A preparation process of high-toughness steel forging for ball mill

Through induction furnace melting and segmentation process optimization, high-toughness steel forgings are prepared, which solves the problem of insufficient wear resistance and mechanical properties of steel forgings used in ball mills, and achieves improvements in wear resistance and service life.

CN115927967BActive Publication Date: 2024-10-01MERRILL LYNCH TECH (PANZHIHUA) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211655278.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-22
Publication Date
2024-10-01
Estimated Expiration
2042-12-22

AI Technical Summary

Technical Problem

The existing forged steel for ball mills has insufficient wear resistance and mechanical properties, and has a short service life. Moreover, the metal heat treatment process has a great impact on performance, making it difficult to balance strength and toughness.

Method used

The induction furnace is used to melt scrap steel, high-carbon ferrochrome, vanadium-aluminum alloy, tungsten-rhenium alloy and other raw materials to prepare high-toughness steel forging. Through segmented heating, quenching and low-temperature tempering processes, the crystal structure is optimized and the wear resistance is improved.

Benefits of technology

It significantly improves the wear resistance, hardness and toughness of steel forging for ball mills, prolongs the service life, avoids the decrease in strength and plasticity caused by unreasonable composition matching, and enhances the resistance to abrasive wear.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a preparation process of high-toughness steel forging for ball mill, wherein scrap steel, high-carbon ferrochrome, vanadium aluminum alloy, tungsten-rhenium alloy, zirconium alloy and other raw materials are added into an induction furnace for smelting, and after the raw materials are completely dissolved at high temperature, a qualified alloy liquid is obtained, and then the alloy liquid is cast to form a forged steel casting, and then the forged steel casting is heated and kept in sections, and then a quenching process is performed, and after section heating and low-temperature tempering, a forged steel matrix is ​​obtained, and then grinding and polishing, ultrasonic cleaning, and drying are performed to obtain high-toughness steel forging for ball mill. The invention can improve the defects of coarse crystal structure and poor wear resistance of existing steel forging for ball mill, and the process flow is simple and the service life of the workpiece is extended.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of wear-resistant materials, and in particular to a preparation process of high-toughness steel forging for a ball mill. Background Art

[0002] Ball mill is a widely used grinding equipment in various infrastructure industries. Steel forging is used as the grinding material medium in the ball mill. It is subjected to collision and friction between steel forgings and between steel forgings and materials for a long time, so there are certain requirements for its wear resistance and mechanical properties. The chemical composition of steel can vary greatly. In actual production, steel often contains different alloy elements according to different uses, such as manganese, nickel, vanadium, etc., which can affect the existing steel forging for ball mills by changing the inherent composition of steel. The problems of insufficient wear resistance and mechanical properties, as well as the service life and grinding effect of steel forgings, and the metal heat treatment process of forged steel will also have a great impact on the performance of forged steel. Summary of the invention

[0003] The invention aims to provide a preparation process of high-toughness steel forging for a ball mill, wherein scrap steel, high-carbon ferrochrome, vanadium-aluminum alloy, tungsten-rhenium alloy, zirconium alloy and other preparation raw materials are added into an induction furnace for smelting, and after the raw materials are completely melted at high temperature, a qualified alloy liquid is obtained, and then the alloy liquid is cast to form a forged steel casting, and then the forged steel casting is heated and kept warm in sections, and then a quenching process is performed, and after section heating and low-temperature tempering, a forged steel matrix is ​​obtained, and then grinding and polishing, ultrasonic cleaning and drying are performed to obtain high-toughness steel forging for a ball mill, which can improve the defects of rough crystal structure and poor wear resistance of existing steel forging for a ball mill, has a simple process flow and extends the service life of the workpiece.

[0004] The technical solution adopted by the present invention is as follows:

[0005] A preparation process of a high-toughness steel forging for a ball mill, wherein the high-toughness steel forging for a ball mill comprises, by mass fraction, C: 1.45-1.75%, Si: 0.75-0.8%, Mn: 1.0-1.12%, Al: 0.1-0.25%, Cr: 8.5-10%, Re: 0.03-0.1%, W: 0.3-0.8%, Zr: 0.05-0.15%, Nb: 0.02-0.045%, Mo: 0.4-0.7%, Sr: 0.05-0.15%, V: 0.05-0.15%, P: ≤0.03%, S: ≤0.02%, and the rest is Fe and unavoidable impurities.

[0006] The preparation process of high toughness steel forging for ball mill comprises the following steps:

[0007] S1. According to the weight ratio of each chemical component of high-toughness steel forging for ball mill, scrap steel, high-carbon ferrochrome, vanadium-aluminum alloy, tungsten-rhenium alloy, zirconium alloy and prepared raw materials are added into an induction furnace for smelting. After the raw materials are completely melted at high temperature, the molten materials are stirred, and then kept still for a period of time under a heat preservation state to obtain a qualified alloy liquid, and then the alloy liquid is cast into a mold to obtain a forged steel casting;

[0008] S2, air-cooling the casting to room temperature, then heating and keeping the cooled forged steel casting in sections, and then performing a quenching process;

[0009] S3, using a cleaning agent to remove impurities and oil stains from the surface of the substrate, the cleaning agent includes one or more of industrial ethylene dichloride, industrial carbon tetrachloride, industrial trichloroethylene, industrial alcohol with a concentration of not less than 95.6%, concentrated nitric acid with a concentration of not less than 98%, and alkaline degreasing liquid, and drying after cleaning;

[0010] S4, heating the obtained forged steel blank in sections and then tempering it at low temperature to obtain a forged steel matrix;

[0011] S5. Grind and polish the forged steel substrate after step S4, perform ultrasonic cleaning, and dry to obtain a high-toughness steel forging for a ball mill.

[0012] In the above technical solution, preferably, the mass fraction of rhenium element in the tungsten-rhenium alloy used in the high-toughness steel forging for the ball mill is less than 10% of the total mass fraction of the tungsten-rhenium alloy.

[0013] In the above technical solution, preferably, the zirconium alloy in S1 uses one or both of Zr-1Nb and Zr-2.5Nb.

[0014] In the above technical solution, preferably, the smelting temperature in S1 is 1500-1560°C.

[0015] Preferably, the above technical solution is characterized in that the pouring temperature in S1 is 1420-1450°C.

[0016] In the above technical scheme, preferably, the specific process of segmented heating in S2 is: heating the casting to 430-455°C at a heating rate of 6.5-7.5°C / min, keeping warm for 20-35min, heating it to 770-790°C at a heating rate of 5.5-6.5°C / min, keeping warm for 25-35min, heating it to 940-960°C at a heating rate of 3.5-4.5°C / min, keeping warm for 13-18min, then oil quenching to 730-750°C, then quenching to room temperature through water, keeping warm for 30-40min, then heating it to 260-270°C at a heating rate of 4-5.5°C / min, keeping warm for 25-30min, heating it to 355-365°C at a heating rate of 2-3.5°C / min, keeping warm for 20-30min, and then air cooling to room temperature.

[0017] In the above technical scheme, preferably, the specific process of S4 medium and low temperature tempering is: heating the forged steel blank to 225-240°C, keeping warm for 25-30 minutes, heating to 280-290°C, keeping warm for 45-55 minutes, heating to 320-325°C, keeping warm for 50-60 minutes, heating to 410-415°C, keeping warm for 70-75 minutes, heating to 570°C, keeping warm for 120-130 minutes, air cooling to room temperature, and then heating to 240-250°C, keeping warm for 1.5-2 hours to obtain a forged steel matrix.

[0018] Beneficial effects of the present invention:

[0019] The present invention innovatively designs a preparation process of high-toughness steel forging for ball mill. In the process of preparing high-toughness steel forging, the reasonable matching of multiple alloy components such as manganese, nickel, chromium and molybdenum ensures that the strength of the forged steel can be increased while ensuring that the forged steel has high toughness and plasticity, avoiding the obvious decrease in the plasticity and toughness of the material due to the increase in strength, overcoming the contradiction that the material cannot take into account both strength and plasticity and toughness due to unreasonable matching of various components, and can refine the microstructure grains, improve the wear resistance of the forged steel, and make the wear-resistant ball blank have mechanical properties such as hardness, strength and toughness. The performance of the wear-resistant balls is improved to a certain extent; the segmented tempering method is beneficial to further stress relief of the wear-resistant balls to prevent cracking and deformation. During the abrasive wear process, the large-sized hard particles can resist the micro-cutting effect of the abrasive particles and prevent the abrasive particles from embedding into the matrix: when the abrasive particles are embedded in a certain part of the matrix and sliding cutting occurs, the hard particles can hinder the sliding cutting of the abrasive particles; the small-sized particles and the fine Bema complex phase can enhance the yield strength of the matrix, improve its ability to resist deformation, provide better support for the hard particles, and prevent the large-sized hard particles from falling off when continuously subjected to external forces.

[0020] By rationally matching multiple alloy components such as manganese, nickel, chromium and molybdenum, it is ensured that the strength of forged steel can be increased while ensuring that the forged steel has high toughness and plasticity, avoiding the obvious decrease in material plasticity and toughness due to increased strength, and overcoming the contradiction that the material cannot take into account both strength and plasticity and toughness due to unreasonable matching of various components. DETAILED DESCRIPTION

[0021] Embodiment 1:

[0022] The invention provides a preparation process of a high-toughness steel forging for a ball mill. The high-toughness steel forging for a ball mill comprises, in mass fraction, C: 1.45-1.75%, Si: 0.75-0.8%, Mn: 1.0-1.12%, Al: 0.1-0.25%, Cr: 8.5-10%, Re: 0.03-0.1%, W: 0.3-0.8%, Zr: 0.05-0.15%, Nb: 0.02-0.045%, Mo: 0.4-0.7%, Sr: 0.05-0.15%, V: 0.05-0.15%, P: ≤0.03%, S: ≤0.02%, and the rest is Fe and unavoidable impurities.

[0023] The preparation process of the high-toughness steel forging for a ball mill comprises the following steps:

[0024] S1. According to the weight ratio of each chemical component of high-toughness steel forging for ball mill, scrap steel, high-carbon ferrochrome, vanadium-aluminum alloy, tungsten-rhenium alloy, zirconium alloy and prepared raw materials are added into an induction furnace for smelting at a smelting temperature of 1500° C. After the raw materials are completely melted at high temperature, the molten materials are stirred, and then kept still for a period of time under a heat preservation state to obtain a qualified alloy liquid, and then the alloy liquid is cast into a mold to obtain a forged steel casting;

[0025] S2, air-cooling the casting to room temperature, then heating the cooled forged steel casting in sections, heating the casting to 455°C at a heating rate of 6.5°C / min, keeping the temperature for 20min, heating the casting to 770°C at a heating rate of 6.5°C / min, keeping the temperature for 35min, heating the casting to 960°C at a heating rate of 3.5°C / min, keeping the temperature for 3 hours, and then performing a quenching process by water quenching. When the temperature is reduced to 720°C, the temperature is further increased to 950°C, and the temperature is kept for 1 hour. The casting is quenched again by oil quenching, the temperature is reduced to 530°C, and the temperature is kept for 2 hours. After that, the casting is cooled to room temperature in air to obtain a forged steel embryo;

[0026] S3, using a cleaning agent to remove impurities and oil stains from the surface of the substrate, the cleaning agent includes one or more of industrial ethylene dichloride, industrial carbon tetrachloride, industrial trichloroethylene, industrial alcohol with a concentration of not less than 95.6%, concentrated nitric acid with a concentration of not less than 98%, and alkaline degreasing liquid, and drying after cleaning;

[0027] S4, subjecting the forged steel body obtained through the quenching process to low temperature tempering, heating the forged steel body to 225° C., keeping the temperature for 25 min, heating to 280° C., keeping the temperature for 55 min, heating to 320° C., keeping the temperature for 60 min, heating to 410° C., keeping the temperature for 75 min, heating to 570° C., keeping the temperature for 120 min, air cooling to room temperature, and then heating to 250° C., keeping the temperature for 1.5 to obtain a forged steel matrix;

[0028] S5. Grind and polish the forged steel substrate after step S4, perform ultrasonic cleaning, and dry to obtain a high-toughness steel forging for a ball mill.

[0029] Embodiment 2:

[0030] The invention provides a preparation process of a high-toughness steel forging for a ball mill. The high-toughness steel forging for a ball mill comprises, in mass fraction, C: 1.75%, Si: 0.75%, Mn: 1.12%, Al: 0.1%, Cr: 10%, Re: 0.03%, W: 0.8%, Zr: 0.05%, Nb: 0.045%, Mo: 0.4%, Sr: 0.15%, V: 0.05%, P: ≤0.03%, S: ≤0.02%, and the rest is Fe and unavoidable impurities.

[0031] The preparation process of the high-toughness steel forging for a ball mill comprises the following steps:

[0032] S1. According to the weight ratio of each chemical component of high-toughness steel forging for ball mill, scrap steel, high-carbon ferrochrome, vanadium-aluminum alloy, tungsten-rhenium alloy, zirconium alloy and prepared raw materials are added into an induction furnace for smelting at a smelting temperature of 1560° C. After the raw materials are completely melted at high temperature, the molten materials are stirred, and then kept still for a period of time under a heat preservation state to obtain a qualified alloy liquid, and then the alloy liquid is cast into a mold to obtain a forged steel casting;

[0033] S2, air-cooling the casting to room temperature, then heating the cooled forged steel casting in sections, heating the casting to 430°C at a heating rate of 7.5°C / min, keeping the temperature for 35min, heating the casting to 790°C at a heating rate of 5.5°C / min, keeping the temperature for 25min, heating the casting to 940°C at a heating rate of 4.5°C / min, keeping the temperature for 3 hours, and then performing a quenching process by water quenching. When the temperature is reduced to 760°C, the temperature is further increased to 910°C, and the temperature is kept for 2 hours. The casting is quenched again by oil quenching, the temperature is reduced to 500°C, and the temperature is kept for 2 hours, and then cooled to room temperature in air to obtain a forged steel embryo;

[0034] S3, using a cleaning agent to remove impurities and oil stains from the surface of the substrate, the cleaning agent includes one or more of industrial ethylene dichloride, industrial carbon tetrachloride, industrial trichloroethylene, industrial alcohol with a concentration of not less than 95.6%, concentrated nitric acid with a concentration of not less than 98%, and alkaline degreasing liquid, and drying after cleaning;

[0035] S4, subjecting the forged steel body obtained through the quenching process to low temperature tempering, heating the forged steel body to 240° C., keeping the temperature for 25 min, heating to 290° C., keeping the temperature for 45 min, heating to 325° C., keeping the temperature for 50 min, heating to 415° C., keeping the temperature for 70 min, heating to 570° C., keeping the temperature for 130 min, air cooling to room temperature, and then heating to 240° C., keeping the temperature for 2 h to obtain a forged steel matrix;

[0036] S5. Grind and polish the forged steel substrate after step S4, perform ultrasonic cleaning, and dry to obtain a high-toughness steel forging for a ball mill.

[0037] Embodiment 3:

[0038] The invention provides a preparation process of a high-toughness steel forging for a ball mill. The high-toughness steel forging for a ball mill comprises, in mass fraction, C: 1.65%, Si: 0.78%, Mn: 1.1%, Al: 0.15%, Cr: 9.2%, Re: 0.05%, W: 0.5%, Zr: 0.1%, Nb: 0.03%, Mo: 0.5%, Sr: 0.1%, V: 0.1%, P: ≤0.03%, S: ≤0.02%, and the rest is Fe and unavoidable impurities.

[0039] The preparation process of the high-toughness steel forging for a ball mill comprises the following steps:

[0040] S1. According to the weight ratio of each chemical component of high-toughness steel forging for ball mill, scrap steel, high-carbon ferrochrome, vanadium-aluminum alloy, tungsten-rhenium alloy, zirconium alloy and prepared raw materials are added into an induction furnace for smelting at a smelting temperature of 1540° C. After the raw materials are completely melted at high temperature, the molten materials are stirred, and then kept still for a period of time under a heat preservation state to obtain a qualified alloy liquid, and then the alloy liquid is cast into a mold to obtain a forged steel casting;

[0041] S2, air-cooling the casting to room temperature, then heating the cooled forged steel casting in sections, heating the casting to 440°C at a heating rate of 7°C / min, keeping the temperature for 30 minutes, heating the casting to 783°C at a heating rate of 6°C / min, keeping the temperature for 30 minutes, heating the casting to 949°C at a heating rate of 4.2°C / min, keeping the temperature for 3 hours, and then performing a quenching process by water quenching. When the temperature is reduced to 740°C, the temperature is further increased to 940°C, and the temperature is kept for 1.5 hours. The casting is quenched again by oil quenching, the temperature is reduced to 515°C, and the temperature is kept for 2 hours. After that, it is cooled to room temperature in air to obtain a forged steel embryo;

[0042] S3, using a cleaning agent to remove impurities and oil stains from the surface of the substrate, the cleaning agent includes one or more of industrial ethylene dichloride, industrial carbon tetrachloride, industrial trichloroethylene, industrial alcohol with a concentration of not less than 95.6%, concentrated nitric acid with a concentration of not less than 98%, and alkaline degreasing liquid, and drying after cleaning;

[0043] S4. The forged steel body obtained by the quenching process is subjected to low temperature tempering, the forged steel body is heated to 233°C, kept at this temperature for 27 minutes, heated to 285°C, kept at this temperature for 50 minutes, heated to 322°C, kept at this temperature for 55 minutes, heated to 412°C, kept at this temperature for 71 minutes, heated to 570°C, kept at this temperature for 120 minutes, air-cooled to room temperature, and then heated to 2405°C, kept at this temperature for 1.5 hours to obtain a forged steel matrix. ;

[0044] S5. Grind and polish the forged steel substrate after step S4, perform ultrasonic cleaning, and dry to obtain a high-toughness steel forging for a ball mill.

[0045] Comparative Example 1:

[0046] The invention provides a preparation process of a high-toughness steel forging for a ball mill. The high-toughness steel forging for a ball mill comprises, in mass fraction, C: 1.2%, Si: 0.9%, Mn: 1.0%, Al: 0.25%, Cr: 8%, Re: 0.1%, W: 0.8%, Zr: 0.05%, Nb: 0.02%, Mo: 0.7%, Sr: 0.15%, V: 0.05%, P: 0.05%, S: 0.04%, and the rest is Fe and unavoidable impurities.

[0047] The preparation process of the high-toughness steel forging for the ball mill provided in this comparative example is the same as that in Example 1.

[0048] Comparative Example 2:

[0049] The invention provides a preparation process of a high-toughness steel forging for a ball mill. The high-toughness steel forging for a ball mill comprises, in mass fraction, C: 1.6%, Si: 0.75%, Mn: 1.1%, Al: 0.15%, Cr: 8.9%, Re: 0.03%, W: 0.3%, Zr: 0.05%, Nb: 0.045%, Mo: 0.5%, Sr: 0.1%, V: 0.1%, P: ≤0.03%, S: ≤0.02%, and the rest is Fe and unavoidable impurities.

[0050] The preparation process of the high-toughness steel forging for a ball mill comprises the following steps:

[0051] S1. According to the weight ratio of each chemical component of high-toughness steel forging for ball mill, scrap steel, high-carbon ferrochrome, vanadium-aluminum alloy, tungsten-rhenium alloy, zirconium alloy and prepared raw materials are added into an induction furnace for smelting at a smelting temperature of 1470° C. After the raw materials are completely melted at high temperature, the molten materials are stirred, and then kept still for a period of time under a heat preservation state to obtain a qualified alloy liquid, and then the alloy liquid is cast into a mold to obtain a forged steel casting;

[0052] S2, air-cooling the casting to room temperature, then heating the cooled forged steel casting in sections, heating the casting to 465°C at a heating rate of 6°C / min, keeping the temperature for 15 minutes, heating the casting to 800°C at a heating rate of 7°C / min, keeping the temperature for 25 minutes, heating the casting to 960°C at a heating rate of 3.5-5°C / min, keeping the temperature for 2 hours, performing a quenching process by water quenching, cooling the casting to 500°C, keeping the temperature for 1.5 hours, and cooling the casting to room temperature in air to obtain a forged steel embryo;

[0053] S3, using a cleaning agent to remove impurities and oil stains from the surface of the substrate, the cleaning agent includes one or more of industrial ethylene dichloride, industrial carbon tetrachloride, industrial trichloroethylene, industrial alcohol with a concentration of not less than 95.6%, concentrated nitric acid with a concentration of not less than 98%, and alkaline degreasing liquid, and drying after cleaning;

[0054] S4, subjecting the forged steel body obtained through the quenching process to low-temperature tempering, heating the forged steel body to 240° C., keeping the temperature for 20 min, heating to 300° C., keeping the temperature for 55 min, heating to 350° C., keeping the temperature for 60 min, heating to 435° C., keeping the temperature for 70 min, heating to 600° C., keeping the temperature for 130 min, air-cooling to room temperature, and then heating to 170° C., keeping the temperature for 1.5 h to obtain a forged steel matrix;

[0055] S5. Grind and polish the forged steel substrate after step S4, perform ultrasonic cleaning, and dry to obtain a high-toughness steel forging for a ball mill.

[0056] Table 1 Comparison of steel forging wear per half hour

[0057]

[0058] It can be seen from Table 1 that the wear amount of Examples 1-3 is small and relatively stable under the condition of meeting the material ratio and process requirements, and the wear amount is lower than that of Comparative Examples 1 and 2. Various alloys are added to the high-toughness steel forging to improve the performance of the forged steel, increase its strength, toughness and wear resistance, and the segmented tempering method is beneficial to further stress relief of the wear-resistant balls to prevent cracking and deformation. During the abrasive wear process, large-sized hard particles can resist the micro-cutting effect of the abrasive particles and prevent the abrasive particles from embedding into the matrix: when the abrasive particles are embedded in a certain part of the matrix and sliding cutting occurs, the hard particles can hinder the sliding cutting of the abrasive particles; small-sized particles and fine Bema complex phases can enhance the yield strength of the matrix, improve its ability to resist deformation, provide better support for the hard particles, and prevent large-sized hard particles from falling off when continuously subjected to external forces. After the samples were heated to 940°C, they were subjected to dual-medium quenching, and the resulting structure was a fine martensitic structure. Under impact wear conditions, the wear amount of Comparative Example 2 was greater than that of Example 1. This was because a large amount of martensitic hard-brittle phase structure was not conducive to wear resistance, resulting in a decrease in impact wear performance. Isothermal treatment in a lower bainite phase transformation temperature zone could obtain a bainite duplex structure with better comprehensive mechanical properties, thereby obtaining better wear resistance.

[0059] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, can be combined in any manner.

[0060] Any feature disclosed in this specification (including any additional claims and abstract), unless otherwise stated, may be replaced by other alternative features that are equivalent or have similar purposes. That is, unless otherwise stated, each feature is only an example of a series of equivalent or similar features.

Claims

1. A process for preparing high-toughness steel forging for ball mill, characterized in that: High toughness steel forging for ball mill includes, by mass fraction, C: 1.45-1.75%, Si: 0.75-0.8%, Mn: 1.0-1.12%, Al: 0.1-0.25%, Cr: 8.5-10%, Re: 0.03-0.1%, W: 0.3-0.8%, Zr: 0.05-0.15%, Nb: 0.02-0.045%, Mo: 0.4-0.7%, Sr: 0.05-0.15%, V: 0.05-0.15%, P: ≤0.03%, S: ≤0.02%, and the rest is Fe and unavoidable impurities; The preparation process of high toughness steel forging for ball mill comprises the following steps: S1. According to the weight ratio of each chemical component of high-toughness steel forging for ball mill, scrap steel, high-carbon ferrochrome, vanadium-aluminum alloy, tungsten-rhenium alloy, zirconium alloy and prepared raw materials are added into an induction furnace for smelting. After the raw materials are completely melted at high temperature, the molten materials are stirred, and then kept still for a period of time under a heat preservation state to obtain a qualified alloy liquid, and then the alloy liquid is cast into a mold to obtain a forged steel casting; S2, air-cooling the casting to room temperature, then heating and keeping the cooled forged steel casting in sections, and then performing a quenching process; S3, using a cleaning agent to remove impurities and oil stains from the surface of the substrate, the cleaning agent includes one or more of industrial ethylene dichloride, industrial carbon tetrachloride, industrial trichloroethylene, industrial alcohol with a concentration of not less than 95.6%, concentrated nitric acid with a concentration of not less than 98%, and alkaline degreasing liquid, and drying after cleaning; S4, heating the obtained forged steel blank in sections and then tempering it at low temperature to obtain a forged steel matrix; S5. Grind and polish the forged steel substrate after step S4, perform ultrasonic cleaning, and dry to obtain a high-toughness steel forging for a ball mill.

2. The process for preparing high toughness steel forging for ball mill as claimed in claim 1, characterized in that: The mass fraction of rhenium element in the tungsten-rhenium alloy used in the high-toughness steel forging for the ball mill is less than 10% of the total mass fraction of the tungsten-rhenium alloy.

3. The process for preparing high toughness steel forging for ball mill as claimed in claim 1, characterized in that: The zirconium alloy described in S1 uses one or both of Zr-1Nb and Zr-2.5Nb.

4. The process for preparing high toughness steel forging for ball mill as claimed in claim 1, characterized in that: The smelting temperature in S1 is 1500-1560°C.

5. The process for preparing high toughness steel forging for ball mill as claimed in claim 1, characterized in that: The pouring temperature in S1 is 1420-1450°C.

6. The process for preparing high toughness steel forging for ball mill as claimed in claim 1, characterized in that: The specific process of segmented heating in S2 is as follows: heating the casting to 430-455°C at a heating rate of 6.5-7.5°C / min, keeping warm for 20-35min, heating the casting to 770-790°C at a heating rate of 5.5-6.5°C / min, keeping warm for 25-35min, heating the casting to 940-960°C at a heating rate of 3.5-4.5°C / min, keeping warm for 13-18min, then oil quenching to 730-750°C, then water quenching to room temperature, keeping warm for 30-40min, then heating the casting to 260-270°C at a heating rate of 4-5.5°C / min, keeping warm for 25-30min, heating the casting to 355-365°C at a heating rate of 2-3.5°C / min, keeping warm for 20-30min, and then air cooling to room temperature.

7. The process for preparing high toughness steel forging for ball mill as claimed in claim 1, characterized in that: The specific process of S4 medium and low temperature tempering is as follows: heating the forged steel blank to 225-240°C, keeping warm for 25-30 minutes, heating to 280-290°C, keeping warm for 45-55 minutes, heating to 320-325°C, keeping warm for 50-60 minutes, heating to 410-415°C, keeping warm for 70-75 minutes, heating to 570°C, keeping warm for 120-130 minutes, air cooling to room temperature, and then heating to 240-250°C, keeping warm for 1.5-2 hours to obtain a forged steel matrix.