A method for removing carbon deposits from molecular sieve catalysts

Through the cold plasma treatment device using dielectric barrier discharge technology under low temperature conditions, the metal component aggregation problem caused by carbon accumulation in molecular sieve catalysts is solved, and the effective removal of carbon accumulation and the improvement of catalyst performance is achieved.

CN115869986BActive Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202111162331.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-30
Publication Date
2024-11-12
Estimated Expiration
2041-09-30

AI Technical Summary

Technical Problem

The combustion of carbon deposits in molecular sieve catalysts usually requires high temperatures, which leads to the aggregation of metal components of the catalyst and affects the catalytic performance. It is difficult for the prior art to effectively remove carbon deposits under low temperature conditions.

Method used

Using a cold plasma treatment device, by using discharge gas and dielectric barrier discharge technology with an oxygen content of 30-100% by volume under low temperature conditions, the AC voltage is applied to induce and maintain the micro-combustion of carbon deposits to avoid metal components caused by high temperatures. Gather.

Benefits of technology

It realizes rapid, simple and energy-saving carbon deposition removal under low temperature conditions, avoids the adverse effects of high-temperature combustion on the catalyst, and improves the dispersion of metal components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115869986B_ABST
    Figure CN115869986B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for removing carbon deposits in a molecular sieve catalyst, the method comprising: S1, placing a molecular sieve catalyst containing carbon deposits in a reaction chamber of a cold plasma treatment device; S2, passing a discharge gas into the reaction chamber, the oxygen content of the discharge gas being 30-100% by volume of an inert gas, and the volume ratio of the discharge gas to the molecular sieve catalyst containing carbon deposits being 200-2000; S3, intermittently applying an alternating voltage between a high-voltage electrode and a ground electrode of the cold plasma treatment device so that the generated cold plasma jet processes the molecular sieve catalyst containing carbon deposits, the voltage peak value of the alternating voltage being 6-20kV, and the frequency being 5-20kHz. The method of the present invention can controllably remove carbon deposits of a molecular sieve catalyst under low temperature conditions, avoid the aggregation problem of the catalyst metal components that may be caused by high temperature, and is quick to process, easy to operate, and energy-saving and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for removing carbon deposits in a molecular sieve catalyst, and in particular to a method for removing carbon deposits in a molecular sieve catalyst by initiating carbon deposit combustion under low temperature conditions. Background Art

[0002] Molecular sieves are a type of artificially synthesized hydrated aluminosilicate materials with regular pore structures. Molecular sieve materials generally have excellent adsorption, ion exchange and catalytic properties, and are therefore widely used in various fields such as oil refining and chemical industry. With the development of petrochemical technology and the continuous improvement of energy conservation and emission reduction requirements, the demand for high-performance catalysts in the reaction process is becoming increasingly urgent. The unique pore structure and excellent specific surface area of ​​molecular sieve materials give them excellent catalytic properties for many reaction processes, so they have good application prospects in industrial fields such as catalytic cracking, catalytic reforming, methanol to olefins, and VOCs (volatile organic compounds) removal.

[0003] Carbon deposition is one of the important reasons for the deactivation of molecular sieve catalysts. Carbon deposition will cover the active metal components or cause the molecular sieve pores to be blocked, thus seriously affecting the performance of the catalyst. At present, the main method to solve the carbon deposition problem in industry is to roast the catalyst in an oxygen-containing atmosphere during the catalyst regeneration process. The intense heat release during the combustion process of carbon deposition will cause the catalyst metal particles to sinter, resulting in a serious decrease in the dispersion of the active metal components. The surface of molecular sieve materials often lacks coordination unsaturated sites that interact strongly with metal components, and the surface interaction force with metal atoms is weak. Therefore, the conventional roasting regeneration process will have a significant effect on the activity of the metal-loaded molecular sieve catalyst. Therefore, how to avoid metal aggregation during the carbonization process is a problem that molecular sieve catalysts currently need to solve.

[0004] Cold plasma is a thermodynamically non-equilibrium plasma, which contains a large number of particles such as electrons, ions and free radicals. Cold plasma is in a thermodynamically non-equilibrium state, in which the electron temperature is very high while the overall temperature is low, even at room temperature. This characteristic gives cold plasma many unique applications, such as material surface treatment and modification, low-temperature crystal nucleation and growth, and low-temperature reaction processes. The literature Prog. Energy Combust. Sci. 2013, 39, 61-110 introduces the phenomenon that substances are ignited at temperatures below their ignition point under plasma conditions. Under the action of changing electric fields and free radicals, the combustion reaction activity of carbon deposits is greatly increased, and it can be ignited at temperatures below the ignition point. Dielectric barrier discharge is a cold plasma driven by high-frequency AC voltage, which is composed of a large number of randomly distributed filamentary fine pulse discharges. The micro-pulse energy density of dielectric barrier discharge is high, but the current density can be as high as 0.1~1kA / cm 2, which can trigger the combustion of catalyst carbon deposits at low temperatures. However, since each micropulse lasts for a short time (about 10 to 100 ns), the carbon deposit combustion process cannot be sustained, and the combustion can be controlled within a very small range, thereby avoiding the accumulation of local heat. Therefore, a series of "micro-combustion" processes continuously triggered by cold plasma at a lower temperature can keep the combustion temperature of carbon deposits at room temperature, thereby avoiding the adverse effects caused by the high temperature of the roasting process.

[0005] CN107486253A discloses a method for removing surface carbon species from Ag / Al2O3 catalyst by cold plasma to regenerate the catalyst. However, the low oxygen-containing discharge gas in this technical solution is not easy to activate the carbon species in the molecular sieve pores, and the electrode structure built into the high-voltage electrode is prone to cause local overheating and affect the molecular sieve. Therefore, the process of using cold plasma to induce combustion to remove carbon deposits still requires new technical solutions. Summary of the invention

[0006] The purpose of the present invention is to provide a method for removing carbon deposits in molecular sieve catalysts. The method can controllably remove carbon deposits in molecular sieve catalysts under low temperature conditions, avoiding the aggregation problem of catalyst metal components that may be caused by high-temperature carbon removal, and the method is rapid in processing, simple in operation, energy-saving and environmentally friendly.

[0007] In order to achieve the above object, the present invention provides a method for removing carbon deposits in a molecular sieve catalyst, the method comprising:

[0008] S1, placing the molecular sieve catalyst containing carbon deposits in a reaction chamber of a cold plasma treatment device;

[0009] S2, introducing a discharge gas into the reaction chamber, wherein the discharge gas is an inert gas with an oxygen content of 30-100 volume %, and the volume ratio of the discharge gas to the molecular sieve catalyst containing carbon deposits is 200-2000;

[0010] S3. Intermittently applying an alternating voltage between the high-voltage electrode and the ground electrode of the cold plasma treatment device so that the generated cold plasma jet treats the molecular sieve catalyst containing carbon deposits, wherein the peak voltage of the alternating voltage is 3-20 kV and the frequency is 3-20 kHz.

[0011] Through the above technical scheme, the method of the present invention initiates and maintains a controllable carbon deposit combustion process through cold plasma, so that the carbon deposits in the catalyst are burned under low temperature conditions, which can avoid the aggregation problem of catalyst metal components caused by high-temperature removal of carbon deposits in the catalyst. In addition, the method is simple, fast, energy-saving and environmentally friendly.

[0012] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:

[0014] Figure 1 It is a structural schematic diagram of a specific implementation of a cold plasma processing device in which the reaction chamber composed of an insulating medium is tubular;

[0015] Figure 2 It is a structural schematic diagram of a specific implementation of a cold plasma processing device in which a reaction chamber composed of an insulating medium is plate-type;

[0016] Figure 3 It is a spectrum of the discharge voltage and discharge current of the dielectric barrier discharge in the cold plasma processing device in Example 1 changing with time.

[0017] Description of Reference Numerals

[0018] 1- High voltage electrode 2- Ground electrode 3- Insulation medium

[0019] 4- Molecular sieve catalyst containing carbon deposits 5- Cold plasma generator 6- Air inlet

[0020] 7-Air outlet DETAILED DESCRIPTION

[0021] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0022] In the present invention, unless otherwise specified, directional words such as "upper" and "lower" generally refer to "upper" and "lower" when the cold plasma processing apparatus of the present invention can be used normally.

[0023] The method of the present invention places the carbon deposited molecular sieve in a cold plasma reaction chamber, and by controlling the plasma discharge voltage and frequency, the carbon deposits in the molecular sieve catalyst can be ignited in a discharge gas with a specific oxygen content, and the combustion process is controlled within a very small range, thereby achieving the purpose of removing carbon deposits on the catalyst. The temperature of the reaction system is relatively low, avoiding the problem of aggregation of catalyst metal components that may be caused by high temperature. The operation is simple, efficient, energy-saving and environmentally friendly.

[0024] In a specific embodiment of the present invention, the discharge gas is an inert gas with an oxygen content of 60-100 volume % to better activate the carbon species present in the molecular sieve pores, thereby effectively removing the carbon deposits in the molecular sieve catalyst, wherein the inert gas is one or more of nitrogen, argon, helium and neon, for example, the discharge gas is oxygen, and the discharge gas can also be a mixed gas of oxygen and one or more of nitrogen, argon, helium and neon; the volume ratio of the discharge gas to the molecular sieve catalyst containing carbon deposits is preferably 200-1800, and the carbon deposit content of the molecular sieve catalyst containing carbon deposits can vary in a large range, for example, 1-10% by mass.

[0025] In a specific embodiment of the present invention, the temperature of the reaction chamber is 20-60° C., preferably 20-50° C. The present invention does not specifically limit the method of monitoring the temperature of the reaction chamber, for example, the temperature of the reaction chamber can be monitored by an infrared temperature measuring probe to ensure that combustion occurs within a controllable range.

[0026] In a specific embodiment of the present invention, the peak voltage of the AC voltage is preferably 6-20 kV, and the frequency is preferably 5-20 kHz.

[0027] In a specific embodiment of the present invention, in step S3, the interval time of intermittently applying the AC voltage is 2-20 minutes, so as to dissipate heat from the reaction chamber in the interval time between two applications of the AC voltage, the time of applying the AC voltage once is 5-20 minutes, and the total time of applying the AC voltage is 20-60 minutes.

[0028] According to the present invention, the present invention does not specifically limit the type of molecular sieve catalyst containing carbon deposits to be treated. In a specific embodiment of the present invention, the molecular sieve catalyst is a Pt-loaded molecular sieve catalyst, the molecular sieve contained in the molecular sieve catalyst is an LTL-type molecular sieve or a Y-type molecular sieve, and the content of Pt in the molecular sieve catalyst is 0.2-1.5% by mass.

[0029] According to the present invention, the discharge form of the discharge gas can be dielectric barrier discharge. In a specific embodiment of the present invention, the discharge interval of the dielectric barrier discharge is 3-20mm, preferably 5-15mm, and the discharge interval of the dielectric barrier discharge refers to the vertical distance between the high-voltage electrode and the ground electrode minus the total thickness of the insulating medium. The insulating medium used in the dielectric barrier discharge is double-layer or single-layer, the single-layer refers to a layer of insulating medium between the high-voltage electrode and the ground electrode, and the double-layer refers to two layers of insulating medium between the high-voltage electrode and the ground electrode, and the thickness of each layer of insulating medium can be 0.3-2mm. The material of the insulating medium is well known to those skilled in the art, for example, it can be selected from one or more of quartz, corundum, glass and polytetrafluoroethylene.

[0030] According to the present invention, the cold plasma treatment device comprises a high voltage electrode 1, a ground electrode 2, a reaction chamber composed of an insulating medium and a cold plasma generator 5; the high voltage electrode 1 and the ground electrode 2 are independently connected to the cold plasma generator by wires; the reaction chamber composed of the insulating medium is tubular or plate-type. Preferably, the cold plasma treatment device may also include auxiliary components, such as an electrode heat sink and a fixing device for fixing the electrode and the reaction chamber, etc. The specific arrangement of the electrode heat sink and the fixing device is well known to those skilled in the art and will not be repeated here.

[0031] In a specific embodiment of the present invention, Figure 1 As shown, in the reaction chamber formed by the insulating medium 3, an insulating medium tube, that is, in the specific embodiment in which the reaction chamber is tubular, both ends of the insulating medium tube are closed, an air inlet 6 is provided on the side wall of one end of the reaction chamber, and an air outlet 7 is provided on the side wall of the other end, and the molecular sieve catalyst 4 containing carbon deposits to be treated is placed in the reaction chamber, the high-voltage electrode 1 is wound around the outer side wall of the insulating medium tube, and the grounding electrode 2 is arranged in the insulating medium tube. The present invention does not specifically limit the method of closing both ends of the insulating medium tube, for example, a detachable insulating plug can be used to close both ends of the insulating medium tube. The materials of the high-voltage electrode and the grounding electrode can be independently selected from one or more of stainless steel, copper, iron and aluminum. Preferably, the high-voltage electrode is a stainless steel mesh or copper tape wound around the outer side wall of the insulating medium tube, and the grounding electrode is a stainless steel rod. Optionally, a layer of insulating medium tube is arranged on the outer surface of the grounding electrode 2.

[0032] In another specific embodiment of the present invention, Figure 2As shown, in the specific embodiment in which the reaction chamber formed by the insulating medium is a plate-type, the reaction chamber includes a first insulating medium plate and a second insulating medium plate, the first insulating medium plate and the second insulating medium plate are arranged oppositely to form the upper layer and the lower layer of the reaction chamber, the material of the reaction chamber body is the same as the material of the insulating medium, the reaction chamber body can be annular, such as a circular ring, one end of the reaction chamber body is provided with an air inlet 6, and the other end is provided with an air outlet 7; the high-voltage electrode 1 is arranged on the outer side of the first insulating medium plate, and the grounding electrode 2 is arranged on the outer side of the second insulating medium plate. In this embodiment, preferably, the high-voltage electrode is arranged closely on the outer side of the first insulating medium plate, and the grounding electrode is arranged closely on the outer side of the second insulating medium plate, and the insulating medium used for dielectric barrier discharge is double-layered. The materials of the high-voltage electrode and the grounding electrode can be independently selected from one or more of stainless steel, copper, iron and aluminum. Preferably, the high-voltage electrode and the grounding electrode are independently stainless steel plates. Optionally, the first insulating dielectric plate and the grounding electrode are arranged opposite to each other to form the upper and lower layers of the reaction chamber, and the high-voltage electrode 1 is arranged on the outer side of the first insulating dielectric plate. In this case, the insulating medium used for dielectric barrier discharge is a single layer.

[0033] The present invention is further described below by way of examples, but the present invention is not limited thereto.

[0034] In the example, the carbon content of the molecular sieve containing carbon deposits is determined by high-frequency combustion-infrared absorption method. The metal dispersion of the molecular sieve containing carbon deposits is tested by H2 chemical adsorption method. Specifically, the molecular sieve catalyst containing carbon deposits is first reduced with H2 at 480°C for 1 hour before the test. During the test, the number of surface metal atoms M is determined by H2 pulse adsorption. s , the metal dispersion R is determined by M s and the total number of metal atoms M t The ratio is expressed as .

[0035] Example 1

[0036] S1. Take 3 g of carbon-deactivated Pt / KL molecular sieve catalyst particles with a carbon content of 2.06 mass % as the catalyst to be treated, wherein the Pt content is 1.0 mass %. Place the catalyst to be treated in a cold plasma treatment device with a flat-plate structure reaction chamber. The structure of the cold plasma treatment device is as follows: Figure 2As shown, a flat-plate reaction chamber and a cold plasma generator are formed of a high-voltage electrode, a ground electrode, and an insulating medium; the upper and lower layers of the reaction chamber are formed by a first insulating medium plate and a second insulating medium plate arranged opposite to each other, the reaction chamber body is a quartz ring, one end of the reaction chamber body is provided with an air inlet 6, and the other end is provided with an air outlet 7, the first insulating medium plate and the second insulating medium plate are respectively plate-type quartz dielectric layers, the thickness of each quartz dielectric layer is 0.5 mm, and the discharge interval is 10 mm; stainless steel plates are used as high-voltage electrodes and ground electrodes respectively.

[0037] S2, introducing a mixed gas of oxygen and nitrogen with an oxygen content of 80% by volume (referred to as oxygen / nitrogen) as a discharge gas into the reaction chamber, and the volume ratio of the discharge gas to the carbon-deactivated Pt / KL molecular sieve catalyst (referred to as the gas / agent volume ratio) is 600:1;

[0038] S3. Adjust the cold plasma generator to intermittently apply AC voltage between the high voltage electrode and the ground electrode, with a voltage peak of 10 kV and a discharge pulse frequency of 7.5 kHz, to induce dielectric barrier discharge at 40 °C. The voltage and current changes over time during the discharge process are shown in Figure 3 As shown. The interval time of intermittently applying the AC voltage is 5 minutes, and the flow rate of the mixed gas is kept unchanged during the period of pausing the voltage application. The time of applying the AC voltage once is 5 minutes. The AC voltage is applied 6 times in the treatment process, and the total time of applying the AC voltage is 30 minutes. After the discharge is completed, the cold plasma treatment device is still maintained at 40°C. After the treatment, the carbon content of the catalyst is 0.10% by mass, and the metal dispersion is 0.53%.

[0039] Example 2

[0040] The carbon-deactivated molecular sieve catalyst was treated in the same manner as in Example 1, except that the catalyst to be treated was 3 g of carbon-deactivated Pt / HY molecular sieve catalyst particles with a carbon content of 3.35% by mass, wherein the Pt content was 0.5% by mass. The carbon content of the treated catalyst was 0.11% by mass, and the metal dispersion was 0.54%.

[0041] Example 3

[0042] The Pt / KL molecular sieve catalyst deactivated by carbon deposition was treated in the same manner as in Example 1, except that the discharge gas was a mixed gas of oxygen and nitrogen with an oxygen content of 60% by volume. The carbon content of the catalyst after treatment was 0.12% by mass, and the metal dispersion was 0.52%.

[0043] Example 4

[0044] The Pt / KL molecular sieve catalyst deactivated by carbon deposition was treated in the same manner as in Example 1, except that the discharge gas was pure oxygen. The carbon content of the catalyst after treatment was 0.09% by mass, and the metal dispersion was 0.53%.

[0045] Example 5

[0046] The Pt / KL molecular sieve catalyst deactivated by carbon deposition was treated in the same manner as in Example 1, except that the discharge gas was a mixed gas of oxygen and nitrogen with an oxygen content of 40% by volume. The carbon content of the catalyst after treatment was 0.15% by mass, and the metal dispersion was 0.52%.

[0047] Example 6

[0048] The Pt / KL molecular sieve catalyst deactivated by carbon deposition was treated in the same manner as in Example 1, except that the discharge gas was a mixed gas of oxygen and argon with an oxygen content of 80% by volume (referred to as oxygen / argon). The carbon content of the catalyst after treatment was 0.13% by mass, and the metal dispersion was 0.52%.

[0049] Example 7

[0050] The carbon-deactivated Pt / KL molecular sieve catalyst was treated in the same manner as in Example 1, except that the volume ratio of the discharge gas to the carbon-deactivated Pt / KL molecular sieve catalyst was 200: 1. The carbon content of the treated catalyst was 0.14% by mass, and the metal dispersion was 0.51%.

[0051] Example 8

[0052] The carbon-deactivated Pt / KL molecular sieve catalyst was treated in the same manner as in Example 1, except that the volume ratio of the discharge gas to the carbon-deactivated Pt / KL molecular sieve catalyst was 1200: 1. The carbon content of the treated catalyst was 0.09% by mass, and the metal dispersion was 0.53%.

[0053] Example 9

[0054] The Pt / KL molecular sieve catalyst deactivated by carbon deposition was treated in the same manner as in Example 1, except that the voltage peak was 6 kV and the frequency of the discharge pulse was 5 kHz. The carbon content of the treated catalyst was 0.11% by mass and the metal dispersion was 0.53%.

[0055] Example 10

[0056] The same method as in Example 1 was used to treat the carbon-deposited deactivated Pt / KL molecular sieve catalyst, except that the voltage peak was 20 kV and the discharge frequency was 20 kHz. The carbon content of the treated catalyst was 0.10% by mass and the metal dispersion was 0.51%.

[0057] Example 11

[0058] The same method as in Example 1 was used to treat the carbon-deposited deactivated Pt / KL molecular sieve catalyst, except that the AC voltage was applied for 10 minutes each time, and the AC voltage was applied 6 times during the treatment process, that is, the total AC voltage application time was 60 minutes. After the treatment, the catalyst carbon content was 0.09% by mass, and the metal dispersion was 0.51%.

[0059] Example 12

[0060] S1. Take 3 g of carbon-deactivated Pt / KL molecular sieve catalyst particles with a carbon content of 2.17 mass % as the catalyst to be treated, wherein the Pt content is 1.0 mass %. Place the catalyst to be treated in a cold plasma treatment device with a tubular reaction chamber. The structure of the cold plasma treatment device is as follows: Figure 1 As shown, it includes a high-voltage electrode, a grounding electrode, an insulating medium tube and a cold plasma generator. The insulating medium tube is a single-layer quartz material with a thickness of 1 mm. Both ends of the insulating medium tube are sealed with polytetrafluoroethylene plugs. The side wall of one end of the insulating medium tube is provided with an air inlet 6, and the side wall of the other end is provided with an air outlet 7. A copper tape is tightly wound around the outer side wall of the insulating medium tube as a high-voltage electrode, and a thin stainless steel rod is inserted into the reaction chamber as a grounding electrode.

[0061] S2. The discharge interval of the reaction chamber is 5 mm. A mixed gas of oxygen and nitrogen with an oxygen content of 80% by volume is introduced into the reaction chamber as the discharge gas, and the volume ratio of the discharge gas to the carbon-deactivated Pt / KL molecular sieve catalyst is 600:1;

[0062] S3. Adjust the cold plasma generator to apply a high-frequency AC voltage between the high-voltage electrode and the ground electrode, with a voltage peak of 10 kV and a discharge pulse frequency of 7.5 kHz, to induce dielectric barrier discharge at 45°C. The interval between intermittent application of the AC voltage is 5 minutes, and the flow rate of the mixed gas is kept unchanged during the period of pausing the application of the voltage. The time for applying the AC voltage once is 5 minutes, and the AC voltage is applied 6 times during the treatment process, and the total time for applying the AC voltage is 30 minutes. After the discharge is completed, the cold plasma treatment device is still maintained at 45°C. The carbon content of the catalyst after treatment is 0.09% by mass, and the metal dispersion is 0.52%.

[0063] Example 13

[0064] The Pt / KL molecular sieve catalyst deactivated by carbon deposition was treated in the same manner as in Example 12, except that the discharge interval of the reaction chamber was 15 mm. The carbon content of the catalyst after treatment was 0.15% by mass, and the metal dispersion was 0.53%.

[0065] Example 14

[0066] The Pt / KL molecular sieve catalyst deactivated by carbon deposition was treated in the same manner as in Example 12, except that the insulating medium tube was made of corundum. After treatment, the carbon content of the catalyst was 0.10% by mass and the metal dispersion was 0.53%.

[0067] Example 15

[0068] The same method as in Example 12 was used to treat the carbon-deposited deactivated Pt / KL molecular sieve catalyst particles, except that the insulating medium tube was made of glass. The carbon content of the treated catalyst was 0.12% by mass, and the metal dispersion was 0.51%.

[0069] Comparative Example 1

[0070] The Pt / KL molecular sieve catalyst deactivated by carbon deposition was treated in the same manner as in Example 1, except that the discharge gas used was a mixed gas of oxygen and nitrogen with an oxygen content of 10% by volume. The carbon content of the catalyst after treatment was 0.66% by mass, and the metal dispersion was 0.51%.

[0071] Comparative Example 2

[0072] The carbon-deactivated Pt / KL molecular sieve catalyst was treated in the same manner as in Example 1, except that the volume ratio of the discharge gas to the carbon-deactivated Pt / KL molecular sieve catalyst was 100: 1. The carbon content of the treated catalyst was 0.61% by mass, and the metal dispersion was 0.50%.

[0073] Comparative Example 3

[0074] The Pt / KL molecular sieve catalyst deactivated by carbon deposition was treated in the same manner as in Example 1, except that the voltage peak was 30 kV and the frequency of the discharge pulse was 25 kHz. The carbon content of the treated catalyst was 0.14% by mass and the metal dispersion was 0.43%.

[0075] Comparative Example 4

[0076] The same method as in Example 1 was used to treat the Pt / KL molecular sieve catalyst deactivated by carbon deposition, except that in step S3, an AC voltage was continuously applied between the high voltage electrode and the ground electrode for 60 minutes without a pause. After the treatment, the carbon content of the catalyst was 0.13% by mass, and the metal dispersion was 0.40%.

[0077] Comparative Example 5

[0078] The Pt / KL molecular sieve catalyst deactivated by carbon deposition was treated in the same manner as in Example 12, except that the thin stainless steel rod inside the insulating medium tube was used as the high-voltage electrode, and the copper tape outside the insulating medium tube was used as the grounding electrode, i.e., the high and low voltage electrodes were opposite to those in Example 12. The carbon content of the catalyst after treatment was 0.20% by mass, and the metal dispersion was 0.44%.

[0079] Comparative Example 6

[0080] Take 3g of the carbon-deactivated Pt / KL molecular sieve catalyst particles with a carbon content of 2.06% by mass as described in Example 1, crush them into fine particles with a diameter of 0.25-0.50mm, place them in the reaction tube of the catalyst treatment device, and heat them to 400°C under a nitrogen atmosphere. After the temperature stabilizes, gradually introduce air into the reactor to continuously char the carbon-deposited catalyst at 400°C for 2h under an air atmosphere. After charring, the system is gradually cooled to 20°C in an air atmosphere. The carbon content of the catalyst after charring treatment is 0.25% by mass, and the metal dispersion is 0.43%.

[0081] Comparative Example 7

[0082] 3 g of the carbon-deactivated Pt / KL molecular sieve catalyst particles with a carbon content of 2.17 mass % described in Example 12 were treated according to the method of Comparative Example 6, except that the carbonization temperature was 450° C. After the carbonization treatment, the carbon content of the catalyst was 0.12 mass % and the metal dispersion was 0.29%.

[0083] Comparative Example 8

[0084] 3 g of the carbon-deactivated Pt / KL molecular sieve catalyst particles with a carbon content of 2.17 mass % described in Example 12 were treated according to the method of Comparative Example 6, except that the carbonization temperature was 520° C. After the carbonization treatment, the carbon content of the catalyst was 0.07 mass % and the metal dispersion was 0.03%.

[0085] The experimental conditions for removing carbon deposits with molecular sieve catalysts in various examples and comparative examples are shown in Table 1, and the results are summarized in Table 2.

[0086]

[0087] Table 2

[0088]

[0089] As can be seen from Table 2, the method of the present invention can controllably remove carbon deposits from molecular sieve catalysts at a relatively low temperature. The metal components of the catalyst obtained after removing the carbon deposits have a high degree of dispersion, which effectively reduces the aggregation of metal components during the decarbonization process.

[0090] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0091] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0092] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for removing carbon deposits from a molecular sieve catalyst, the method comprising: S1, placing the molecular sieve catalyst containing carbon deposits in a reaction chamber of a cold plasma treatment device; S2, introducing a discharge gas into the reaction chamber, wherein the discharge gas is an inert gas with an oxygen content of 30-100 volume %, and the volume ratio of the discharge gas to the molecular sieve catalyst containing carbon deposits is 200-2000; the inert gas is one or more of nitrogen, argon, helium and neon; S3, intermittently applying an alternating voltage between the high-voltage electrode and the ground electrode of the cold plasma treatment device, so that the generated cold plasma jet treats the molecular sieve catalyst containing carbon deposits, the voltage peak of the alternating voltage is 6-20 kV, and the frequency is 5-20 kHz; the interval time of intermittently applying the alternating voltage is 2-20 min, the time of applying the alternating voltage once is 5-20 min, and the total time of applying the alternating voltage is 20-60 min; The cold plasma treatment device comprises a high voltage electrode (1), a ground electrode (2), a reaction chamber formed by an insulating medium (3), and a cold plasma generator (5); The high-voltage electrode (1) and the ground electrode (2) are each independently connected to the cold plasma generator via electric wires; the reaction chamber formed by the insulating medium is tubular or plate-type; When the reaction chamber formed by the insulating medium (3) is tubular, both ends of the insulating medium tube are closed, a gas inlet (6) is provided on the side wall at one end of the reaction chamber, and a gas outlet (7) is provided on the side wall at the other end, the high-voltage electrode (1) is wound around the outer side wall of the insulating medium tube, and the grounding electrode (2) is arranged in the insulating medium tube; When the reaction chamber formed by the insulating medium (3) is of plate type, the reaction chamber comprises a first insulating medium plate and a second insulating medium plate, the first insulating medium plate and the second insulating medium plate are arranged relative to each other to form the upper layer and the lower layer of the reaction chamber, one end of the reaction chamber body is provided with an air inlet (6), and the other end is provided with an air outlet (7); the high-voltage electrode (1) is arranged on the outer side surface of the first insulating medium plate, and the grounding electrode (2) is arranged on the outer side surface of the second insulating medium plate.

2. The method according to claim 1, wherein: The discharge gas is an inert gas with an oxygen content of 60-100 volume %, and the volume ratio of the discharge gas to the molecular sieve catalyst containing carbon deposits is 200-1800.

3. The method according to claim 1, wherein: The temperature of the reaction chamber is 20-60°C.

4. The method according to claim 1, wherein: The molecular sieve catalyst is a Pt-loaded molecular sieve catalyst, the molecular sieve contained in the molecular sieve catalyst is an LTL-type molecular sieve or a Y-type molecular sieve, and the content of Pt in the molecular sieve catalyst is 0.2-1.5% by mass.

5. The method according to claim 1, wherein: The discharge form of the discharge gas is dielectric barrier discharge, and the discharge interval of the dielectric barrier discharge is 3-20 mm.

6. The method according to claim 5, wherein: The insulating medium used in the dielectric barrier discharge is double-layer or single-layer, the thickness of each layer of the insulating medium is 0.3-2 mm, and the material of the insulating medium is selected from one or more of quartz, corundum, glass and polytetrafluoroethylene.

7. The method according to claim 1, wherein: When the reaction chamber formed by the insulating medium (3) is tubular, a layer of insulating medium tube is disposed outside the grounding electrode (2); When the reaction chamber formed by the insulating medium (3) is in plate form, the first insulating medium plate and the grounding electrode are arranged opposite to each other to form the upper and lower layers of the reaction chamber, and the high-voltage electrode (1) is arranged on the outer side of the first insulating medium plate.

Citation Information

Patent Citations

  • Method for in-situ regeneration of inactivated Ag / Al2O3 catalyst by dielectric barrier discharge plasma

    CN107486253A

  • Atmospheric pressure cold plasma regeneration method for nanogold catalyst

    CN102600866A

  • Regeneration method of catalyst for synthesizing isopropylbenzene

    CN104549563A

  • Dielectric barrier discharge plasma system with catalyst and method for removing carbon dioxide and methane using the same

    KR1020150078105A

  • Method of regenerating zeolite catalyst for aromatization of acetylene by plasma treatment

    US20190262816A1