A method for converting vanadium by co-roasting vanadium slag with sodium and calcium
The method of converting vanadium through sodium-calcium co-roasting of vanadium slag uses one roasting and two leaching processes to simplify the process and improve the vanadium extraction rate. It solves the problems of strict impurity content requirements of vanadium slag and difficult phosphorus purification problems in the existing process, and realizes vanadium Efficient extraction and product quality improvement.
Patent Information
- Application Number
- CN202210957350.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-10
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing vanadium extraction process from vanadium slag has problems such as strict requirements on impurity content in vanadium slag, low extraction rate, complex process, and difficulty in phosphorus purification, which limits the efficient extraction of vanadium.
The method of converting vanadium by co-roasting sodium and calcium vanadium slag is used to generate water-soluble and acid-soluble vanadate through one oxidation roasting and two leaching processes, simplifying the process, improving the extraction rate of vanadium, and through recycling and low pH value. Acid leaching enables efficient separation and purification of vanadium.
It improves the extraction rate of vanadium, simplifies the process flow, enhances the tolerance to the impurity content of vanadium slag, solves the problem of phosphorus removal in acidic vanadium solution, and improves product quality.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of vanadium metallurgy and chemical industry, and in particular relates to a method for converting vanadium by co-roasting vanadium slag with sodium and calcium. Background Art
[0002] Vanadium slag is the main raw material for extracting vanadium oxide. At present, there are two main industrial processes for vanadium extraction: sodium slag roasting conversion-water leaching-ammonium vanadate precipitation (sodium process) and vanadium slag calcination roasting conversion-sulfuric acid leaching-vanadate precipitation (calcification process). The common point of the above two processes is that they both require the addition of salt-forming additives, and both have their own technical difficulties, which affect the vanadium extraction rate. Among them, the sodium process has strict requirements on the content of impurities such as calcium oxide and manganese oxide in the vanadium slag, otherwise the vanadium extraction rate will be greatly reduced; despite this, it is usually necessary to use two sodium roastings and two water leachings to achieve a satisfactory vanadium extraction rate. Therefore, the extraction of vanadium slag is limited by the sodium vanadium extraction process. In the calcification process, the acid leaching method is used to dissolve the vanadium-containing phases such as calcium vanadate, manganese vanadate, and magnesium vanadate in the clinker, which has good adaptability to vanadium slag. However, due to the high vanadium concentration and high temperature of the leaching slurry, vanadium hydrolysis enters the residue and causes vanadium loss, the vanadium leaching rate fluctuates greatly, and the process control is difficult; at the same time, due to the complex polymerization form of phosphorus in the vanadium solution under acidic conditions, purification and phosphorus removal are difficult, which also strictly limits the phosphorus content of vanadium slag. Overall, the existing sodium vanadium extraction and calcification vanadium extraction processes have their own shortcomings, which restrict the efficient extraction of vanadium. Summary of the invention
[0003] In view of the above-mentioned deficiencies in the prior art, the present invention provides a method for converting vanadium by co-roasting vanadium slag with sodium and calcium. On the basis of making full use of the initial impurities such as calcium oxide and manganese oxide in the vanadium slag, a method of one roasting and two leaching is adopted, which not only simplifies the process flow, but also improves the adaptability of the process to the quality of vanadium slag, and solves the problem of vanadium solution purification, so that the process is smooth, the vanadium yield is increased, and the product quality is improved, which is of great significance to the extraction of vanadium.
[0004] In order to achieve the above-mentioned object of the invention, the technical solution adopted by the present invention is:
[0005] A method for converting vanadium by co-roasting vanadium slag with sodium and calcium is provided, comprising the following steps:
[0006] S1. Oxidative roasting of vanadium slag with sodium-calcium additives at 800° C. to 860° C. for 30 to 90 minutes to obtain sodium-calcium roasted clinker;
[0007] S2, leaching the sodium-calcium roasted clinker with water or acid leaching vanadium solution, and separating the solid and liquid to obtain a weakly alkaline sodium vanadate solution and a primary residue;
[0008] S3, acid leaching the primary residue and separating the solid and liquid to obtain acid leaching vanadium liquid and secondary residue;
[0009] S4, returning the acid leaching vanadium solution to step S2 to leach the vanadium slag sodium calcium roasted clinker;
[0010] S5. Processing the weakly alkaline sodium vanadate solution to obtain a vanadium oxide product.
[0011] Furthermore, in step S1, the main components of the vanadium slag are: V2O5 10%-25%, SiO2 10-20%, FeO 30-40%, MnO 5%-10%, MgO 1%-5%, CaO 5%-10%.
[0012] Furthermore, in step S1, the particle size of the vanadium slag is 0.074 mm to 0.100 mm.
[0013] Furthermore: in step S1, the sodium salt additive in the sodium-calcium additive is at least one of sodium carbonate, sodium bicarbonate and sodium chloride.
[0014] Further: in step S1, the calcium salt additive in the sodium-calcium additive is at least one of calcium carbonate, calcium oxalate, calcium oxide, calcium hydroxide, calcium chloride, and high-calcium vanadium slag.
[0015] Further: in step S1, the particle size of the calcium salt additive in the sodium-calcium additive is 0.050 mm to 0.100 mm.
[0016] Further: in step S2, the leaching temperature of the sodium-lime roasted clinker is 80°C to boiling; the leaching time is 30 to 90 minutes; and the leaching liquid-solid ratio is 1.5 to 3:1 mL / g.
[0017] Further: in step S3, the primary residue acid leaching temperature is 50°C to 80°C; the leaching time is 30 to 90 min; and the leaching liquid-solid ratio is 2.0 to 4.0:1 mL / g.
[0018] Further: in step S3, the acid used for acid leaching of the primary residue is sulfuric acid or hydrochloric acid; the pH value of the acid leaching slurry is 0.5 to 1.5.
[0019] The beneficial effects of the present invention are:
[0020] The present invention adopts vanadium slag and sodium-calcium additives to co-roast to obtain sodium-calcium roasted clinker, wherein the vanadium exists in two forms of water-soluble vanadate and acid-soluble vanadate, and vanadium in the vanadium slag can be separated simply and efficiently by sequentially using water or low-vanadium solution leaching and acid leaching. The present invention simplifies the existing vanadium extraction process, improves the vanadium extraction rate, solves the technical problem of phosphorus removal and purification in acidic vanadium solution, improves the tolerance of the process to the impurity content in the vanadium slag, and has broad application prospects. DETAILED DESCRIPTION
[0021] The specific implementation modes of the present invention are described below so that those skilled in the art can understand the present invention. However, it should be clear that the present invention is not limited to the scope of the specific implementation modes. For those of ordinary skill in the art, as long as various changes are within the spirit and scope of the present invention as defined and determined by the attached claims, these changes are obvious, and all inventions and creations utilizing the concept of the present invention are protected.
[0022] Specifically, the present invention provides a method for converting vanadium by co-roasting vanadium slag with sodium and calcium, the method comprising the following steps:
[0023] a. Oxidative roasting of vanadium slag with sodium-calcium additives at 800°C to 860°C to obtain sodium-calcium roasted clinker;
[0024] b. Leaching the sodium-calcium roasted clinker with an acidic low-vanadium solution (primary leaching), and separating the solid from the liquid to obtain a weakly alkaline sodium vanadate solution (weakly alkaline high-vanadium solution, referred to as high-vanadium solution) and a primary residue (high-vanadium residue);
[0025] c. Acid leaching of the primary residue (secondary leaching) and solid-liquid separation to obtain acid leaching vanadium liquid (acidic low-vanadium liquid, referred to as low-vanadium liquid) and secondary residue (low-vanadium residue, waste residue);
[0026] d. Return the low-vanadium solution directly to step b to leach the sodium-calcium roasted clinker;
[0027] e. The high-vanadium liquid can be treated by conventional methods to produce vanadium oxide products.
[0028] The vanadium slag of the present invention is produced in the process of steelmaking with vanadium-containing molten iron, and most of the vanadium in the vanadium slag of the present invention exists in the form of FeV2O4 and MnV2O4 in the vanadium-containing spinel. The components of the vanadium slag are: V2O5 10%-25%, SiO2 10-20%, FeO 30-40%, MnO 5%-10%, MgO 1%-5%, and CaO 5%-10%.
[0029] In step a, the vanadium slag is oxidized and roasted at 800°C to 860°C to convert vanadium-containing minerals such as FeV2O4 and MnV2O4 into water-soluble sodium vanadate (NaVO3) and acid-soluble calcium vanadate (Ca(VO3)2) to obtain vanadium slag sodium-calcium roasted clinker.
[0030] In step b, the vanadium slag sodium calcium roasted clinker is leached with low vanadium liquid (high vanadium residue acid leaching liquid) to obtain a weakly alkaline high vanadium liquid, which can be directly purified and dephosphorized using existing mature purification processes, solving the problem of descaling and purification of existing acidic vanadium solutions.
[0031] In step c, the high-vanadium residue produced in step b is leached with acid. Since the vanadium content is relatively low, and the leaching solution is returned to step b for recycling, a lower leaching pH value, a higher leaching temperature, and a larger liquid-solid ratio can be used, which is conducive to fully leaching the vanadium in the high-vanadium residue and improving the comprehensive extraction rate of vanadium.
[0032] The existing industrial vanadium slag vanadium extraction processes are mainly sodium process and calcification process. The reaction of generating vanadate during roasting is as follows:
[0033] (I) Sodium roasting of vanadium slag
[0034] 4FeV2O4+4Na2O+5O2=8NaVO3+2Fe2O3
[0035] 4MnV2O4+4Na2O+5O2=8NaVO3+2Mn2O3
[0036] Na2O represents sodium salt additives such as Na2CO3, NaHCO3, and NaCl. Although the water-soluble sodium vanadate (NaVO3) generated by the reaction has a good effect on vanadium leaching, it also has the following side reactions:
[0037] 4FeV2O4+4CaO+5O2=4Ca(VO3)2+2Fe2O3
[0038] 4MnV2O4+4CaO+5O2=4Ca(VO3)2+2Mn2O3
[0039] MnV2O4+O2=Mn(VO3)2
[0040] P2O5+Na2O=Na3PO4
[0041] Vanadium-containing minerals such as Ca(VO3)2 and Mn(VO3)2 produced by side reactions are insoluble in water and remain in the residue during the leaching process, reducing the leaching rate of vanadium. The Na3PO4 generated by the reaction is soluble in water, and a weak alkaline solution is obtained by leaching. Phosphorus can be easily removed by conventional phosphorus removal and purification processes. Despite this, sodium vanadium extraction has strict restrictions on the CaO and MnO content of vanadium slag and has poor adaptability to vanadium slag.
[0042] (II) Calcification roasting of vanadium slag
[0043] 4FeV2O4+4CaO+5O2=4Ca(VO3)2+2Fe2O3
[0044] 4MnV2O4+4CaO+5O2=4Ca(VO3)2+2Mn2O3
[0045] 4FeV2O4+4MnO+5O2=4Mn(VO3)2+2Fe2O3
[0046] MnV2O4+O2=Mn(VO3)2
[0047] 4FeV2O4+4MgO+5O2=4Mg(VO3)2+2Fe2O3
[0048] CaO, MnO, and MgO can come from vanadium slag or be external components. The reaction converts FeV2O4, MnV2O4 and other vanadium-containing minerals in vanadium slag into acid-soluble Ca(VO3)2, Mn(VO3)2 and other vanadates. The vanadium in them can be dissolved by acid leaching process. The reaction is as follows:
[0049] 5Ca(VO3)2+6H + +3SO4 2- +4H2O=H2V 10 O 28 4- +2Ca 2+- +3CaSO4·2H2O
[0050] 5Mn(VO3)2+6H + =H2V 10 O 28 4- +5Mn 2+ +3H2O
[0051] For vanadium slag calcified clinker, due to the high vanadium content, high leaching temperature or too low leaching pH value, there are the following side reactions:
[0052] H2V 10 O 28 4- +4H + =5V2O5+3H2O
[0053] The hydrolysis-generated colloid enters the residue and causes vanadium loss, which reduces the vanadium extraction rate. Therefore, in the usual process operation, both the pH value of the reaction system and the leaching reaction temperature must be controlled. Due to these conditions, the vanadium extraction rate is limited.
[0054] In view of the above technical analysis, the present invention starts with improving the roasting conditions of vanadium slag, and better solves the existing technical problems. The main reactions are as follows:
[0055] (I) Sodium-calcium vanadium slag roasting reaction
[0056] 4FeV2O4+2Na2O+2CaO+5O2=2Na2Ca(VO3)4+2Fe2O3
[0057] Na2O in the reaction represents sodium salt additives such as Na2CO3, NaHCO3, and NaCl; CaO represents calcium salt additives such as calcium carbonate, calcium oxalate, calcium oxide, calcium hydroxide, and calcium chloride, which can come from the vanadium slag itself or be an external additive; if the content of vanadium slag itself is high, no external additive is needed, that is, the tolerance for the impurity content of the vanadium slag itself is relaxed. The reaction generates sodium calcium vanadate (Na2Ca(VO3)4) with good water solubility, and the sodium vanadate (NaVO3) can be dissolved by water leaching, and the calcium vanadate (Ca(VO3)2) can be leached out by acid.
[0058] (II) Calcium sodium vanadate leaching reaction
[0059] Water immersion reaction: Na2Ca(VO3)4=2VO3 - +2Na + +Ca(VO3)2
[0060] Water immersion reaction: Ca(VO3)2+4H + +SO4 2- =2VO2 + +CaSO4+2H2O
[0061] The water leaching reaction in the leaching reaction is the same as that of sodium vanadium extraction, but the leaching object is sodium calcium vanadate (Na2Ca(VO3)4) in the clinker, while the leaching object of the former is sodium vanadate (NaVO3); the acid leaching reaction is different from the calcification vanadium extraction, and the leaching object is calcium vanadate (Ca(VO3)2), but the leaching product of the present invention is anhydrous calcium sulfate (CaSO4), and the acid leaching product of calcification vanadium extraction is dihydrate calcium sulfate (CaSO4·2H2O). The difference is that the pH value of the leaching of the present invention can be as low as 0.5-1.5, while the pH value of calcification vanadium extraction can only be controlled at 2.5-3.5, or even 2.8-3.3. The advantage is that the leaching rate of vanadium is higher. Since the vanadium concentration itself is low, the hydrolysis reaction of vanadium will not occur even at a higher leaching temperature, so the leaching rate of vanadium of the present invention is higher.
[0062] (III) Low-vanadium liquid return water immersion reaction
[0063] Na2Ca(VO3)4+2VO2 + +2Na + +4OH - =4VO3 - +4Na + +Ca(VO3)2+2H2O
[0064] Obviously, the return of low-vanadium liquid for recycling not only utilizes the vanadium but also the acid in it. More importantly, it produces a weakly alkaline high-vanadium liquid. Mature phosphorus removal and purification processes can be used. Even if there are calcium, manganese, magnesium and other ions in it, they will be hydrolyzed and precipitated out, thus achieving the purification of the high-vanadium liquid.
[0065] The present invention will be further described in detail below through specific examples.
[0066] The vanadium slag is ground to a particle size of 0.074 mm to 0.100 mm for later use. The main components of the vanadium slag powder are 16.8% V2O5, 17.6% SiO2, 38.6% FeO, 8.5% MnO, 6.5% CaO, and 3.7% MgO.
[0067] Example 1
[0068] Take 200g of vanadium slag powder, add 6.92g of calcium carbonate and 15.38g of sodium carbonate, and oxidize and roast at 800℃ for 90min to obtain vanadium slag sodium calcium roasted clinker. Add 445ml of water to the clinker and leach for 90min under boiling state. After filtration, the vanadium content of high vanadium residue is 3.05%. The high vanadium residue is leached with sulfuric acid, and the pH value of the leaching slurry is controlled to 1.5. Leach at 50℃ for 90min, and the solid-liquid separation obtains low vanadium liquid and low vanadium residue. The vanadium content of the low vanadium residue is 0.35%. The total vanadium conversion rate is calculated to be 96.45%.
[0069] Example 2
[0070] Take 200g vanadium slag powder, add 5.80g calcium oxalate and 24.69g sodium bicarbonate, and oxidize and roast at 840℃ for 60min to obtain vanadium slag sodium calcium roasted clinker. Add 346ml water to the clinker and leach at 80℃ for 60min. After filtering, the vanadium content of the high vanadium residue is 3.37%. The high vanadium residue is leached with hydrochloric acid, and the pH value of the leaching slurry is controlled to 1.0. Leach at 80℃ for 60min, and the solid-liquid separation is used to obtain low vanadium liquid and low vanadium residue. The vanadium content of the low vanadium residue is 0.41%. The total vanadium conversion rate is calculated to be 95.54%.
[0071] Example 3
[0072] Take 200g of vanadium slag powder, add 4.35g of calcium oxide and 17.37g of sodium chloride, and oxidize and roast at 800℃ for 30min to obtain vanadium slag sodium calcium roasted clinker. Add 555ml of water to the clinker and leach at 90℃ for 30min. After filtering, the vanadium content of the high-vanadium residue is 3.89%. The high-vanadium residue is leached with sulfuric acid, and the pH value of the leaching slurry is controlled to 0.5. Leach at 50℃ for 30min, and the solid-liquid separation is used to obtain low-vanadium liquid and low-vanadium residue. The vanadium content of the low-vanadium residue is 0.39%. The total vanadium conversion rate is calculated to be 95.81%.
[0073] Example 4
[0074] Take 200g of vanadium slag powder, add 6.34g of calcium hydroxide and 11.00g of sodium hydroxide, and oxidize and roast at 800℃ for 80min to obtain vanadium slag sodium calcium roasted clinker. Add 650ml of water to the clinker and leach at 80℃ for 80min. After filtering, the vanadium content of the high-vanadium residue is 4.28%. The high-vanadium residue is leached with hydrochloric acid, and the pH value of the leaching slurry is controlled to 1.0. Leach at 80℃ for 80min, and the solid-liquid separation is used to obtain low-vanadium liquid and low-vanadium residue. The vanadium content of the low-vanadium residue is 0.45%. The total vanadium conversion rate is calculated to be 95.13%.
[0075] Example 5
[0076] Take 200g of vanadium slag powder, add 10.46g of calcium chloride and 12.10g of sodium carbonate, and oxidize and roast at 860℃ for 90min to obtain vanadium slag sodium calcium roasted clinker. Add 625ml of water to the clinker and leach at 85℃ for 85min. After filtering, the vanadium content of the high-vanadium residue is 4.71%. The high-vanadium residue is leached with sulfuric acid, and the pH value of the leaching slurry is controlled to 1.3. The leaching is carried out at 60℃ for 60min. The solid-liquid separation obtains low-vanadium liquid and low-vanadium residue. The vanadium content of the low-vanadium residue is 0.37%. The total vanadium conversion rate is calculated to be 95.79%.
[0077] Example 6
[0078] Take 200g vanadium slag powder, add 9.77g calcium carbonate and 18.95g sodium bicarbonate, and oxidize and roast at 830℃ for 70min to obtain vanadium slag sodium calcium roasted clinker. Add 549ml water to the clinker and leach at 95℃ for 35min. After filtering, the vanadium content of the high vanadium residue is 4.17%. The high vanadium residue is leached with hydrochloric acid, and the pH value of the leaching slurry is controlled to 0.8. Leach at 80℃ for 50min, and the solid-liquid separation is used to obtain low vanadium liquid and low vanadium residue. The vanadium content of the low vanadium residue is 0.41%. The total vanadium conversion rate is calculated to be 95.30%.
[0079] Example 7
[0080] Take 200g vanadium slag powder, add 3.73g calcium oxide and 16.82g sodium chloride, and oxidize and roast at 810℃ for 50min to obtain vanadium slag sodium calcium roasted clinker. Add 575ml water to the clinker and leach at 85℃ for 55min. After filtering, the vanadium content of the high vanadium residue is 3.51%. The high vanadium residue is leached with sulfuric acid, and the pH value of the leaching slurry is controlled to 1.1. It is leached at 60℃ for 70min, and the solid-liquid separation is used to obtain low vanadium liquid and low vanadium residue. The vanadium content of the low vanadium residue is 0.43%. The total vanadium conversion rate is calculated to be 95.50%.
[0081] Example 8
[0082] Take 200g vanadium slag powder, add 4.27g calcium hydroxide and 13.60g sodium hydroxide, and oxidize and roast at 830℃ for 40min to obtain vanadium slag sodium calcium roasted clinker. Add 395ml water to the clinker and leach at 96℃ for 35min. After filtering, the vanadium content of the high vanadium residue is 3.15%. The high vanadium residue is leached with hydrochloric acid, and the pH value of the leaching slurry is controlled to 0.8. The leaching is carried out at 80℃ for 80min. The solid-liquid separation obtains low vanadium liquid and low vanadium residue. The vanadium content of the low vanadium residue is 0.38%. The total vanadium conversion rate is calculated to be 96.14%.
[0083] The present invention adopts vanadium slag and sodium-calcium additives to co-roast to obtain sodium-calcium roasted clinker, wherein the vanadium exists in two forms of water-soluble vanadate and acid-soluble vanadate, and vanadium in the vanadium slag can be separated simply and efficiently by sequentially using water or low-vanadium solution leaching and acid leaching. The present invention simplifies the existing vanadium extraction process, improves the vanadium extraction rate, solves the technical problem of phosphorus removal and purification in acidic vanadium solution, improves the tolerance of the process to the impurity content in the vanadium slag, and has broad application prospects.
[0084] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0085] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for converting vanadium by co-roasting vanadium slag with sodium and calcium, It is characterized in that The following steps are involved: S1. Oxidative roasting of vanadium slag with sodium-calcium additives at 800°C-860°C for 30-90 minutes to obtain sodium-calcium roasted clinker; S2, leaching the sodium-calcium roasted clinker with water or acid leaching vanadium solution, and separating the solid and liquid to obtain a weakly alkaline sodium vanadate solution and a primary residue; S3, acid leaching the primary residue and separating the solid and liquid to obtain acid leaching vanadium liquid and secondary residue; S4, returning the acid leaching vanadium solution to step S2 to leach the vanadium slag sodium calcium roasted clinker; S5, producing and treating the weakly alkaline sodium vanadate solution to obtain a vanadium oxide product; In step S2, the sodium-lime roasted clinker leaching temperature is 80°C to boiling temperature; the leaching time is 30 to 90 minutes; the leaching liquid-solid ratio is 1.5 to 3:1 mL / g; In step S3, the acid leaching temperature of the primary residue is 50°C to 80°C; the leaching time is 30 to 90 minutes; and the leaching liquid-solid ratio is 2.0 to 4.0:1 mL / g; In step S3, the acid used for acid leaching of the primary residue is sulfuric acid or hydrochloric acid; and the pH value of the acid leaching slurry is 0.5-1.
5.
2. The method for converting vanadium by co-roasting vanadium slag with sodium and calcium according to claim 1, It is characterized in that In step S1, the main components of the vanadium slag are: V 2 O 5 10%~25%, SiO 2 10~20%, FeO 30~40%, MnO 5%~10%, MgO 1%~5%, CaO 5%~10%.
3. The method for converting vanadium by co-roasting vanadium slag with sodium and calcium according to claim 2, It is characterized in that In step S1, the particle size of the vanadium slag is 0.074 mm to 0.100 mm.
4. The method for converting vanadium by co-roasting vanadium slag with sodium and calcium according to claim 1, Features: In step S1, the sodium salt additive in the sodium-calcium additive is at least one of sodium carbonate, sodium bicarbonate and sodium chloride.
5. The method for converting vanadium by co-roasting vanadium slag with sodium and calcium according to claim 1, Features: In step S1, the calcium salt additive in the sodium-calcium additive is at least one of calcium carbonate, calcium oxalate, calcium oxide, calcium hydroxide, calcium chloride, and high-calcium vanadium slag.
6. The method for converting vanadium by co-roasting vanadium slag with sodium and calcium according to claim 4, Features: In step S1, the particle size of the calcium salt additive in the sodium-calcium additive is 0.050 mm to 0.100 mm.