened, dried, and roasted to obtain a spherical molecular sieve product.

[0004] The above patents all require high-temperature treatment of the binder in the granulation process. During the high-temperature treatment process, a certain chemical reaction occurs, which forms a certain chemical bond with the particles, and volatilizes a portion of the binder solution to achieve a porous structure and a certain strength and toughness, which can then be used in the field of gas adsorption materials. The granulation methods recorded in these patents all require high-temperature sintering, and the materials are stable during the high-temperature sintering process. However, when the adsorbent material is unstable at high temperatures, the above granulation methods are not applicable. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a room-temperature granulation method for gas adsorption material particles. The granulation conditions are mild and the particles are formed at room temperature, thus avoiding the change in the performance of the adsorption material caused by the excessively high temperature in the ordinary granulation method, and obtaining particles with the porosity and high mechanical strength required for gas adsorption.

[0006] To achieve this purpose, the present invention adopts the following technical scheme: A method for granulating gas adsorbent material particles at room temperature, comprising the following steps:

[0007] 1) First, the solvent and the adhesive are mixed and stirred to allow the adhesive to be fully dissolved in the solvent to form a solution or a colloidal solution, thereby forming a mixed solution 1;

[0008] 2) The mixed solution 1 and the gas adsorbent material powder are combined, stirred evenly, and granulated by a granulation device at room temperature. The gas adsorbent material particles are obtained after the solvent in the granulated particles is completely volatilized.

[0009] Wherein, the weight ratio of the adhesive to the solvent and the gas adsorption material powder is: 1:3-30:3:30.

[0010] Preferably, the gas adsorbent powder is oxygen absorbing material powder.

[0011] Preferably, the oxygen absorbing material powder can be added with one or more of activated carbon powder, molecular sieve powder, and activated alumina and uniformly mixed therewith. The selection of activated carbon powder, molecular sieve powder, and activated alumina can be determined according to actual needs, and one, two, or three of them can be selected according to the substances to be adsorbed and removed.

[0012] Wherein, the solvent is an organic or inorganic solvent that can dissolve the adhesive but does not affect the adsorption performance of the gas adsorbent material. Preferably, the solvent is one or more of water, chloroform, tetrahydrofuran, N-methylpyrrolidone, N,N-dimethylformamide, styrene, perchloroethylene, trichloroethylene, ether, ethylene glycol dimethyl ether, toluene, xylene, ethyl acetate, and acetone. More preferably, the solvent is one or more of chloroform, tetrahydrofuran, toluene, N-methylpyrrolidone, and N,N-dimethylformamide. More preferably, the solvent is N-methylpyrrolidone or toluene.

[0013] Wherein, the adhesive is an organic polymer material with adhesive function. Preferably, the adhesive is one or more of polypropylene, polyamide, polyphenylene ether, polyacrylate, povidone, hydroxypropyl methylcellulose, and carboxymethyl cellulose. More preferably, the adhesive is carboxymethyl cellulose or polyphenylene ether.

[0014] Wherein, the activated carbon powder is one or more of 100 mesh, 140 mesh, 200 mesh, 270 mesh, 325 mesh and 400 mesh.

[0015] Wherein, the molecular sieve powder is one or more of 3A, 4A, 5A, and 13X molecular sieves.

[0016] Wherein, the activated alumina is one or more of alumina γ, β, δ, η, and θ.

[0017] Wherein, the equipment for forming the particles can be an extruder, a drum granulator, or a press.

[0018] The stirring speed in step 1) is 10-1000 rpm. Preferably, the mixed solution 1 can be heated to 30-90° C. during stirring to accelerate the dissolution of the adhesive.

[0019] The gas adsorbent particles may be in the shape of strips, balls, honeycombs, cylinders, clover leaves, four-leaf clover leaves, or meshes. The size of the adsorbent formed into a honeycomb shape may be: 5-5000 mm in height, 1-150000 cm2 in cross-sectional area, the aperture of the honeycomb is between 1-20 mm, and the distance between the centers of adjacent holes is between 3-30 mm.

[0020] Furthermore, the present invention also provides a gas adsorption material particle, which is obtained by granulating and molding oxygen absorbing material powder according to the method described in the present invention; the oxygen absorbing material powder is a metal organic compound with the function of adsorbing oxygen.

[0021] The oxygen absorbing material powder can be a metal organic compound with oxygen absorbing function prepared in reference to patent CN1327877, or can be an oxygen absorbing material and an adsorbing material prepared in patent "An oxygen absorbing material and its preparation method and the prepared adsorbing material capable of simultaneously adsorbing oxygen and solvent".

[0022] The oxygen absorbing material can be prepared according to the following method: the raw materials of the oxygen absorbing material include: a metal compound, a ligand L, an alkali metal hydroxide, a pyridine compound and a solvent A; the preparation method of the oxygen absorbing material is: firstly reacting the metal compound, the ligand L and the solvent A, and controlling the concentration of the metal compound and the ligand L in the reaction system to be 0.3-5 mol.L -1 , and obtain product C O L, then alkali metal hydroxide, pyridine compound, solvent A and product C O L reaction, product C O The reagent concentration of L is 0.3-5 mol.L -1 ; Control the solid raw material ratio of alkali metal hydroxide: pyridine compound: C O L=0.3-5:0.3-5:1, the oxygen absorbing material is obtained by reaction;

[0023] The ligand L is prepared according to the method in the patent "A preparation method and application of an oxygen-absorbing material ligand".

[0024] In the preparation of the oxygen absorbing material, the metal compound in the raw material is any one of copper acetate, manganese acetate, zinc acetate, ferrous acetate, manganese sulfate, cobalt sulfate, cobalt carbonate, cobalt oxalate, and cobalt acetate; the alkali metal hydroxide is one or more of lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, cesium hydroxide, and francium hydroxide; the pyridine compound is alkyl pyridine, halogenated pyridine, aminopyridine, bromopyridine, methylpyridine, iodopyridine, chloropyridine, nitropyridine, hydroxypyridine, benzylpyridine, ethylpyridine, cyanopyridine, fluoropyridine, dihydropyridine, pyridine derivative hexadecylpyridine bromide, 4-trifluoromethylnicotinic acid, pyridine hydrochloride 2-hydroxynicotinic acid, 4,4'-dibromo-2,2'-bipyridine, 3-bromo-5-methoxypyridine, 2-bromo-6-methoxypyridine, 2-aminoisonicotinic acid methyl ester, pyridine-2,6-dicarboxylic acid, One or more of 2-chloro-3-pyridine isonicotinoic acid, 4-acetylpyridine methanol, 3,5-pyridinedicarboxylic acid, 5-bromo-2-pyridinecarboxylic acid, 2-methoxy-5-pyridineboric acid, 2-amino-3-pyridinecarboxaldehyde, 6-fluoronicotinic acid, and pyridine-3-acetic acid hydrochloride; the solvent A is one or more of petroleum ether, n-hexane, n-octane, methanol, ethanol, isopropanol, butanol, hexanol, 2-ethylhexanol, cyclohexanone, and methylcyclohexanol.

[0025] Furthermore, the present invention also provides an application of a method for granulating gas adsorbent material particles at room temperature, wherein the method is applied to granulating gas adsorbent material particles that are not suitable for granulation at a high temperature above 200° C. The reason why granulation at a high temperature above 200° C. is not suitable is that some gas adsorbent materials are unstable at high temperatures. For example, when the adsorbent material powder is baked at 200° C. for 24 hours, its gas adsorption performance decreases by more than 20%.

[0026] The present invention granulates the gas adsorption material powder at room temperature and shapes it at room temperature to obtain particles with high porosity and mechanical strength required for gas adsorption, which not only meets the needs of gas adsorption, but also avoids the change of performance of certain adsorption materials caused by excessively high temperature in ordinary granulation methods, and broadens the use of adsorption materials that are unstable at high temperatures. The morphology of the gas adsorption material prepared by the present invention after granulation can be well maintained, the product yield after granulation is high, and the generation of empty shells, cracks, and powder loss is avoided. The obtained particles have high strength and are not easy to pulverize. Through different granulation shapes, the bulk density and specific surface area are increased, and the oxygen absorption capacity of the adsorption material is greatly improved.

[0027] Furthermore, the present invention also provides a technical solution for mixing and granulating adsorption material powders of different properties. Activated carbon powder, molecular sieve powder, alumina powder and oxygen absorbing material are granulated together. These materials are arranged in parallel through a binder, and granulation can be completed at room temperature. The adsorption material particles obtained after granulation will not be pulverized, will not block the adsorption column, and can adsorb oxygen and solvents at the same time. Other gases such as nitrogen, argon and other inert gases can pass smoothly. The gas adsorption material particles obtained by granulation of the present invention can be used in the adsorption column of the glove box. During the circulation of the glove box, the gas in the box must pass through the adsorption column, that is, through the gas adsorption material particles. In the process of passing, oxygen and solvents are adsorbed and removed.

[0028] Furthermore, the present invention also provides an adsorption material particle obtained by granulating oxygen absorbing material powder, which has better oxygen absorption performance than precious metal catalysts and can be reused after simple regeneration, thereby improving the oxygen absorption utilization rate, while also expanding the use range of the adsorption column and providing great convenience.

[0029] The beneficial effects of the present invention are as follows:

[0030] 1. It provides a granulation method at room temperature for gas adsorption materials that are unstable at high temperatures, thus broadening the application scope of more gas adsorption materials;

[0031] 2. It can be used for mixing, molding and granulating gas adsorption material powders of different properties;

[0032] 3. The granulation method is simple, the conditions are mild, high temperature is not required, and the process flow is stable and continuous, which solves the cumbersome operation caused by intermittent process flow. It can achieve stable continuity and convenient operation, and save time, labor, materials and costs.

[0033] 4. The adsorption material particles obtained by granulating the oxygen absorbing material powder have a formed structure, are not easy to pulverize, will not clog the adsorption column, and are easy to use.

[0034] The adsorbent material obtained by the granulation method of the present invention is prepared by forming a solution of a binder polymer and a solvent at room temperature, and then mixing and stirring the solution with adsorbent material powder and then granulating the solution into a shape. The solvent is volatilized at room temperature without high-temperature sintering. The requirements for the hardness and bulk density of the gas adsorbent material can be met, as well as the requirements for the pore size, porosity, specific surface area, etc. of the adsorbent material. The gas adsorbent material can also be made into adsorbent materials of different shapes (honeycomb, cylindrical, circular, clover-shaped, four-leaf clover-shaped, mesh-shaped, etc.) through granulation.

[0035] The granulation method of the gas adsorption material particles of the present invention can complete granulation at room temperature with mild conditions and does not require high temperature conditions. It is suitable for gas adsorption materials that cannot be processed at high temperature, and is also suitable for mixed molding of several gas adsorption materials of different properties. It greatly improves the granulation efficiency, oxygen absorption capacity, and adsorption capacity, while also expanding the limited use range of the adsorption column, reducing costs, and providing great convenience. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is a schematic diagram of the equipment and process used for granulating gas adsorption material particles used in the embodiment of the present invention.

[0037] 1. Solvent storage tank; 2. Adhesive storage tank; 3. Reactor; 4. Discharge metering pump; 5. Oxygen absorbing material storage tank; 6. Alumina / activated carbon / molecular sieve storage tank; 7. Reactor; 8. Discharger; 9. Granulator; 10. Conveyor belt; 11. Vacuum heating dryer. DETAILED DESCRIPTION

[0038] In order to fully understand the purpose, characteristics and effects of the present invention, the technical solution of the present invention is further described below in conjunction with embodiments, but the protection scope of the present invention is not limited to the following embodiments.

[0039] Unless otherwise specified, various raw materials of the present invention can be purchased from the market or prepared according to conventional methods in the art.

[0040] The method for granulating gas adsorbent material particles at room temperature of the present invention is specifically as follows:

[0041] First, according to the mass ratio (i.e., the mass fraction of adhesive is 1, the mass fraction of solvent is m, and the mass fraction of gas adsorbent powder is n), m parts of solvent by weight are added from solvent storage tank 1 to reactor 3, and then 1 part of adhesive by weight is slowly added from adhesive storage tank 2 to the solvent in reactor 3, and stirring is started to accelerate the dissolution of the adhesive; while the reactor 3 is dissolving, n parts of oxygen absorbing material and alumina (and / or activated carbon, molecular sieve) by weight are added from gas adsorbent storage tank 5 and alumina (or activated carbon, molecular sieve) storage tank 6 to reactor 7, and stirring is started to mix them. After the materials in the reactor 7 are mixed evenly, the liquid in the reactor 3 is added into the reactor 7 through the metering pump 4, stirred evenly, and then passed through the discharging device 8, the feeding port of the granulator 9, the screw gear screw, and the mold discharge port of the product of different shapes (the shape can be one or more of honeycomb, spherical, cylindrical, clover, four-leaf clover, mesh, etc.), and finally oxygen absorption products of different shapes, sizes and particle sizes are obtained. The products are transported to the vacuum heating dryer 11 for drying through the conveyor belt 10, and the dried products are subjected to the oxygen absorption cycle performance test at room temperature.

[0042] Example 1 Granulation of Gas Adsorbent Particles Containing Alumina at Normal Temperature

[0043] First, 4 parts by weight of solvent styrene are added from solvent storage tank 1 to reactor 3, and then 1 part by weight of adhesive carboxymethyl cellulose is slowly added from adhesive storage tank 2 to the styrene in reactor 3, stirring is started at a speed of 600 rpm to accelerate the dissolution of carboxymethyl cellulose; while the carboxymethyl cellulose in reactor 3 is dissolved, a total of 5 parts by weight of oxygen absorbing material and γ-active alumina are added from oxygen absorbing material storage tank 5 and alumina storage tank 6 to reactor 7, respectively, and stirring is started to mix them evenly, until a uniform transparent solution is formed in reactor 3 and the materials in reactor 7 are evenly mixed, the solution in reactor 3 is added to reactor 7 through metering pump 4, stirred evenly, and then through discharging device 8, the feeding port of granulator 9, the screw gear screw of the granulator, and the discharging port of clover-shaped product mold, a clover-shaped oxygen absorbing product is obtained, and the product is conveyed to vacuum heating dryer 11 for drying through conveyor belt 10, and then subjected to normal temperature oxygen absorption cycle performance test.

[0044] Example 2 Granulation of gas adsorbent particles at room temperature

[0045] First, 5 parts by weight of solvent styrene are added from solvent storage tank 1 to reactor 3, and then 1 part by weight of adhesive carboxymethyl cellulose is slowly added from adhesive storage tank 2 to the styrene in reactor 3, stirring is started at a speed of 800 rpm to accelerate the dissolution of carboxymethyl cellulose; while the carboxymethyl cellulose in reactor 3 is dissolved, a total of 4 parts by weight of oxygen absorbing material powder and activated carbon powder are added from oxygen absorbing material storage tank 5 and activated carbon storage tank 6 to reactor 7 respectively, stirring is started to mix them evenly, and a uniform transparent solution is formed in reactor 3. After the materials in reactor 7 are evenly mixed, the solution in reactor 3 is added to reactor 7 through metering pump 4, stirred evenly, and then through discharging device 8, the feeding port of granulator 9, the screw gear rotating rod of the granulator, and the discharging port of the strip-shaped product mold, a strip-shaped oxygen absorbing product is obtained, and the product is transported to vacuum heating dryer 11 for drying through conveyor belt 10, and then subjected to normal temperature oxygen absorption cycle performance test.

[0046] Example 3 Granulation of Gas Adsorbent Particles at Room Temperature

[0047] First, 8 parts by weight of solvent toluene are added from solvent storage tank 1 to reactor 3, and then 1 part by weight of adhesive polyphenylene ether is slowly added from adhesive storage tank 2 to the toluene in reactor 3, stirring is started at a speed of 800 rpm to accelerate the dissolution of polyphenylene ether; while the polyphenylene ether in reactor 3 is dissolved, a total of 10 parts by weight of oxygen absorbing material powder and activated carbon powder are added from oxygen absorbing material storage tank 5 and activated carbon storage tank 6 to reactor 7 respectively, stirring is started to mix them evenly, and a uniform transparent solution is formed in reactor 3. After the materials in reactor 7 are evenly mixed, the solution in reactor 3 is added to reactor 7 through metering pump 4, stirred evenly, and then through discharging device 8, the feeding port of granulator 9, the screw gear screw of the granulator, and the discharging port of the spherical product mold, a spherical oxygen absorbing product is obtained, and the product is transported to vacuum heating dryer 11 through conveyor belt 10 for drying, and then the oxygen absorption cycle performance test at room temperature is carried out.

[0048] Example 4 Granulation of Gas Adsorbent Particles at Room Temperature

[0049] First, 10 parts by weight of solvent N-methylpyrrolidone are added from solvent storage tank 1 to reactor 3, and then 1 part by weight of adhesive polyphenylene ether is slowly added from adhesive storage tank 2 to the toluene in reactor 3, stirring is started at a speed of 800 rpm to accelerate the dissolution of carboxymethyl cellulose; while the polyphenylene ether in reactor 3 is dissolved, a total of 8 parts by weight of oxygen absorbing material powder, activated carbon powder and molecular sieve powder are added from oxygen absorbing material storage tank 5, activated carbon and molecular sieve storage tank 6 to reactor 7, respectively, and stirring is started to mix them evenly, until a uniform transparent solution is formed in reactor 3 and the materials in reactor 7 are evenly mixed, the solution in reactor 3 is added to reactor 7 through metering pump 4, stirred evenly, and then through the discharging device 8, the feeding port of granulator 9, the screw gear rotating rod of the granulator, and the discharging port of the honeycomb-shaped product mold, a honeycomb-shaped oxygen absorbing product is obtained, and the product is transported to the vacuum heating dryer 11 through the conveyor belt 10 for drying, and then the oxygen absorption cycle performance test at room temperature is carried out.

[0050] Example 5 Granulation of Gas Adsorbent Particles at Room Temperature

[0051] First, 6 parts by weight of solvent toluene are added from solvent storage tank 1 to reactor 3, and then 1 part by weight of adhesive polyphenylene ether is slowly added from adhesive storage tank 2 to the toluene in reactor 3, stirring is started at a speed of 800 rpm to accelerate the dissolution of carboxymethyl cellulose; while the polyphenylene ether in reactor 3 is dissolved, a total of 8 parts by weight of oxygen absorbing material powder are added from oxygen absorbing material storage tank 5 to reactor 7, stirring is started to mix them evenly, and a uniform transparent solution is formed in reactor 3. After the materials in reactor 7 are evenly mixed, the solution in reactor 3 is added to reactor 7 through metering pump 4, stirred evenly, and then through the discharging device 8, the feeding port of granulator 9, the screw gear rotating rod of the granulator, and the discharging port of the honeycomb-shaped product mold, a honeycomb-shaped oxygen absorbing product is obtained, and the product is transported to the vacuum heating dryer 11 through the conveyor belt 10 for drying, and then the oxygen absorption cycle performance test at room temperature is carried out.

[0052] Equipment and process used for granulation of gas adsorption material particles Figure 1 shown.

[0053] The oxygen absorption performance of the adsorption material particles obtained by granulation is 6-9% (the mass of oxygen adsorption accounts for the mass percentage of the oxygen absorbing material). The oxygen absorption effect is very significant and is extremely effective when used in an anaerobic glove box, which greatly expands the industry application field of the glove box.

[0054] Example 6 Preparation of oxygen absorbing material used in particles

[0055] Preparation of raw materials: cobalt acetate, ligand L, isopropanol, potassium hydroxide, methylpyridine;

[0056] Step 1: Add 0.1 mol of cobalt acetate, 0.1 mol of ligand L, and isopropanol to a 250 mL beaker. The concentration of the reagents is controlled at 4 mol / L of cobalt acetate and ligand L. -1 , under heating conditions (control the temperature at 50-60°C), start stirring, set the stirring rate to 400rpm, and obtain mixed solution A. In another 250mL conical flask, add 0.1mol potassium hydroxide and isopropanol reagent, and the concentration is controlled at 4mol.L -1 , heat and stir at 60°C until the solid is completely dissolved to obtain mixed solution B. Under the heating and stirring conditions of mixed solution 1, add mixed solution B to mixed solution A, and control the addition to be completed within 30 minutes. After keeping the temperature for 4 hours, stop the reaction. Filter the reaction solution to obtain a reddish brown solid product COL with a yield of 95%.

[0057] Step 2: Add 0.15 mol of product COL, 0.12 mol of potassium hydroxide, 0.14 mol of methylpyridine, and solvent methanol to a 250 ml beaker. The reagent concentration is controlled at 4 mol / L potassium hydroxide. -1 The experiment was started under heating and stirring conditions, the stirring rate was set to 300 rpm, and the temperature was slowly raised to 75-85° C. After maintaining the temperature for 6 hours, the reaction was stopped to obtain the oxygen absorbing material.

[0058] The oxygen absorbing material is granulated at room temperature by the method of the present invention to obtain oxygen absorbing material particles (or gas adsorbent material particles). The gas adsorbent material particles granulated by the room temperature granulation method of the present invention have an oxygen absorption rate comparable to or even better than that of precious metal catalysts, and can be reused after simple regeneration.

[0059] Example 7 Preparation of ligand L in oxygen absorbing material

[0060] A 3L reaction vessel was connected to a reflux condenser, a constant pressure dripping device, a temperature control device, and a heating and stirring device. After vacuum replacement, an inert gas was filled in. 2 mol of 2.4-pentanedione, 3 mol of acetic anhydride, and 2.4 mol of methyl orthoformate were added to the reaction vessel in a ratio of 1:1.5:1.2. The reaction was carried out under the protection of an inert gas, with a stirring speed of 300 rpm and a temperature of the mixed solution controlled at 90° C. After the mixed reaction solution was refluxed at the temperature control point for 2 h, the heating was turned off and the temperature was lowered to room temperature under the protection of an inert gas.

[0061] Connect the reaction vessel to the vacuum distillation device, check the air tightness of the device system, and start the condensation stirring device when the air tightness is good. The stirring speed is 300rpm. Slowly connect the vacuum to the device system at room temperature, and adjust the vacuum degree to 30KPa. The boiling degree of the mixed liquid is controlled by adjusting the vacuum degree. When the droplets no longer drip, increase the vacuum degree to 15KPa, and then slowly raise the solution temperature to 60°C. The by-products in the mixture are gradually extracted and collected in the by-product receiving container until no droplets drip, and the device system is restored to normal pressure;

[0062] The above by-product receiving container was replaced with the target intermediate product receiving container, and the vacuum degree was adjusted to 10KPa. The reaction mixture was gradually heated to 100°C, and the solution began to boil. Drops of liquid fell from the target intermediate product receiving container. The temperature of the solution was finally raised to 115°C by controlling the temperature of the solution, and the target intermediate product was collected and weighed. The yield was 88%;

[0063] The target intermediate product is reacted with o-phenylenediamine and methanol under stirring conditions in a reactant ratio of 2:1:6. After the reaction, the product is filtered and dried to obtain the target product, i.e., the oxygen absorbing material ligand L. The oxygen absorbing material of Example 6 can be prepared using the oxygen absorbing material ligand L as the main raw material.

[0064] The present invention can complete granulation at room temperature, the method is simple, the conditions are mild, and high temperature conditions are not required. It is suitable for gas adsorption materials that cannot be processed at high temperature, and is also suitable for mixed molding of several gas adsorption materials with different properties. It greatly improves the granulation efficiency and oxygen absorption capacity, and also expands the use scope of the adsorption column, reduces costs, and provides great convenience.

[0065] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0066] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0067] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for granulating gas adsorbent particles at room temperature, characterized in that: The steps of the normal temperature granulation method are: 1) First, the solvent and the adhesive are mixed and stirred to allow the adhesive to be fully dissolved in the solvent to form a solution or a colloidal solution, thereby forming a mixed solution 1; 2) combining the mixed solution 1 and the gas adsorbent material powder, stirring them evenly, and granulating them through a granulation device at room temperature, and obtaining the gas adsorbent material particles after the solvent in the granulated particles is completely volatilized; The weight ratio of the binder to the solvent and the gas adsorbent powder is: 1:3-30:3-30; The gas adsorption material powder is an oxygen absorbing material powder; the oxygen absorbing material powder is a metal organic compound having the function of absorbing oxygen; The equipment for forming the particles can be an extruder, a drum granulator, or a press; The oxygen absorbing material powder is added to one or more of activated carbon powder, molecular sieve powder, and activated alumina powder, and uniformly mixed therewith; The solvent is selected from one or more of water, chloroform, tetrahydrofuran, N-methylpyrrolidone, N,N-dimethylformamide, styrene, perchloroethylene, trichloroethylene, ether, ethylene glycol dimethyl ether, toluene, xylene, ethyl acetate, and acetone; The binder is one or more of polypropylene, polyamide, polyphenylene ether, polyacrylate, povidone, hypromellose, and carboxymethyl cellulose; The room temperature granulation method of gas adsorption material particles is applied to the granulation of gas adsorption materials that are not suitable for granulation at a high temperature above 200°C; the gas adsorption materials that are not suitable for granulation at a high temperature above 200°C refer to gas adsorption materials that are baked at 200°C for 24 hours, and the gas adsorption performance is reduced by more than 20%; Wherein, the preparation method of the oxygen absorbing material is as follows: Preparation of raw materials: cobalt acetate, ligand L, isopropanol, potassium hydroxide, methylpyridine; Step 1: Add 0.1 mol of cobalt acetate, 0.1 mol of ligand L, and isopropanol to a 250 mL beaker. The concentration of the reagents is controlled at 4 mol / L of cobalt acetate and ligand L. -1 , control the temperature at 50-60°C under heating conditions, start stirring, set the stirring rate to 400rpm, and obtain mixed solution A; add 0.1mol potassium hydroxide to a 250mL conical flask, add isopropanol reagent, and control the concentration to 4mol.L -1 , heating and stirring at 60°C until the solid is completely dissolved to obtain mixed solution B; under the heating and stirring conditions of mixed solution 1, mixed solution B is added to mixed solution A, and the addition is controlled to be completed within 30 minutes; the reaction is stopped after keeping the temperature for 4 hours; the reaction solution is filtered to obtain a reddish brown solid product COL with a yield of 95%; Step 2: Add 0.15 mol of product COL, 0.12 mol of potassium hydroxide, 0.14 mol of methylpyridine, and solvent methanol to a 250 ml beaker. The reagent concentration is controlled at 4 mol / L potassium hydroxide. -1 , start the experiment under heating and stirring conditions, set the stirring rate to 300 rpm, and slowly raise the temperature to 75-85° C.; stop the reaction after keeping the temperature for 6 hours to obtain the oxygen absorbing material; Wherein, the preparation method of the ligand L in the oxygen absorbing material is as follows: A 3L reaction vessel was connected to a reflux condenser, a constant pressure dripping device, a temperature control device, and a heating and stirring device. After vacuum replacement, an inert gas was filled in. 2 mol of 2.4-pentanedione, 3 mol of acetic anhydride, and 2.4 mol of methyl orthoformate were added to the reaction vessel in a ratio of 1:1.5:1.

2. The reaction was carried out under the protection of an inert gas, with a stirring speed of 300 rpm and a temperature of the mixed solution controlled at 90° C. After the mixed reaction solution was refluxed at the temperature control point for 2 h, the heating was turned off and the temperature was lowered to room temperature under the protection of an inert gas. Connect the reaction vessel to the vacuum distillation device, check the air tightness of the device system, and start the condensation stirring device when the air tightness is good. The stirring speed is 300rpm. Slowly connect the vacuum to the device system at room temperature, and adjust the vacuum degree to 30kPa. The boiling degree of the mixed liquid is controlled by adjusting the vacuum degree. When the droplets no longer drip, increase the vacuum degree to 15kPa, and then slowly raise the solution temperature to 60°C. The by-products in the mixture are gradually extracted and collected in the by-product receiving container until no droplets drip, and the device system is restored to normal pressure. The above by-product receiving container was replaced with the target intermediate product receiving container, and the vacuum degree was adjusted to 10 kPa. The reaction mixture was gradually heated to 100 ° C. The solution began to boil, and droplets fell from the target intermediate product receiving container. The temperature of the solution was finally raised to 115 ° C by controlling the temperature, and the target intermediate product was collected and weighed. The yield was 88%; The target intermediate product is reacted with o-phenylenediamine and methanol under stirring conditions, with the reactant ratio being 2:1:

6. After the reaction, the target product, namely the oxygen absorbing material ligand L, is obtained by filtering and drying.

2. The method for granulating gas adsorbent particles at room temperature according to claim 1, characterized in that: The activated carbon powder is one or more of 100 mesh, 140 mesh, 200 mesh, 270 mesh, 325 mesh and 400 mesh.

3. The method for granulating gas adsorbent particles at room temperature according to claim 1, wherein: The molecular sieve powder is one or more of 3A, 4A, 5A, and 13X molecular sieves.

4. The method for granulating gas adsorbent particles at room temperature according to claim 1, wherein: The activated alumina is one or more of alumina γ, β, δ, η, and θ.