Exposed aggregate concrete and construction method thereof

By using specific combinations of aggregates and cementitious agents, adjusting the water-cement ratio and mixing method, the problem of dehydration of exposed aggregate concrete in summer construction is solved, and good compression resistance and permeability effect in high temperature environments is achieved.

CN115959859BActive Publication Date: 2024-11-15QIONGHAI XIN HAI CONCRETE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211514396.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-30
Publication Date
2024-11-15
Estimated Expiration
2042-11-30

AI Technical Summary

Technical Problem

During summer construction, exposed aggregate concrete is prone to dehydration, resulting in a shortening of initial settling time and a decrease in pavement effect. The existing technology has failed to effectively solve this problem.

Method used

The base material is prepared by adjusting the water-cement ratio and mixing method using aggregates including 1-3mm, 12-16mm and 20-25mm gravel and cementitious agents. and slurry to ensure the full combination of aggregate and cementitious agent to avoid dehydration of aggregate.

Benefits of technology

It significantly improves the compressive effect and permeability of exposed aggregate concrete, avoids aggregate dehydration during construction in high temperature environments, and ensures the stability and water permeability of pavement.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a construction method of exposed aggregate concrete, wherein the exposed aggregate concrete comprises aggregate and a binder, wherein the aggregate comprises crushed stones with sizes of 1-3 mm, 12-16 mm and 20-25 mm, and the binder comprises hydroxypropyl methylcellulose, clay mineral powder and steel fiber. In the construction method, the water-cement ratio and the mixing method are adjusted according to the size of the crushed stones to improve the compression resistance and permeability of the exposed aggregate concrete pavement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of concrete, and in particular to exposed concrete and a construction method thereof. Background Art

[0002] The common method of paving sidewalks in landscape projects is to use exposed aggregate concrete for construction. Exposed aggregate concrete is a new type of concrete process in recent years. It has strong water permeability and can also be artistically decorated according to the needs of landscape projects to form a better landscape effect. Exposed aggregate concrete is a porous road surface formed by combining cementing materials and aggregates. Exposed aggregate permeable concrete can increase the permeable and breathable area of ​​the city, strengthen the heat and moisture exchange between the surface and the air, regulate the urban climate, reduce the surface temperature, and help alleviate the urban "heat island effect". Chinese patent CN114369979A discloses an exposed aggregate permeable concrete pavement and its construction process, including a 200mm thick graded crushed stone cushion layer at the bottom, a sand filter layer, a strength C25 permeable concrete layer, a strength C25 exposed aggregate permeable concrete layer arranged in sequence above it, and a colorless transparent layer of double propylene polyurethane sprayed on the top layer; a unique pore structure is formed by matching multiple layers of concrete layers with different particle sizes, thereby improving the water permeability of the exposed aggregate permeable concrete pavement, and through strict construction control, the arrangement of the surface aggregate is improved, so that the aggregate is not easy to fall off. Chinese patent CN109761538A discloses an exposed aggregate concrete and its construction method, wherein the exposed aggregate concrete includes aggregate, polyurethane binder, and finishing agent. The construction method includes: preparing a three-dimensional pattern template; after mixing the aggregate and the polyurethane binder, pouring the concrete for the first time on the three-dimensional pattern template; after the concrete solidifies, removing the three-dimensional pattern template to obtain preformed concrete, pouring the concrete for the second time on the preformed concrete, and then curing and forming, and then spraying the finishing agent. The above two construction methods both solve the technical problem of preventing aggregate from falling off. None of the above patents mentions that in summer construction, the weather is hot and the exposed aggregate concrete is prone to dehydration, resulting in a shortened initial setting time and a reduced pavement paving effect. Summary of the invention

[0003] In view of this, the present invention proposes exposed aggregate concrete and a construction method thereof to solve the above problems.

[0004] The technical solution of the present invention is achieved in this way:

[0005] An exposed aggregate concrete comprises aggregate and a binder, wherein the aggregate comprises crushed stones with sizes of 1-3 mm, 12-16 mm and 20-25 mm, and the binder comprises hydroxypropyl methylcellulose, clay mineral powder and steel fiber.

[0006] Furthermore, the mass ratio of hydroxypropyl methylcellulose, clay mineral powder and steel fiber is 1:3-10:0.1-0.7.

[0007] Furthermore, the length of the steel fiber is 20-30 mm, and the aspect ratio is 1:50-60.

[0008] Further, the following steps are included:

[0009] (1) crushed stones with sizes of 1-3 mm and 12-16 mm, a binder, and cement are mixed to prepare a base material;

[0010] (2) Mix 1-3 mm and 20-25 mm crushed stones, binder and cement, and lay them on the surface of the base material.

[0011] Furthermore, in step (1), by weight, the crushed stone with a size of 1-3 mm is 5-7 parts, the crushed stone with a size of 12-16 mm is 9-11 parts, the binder is 0.8-1.2 parts, and the cement is 25-28 parts, and the water-cement ratio is 0.35-0.37.

[0012] Furthermore, in step (1), the base material is laid to a thickness of 230-250 mm.

[0013] Furthermore, in step (1), the base material is laid to a thickness of 240 mm.

[0014] Furthermore, in step (1), the mass ratio of hydroxypropyl methylcellulose, clay mineral powder and steel fiber in the binder is 1:3-5:0.4-0.7.

[0015] Furthermore, in step (2), by weight, the crushed stone with a size of 1-3 mm is 1-2 parts, the crushed stone with a size of 20-25 mm is 10-12 parts, the binder is 2-4 parts, the cement is 30-33 parts, and the water-cement ratio is 0.42-0.44.

[0016] Furthermore, in step (2), the laying thickness is 280-320 mm.

[0017] Furthermore, in step (2), the laying thickness is 300 mm.

[0018] Furthermore, in step (2), the mass ratio of hydroxypropyl methylcellulose, clay mineral powder and steel fiber is 1:6-10:0.1-0.5.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] In the present invention, aggregate and binder are used to prepare exposed aggregate concrete, the aggregate includes crushed stones with sizes of 1-3mm, 12-16mm and 20-25mm, and the binder includes hydroxypropyl methylcellulose, clay mineral powder and steel fiber. Crushed stones with sizes of 1-3mm, 12-16mm and binder are used to prepare base materials, the water-cement ratio is adjusted, and the crushed stones and 30% of the total water consumption are stirred during the mixing process, and then cement is added for stirring, and finally the binder and the remaining water are added for stirring to obtain the base material. Crushed stones with sizes of 1-3mm, crushed stones with sizes of 20-25mm and binder are mixed, the water-cement ratio is adjusted, crushed stones with sizes of 1-3mm, cement and water are mixed during the mixing process, and then crushed stones with sizes of 20-25mm are added for mixing, and then laid on the base material. The exposed aggregate concrete prepared by the present invention has good compression resistance and permeability effects. Construction under high temperature environment can avoid the occurrence of aggregate dehydration and the like. DETAILED DESCRIPTION

[0021] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention.

[0022] Example 1

[0023] (1) Mix crushed stones with an average size of 1 mm and 12 mm, a binder, and cement. The crushed stones with an average size of 1 mm are 5 parts, the crushed stones with an average size of 12 mm are 9 parts, the binder is 0.8 parts, and the cement is 25 parts. The water-cement ratio is 0.35. The mass ratio of hydroxypropyl methylcellulose, clay mineral powder, and steel fiber in the binder is 1:3:0.4. The length of the steel fiber is 20 mm, and the aspect ratio is 1:50. Stir the crushed stones and 30% of the total water for 2 minutes, then add cement and stir for 50 seconds, and finally add the binder and the remaining water and stir for 3 minutes to obtain a base material. The laying thickness of the base material is 230 mm.

[0024] (2) After the base material has been laid for 2 hours, 1 mm and 20 mm crushed stones, a binder and cement are mixed and laid on the surface of the base material. By weight, the crushed stones with a size of 1 mm are 1 part, the crushed stones with a size of 20 mm are 10 parts, the binder is 2 parts, and the cement is 30 parts. The water-cement ratio is 0.42. The mass ratio of hydroxypropyl methylcellulose, clay mineral powder and steel fiber in the binder is 1:6:0.1. The length of the steel fiber is 20 mm, and the aspect ratio is 1:50. The crushed stones with a size of 1 mm, cement and water are mixed and stirred for 3 minutes, and the crushed stones with a size of 20 mm and the binder are added and stirred for 8 minutes to obtain a slurry. The laying thickness of the slurry is 280 mm.

[0025] Example 2

[0026] (1) Mix crushed stones with an average size of 3 mm and 16 mm, a binder, and cement, wherein the crushed stones with an average size of 3 mm are 7 parts, the crushed stones with an average size of 16 mm are 11 parts, the binder is 1.2 parts, and the cement is 28 parts. The water-cement ratio is 0.37. The mass ratio of hydroxypropyl methylcellulose, clay mineral powder, and steel fiber in the binder is 1:5:0.7. The length of the steel fiber is 30 mm, and the aspect ratio is 1:60. Stir the crushed stones and 40% of the total water for 3 minutes, then add cement and stir for 60 seconds, and finally add the binder and the remaining water and stir for 4 minutes to obtain a base material. The laying thickness of the base material is 250 mm.

[0027] (2) After the base material has been laid for 3 hours, 3 mm and 25 mm crushed stones, a binder and cement are mixed and laid on the surface of the base material. By weight, the crushed stones with a size of 3 mm are 2 parts, the crushed stones with a size of 25 mm are 12 parts, the binder is 4 parts and the cement is 33 parts. The water-cement ratio is 0.44. The mass ratio of hydroxypropyl methylcellulose, clay mineral powder and steel fiber in the binder is 1:10:0.5. The length of the steel fiber is 30 mm and the aspect ratio is 1:60. The crushed stones with a size of 3 mm, cement and water are mixed and stirred for 4 minutes, and the crushed stones with a size of 25 mm and the binder are added and stirred for 10 minutes to obtain a slurry. The laying thickness of the slurry is 320 mm.

[0028] Example 3

[0029] (1) Mix crushed stones with an average size of 2 mm and 14 mm, a binder, and cement, wherein the crushed stones with an average size of 2 mm are 6 parts, the crushed stones with an average size of 14 mm are 10 parts, the binder is 1 part, and the cement is 27 parts. The water-cement ratio is 0.36. The mass ratio of hydroxypropyl methylcellulose, clay mineral powder, and steel fiber in the binder is 1:4:0.5. The length of the steel fiber is 25 mm, and the aspect ratio is 1:60. Stir the crushed stones and 35% of the total water for 2.5 minutes, then add cement and stir for 55 seconds, and finally add the binder and the remaining water and stir for 3.5 minutes to obtain a base material. The laying thickness of the base material is 240 mm.

[0030] (2) After the base material has been laid for 2.5 hours, 2 mm and 25 mm crushed stone, binder and cement are mixed and laid on the surface of the base material. By weight, the crushed stone with a size of 2 mm is 1.5 parts, the crushed stone with a size of 25 mm is 11 parts, the binder is 3 parts, and the cement is 32 parts. The water-cement ratio is 0.43. The mass ratio of hydroxypropyl methylcellulose, clay mineral powder and steel fiber in the binder is 1:8:0.3. The length of the steel fiber is 20 mm, and the aspect ratio is 1:60. The crushed stone with a size of 2 mm, cement and water are mixed and stirred for 3.5 minutes, and the crushed stone with a size of 25 mm and the binder are added and stirred for 9 minutes to obtain a slurry. The slurry is laid with a thickness of 300 mm.

[0031] Example 4

[0032] (1) Mix crushed stones with an average size of 2 mm and 14 mm, a binder, and cement. The crushed stones with an average size of 2 mm are 6 parts, the crushed stones with an average size of 14 mm are 10 parts, the binder is 1 part, and the cement is 27 parts. The water-cement ratio is 0.36. The mass ratio of hydroxypropyl methylcellulose, clay mineral powder, and steel fiber in the binder is 1:4:0.5. The length of the steel fiber is 25 mm, and the aspect ratio is 1:60. Mix the crushed stones with an average size of 2 mm and 14 mm, the binder, and cement, and stir for 8 minutes to obtain a base material. The laying thickness of the base material is 240 mm.

[0033] (2) After the base material has been laid for 2.5 hours, 2 mm and 25 mm crushed stone, binder and cement are mixed and laid on the surface of the base material. By weight, the crushed stone with a size of 2 mm is 1.5 parts, the crushed stone with a size of 25 mm is 11 parts, the binder is 3 parts, the cement is 32 parts, and the water-cement ratio is 0.43. The mass ratio of hydroxypropyl methylcellulose, clay mineral powder and steel fiber in the binder is 1:8:0.3. The length of the steel fiber is 20 mm, and the aspect ratio is 1:60. The crushed stone with a size of 2 mm, cement, crushed stone with a size of 25 mm, the binder and water are mixed and stirred for 10 minutes to obtain a slurry. The slurry is laid to a thickness of 300 mm.

[0034] Example 5

[0035] (1) Mix crushed stones with average sizes of 2 mm and 14 mm, a binder, and cement. The crushed stones with average sizes of 2 mm are 6 parts, the crushed stones with average sizes of 14 mm are 10 parts, the binder is 1 part, and the cement is 27 parts. The water-cement ratio is 0.36. The mass ratio of hydroxypropyl methylcellulose, clay mineral powder, and steel fiber in the binder is 1:4:0.5. The length of the steel fiber is 25 mm, and the aspect ratio is 1:60. Stir the crushed stones, water, and cement for 2.5 minutes, and finally add the binder and the remaining water and stir for 3.5 minutes to obtain a base material. The laying thickness of the base material is 240 mm.

[0036] (2) After the base material has been laid for 2.5 hours, 2 mm and 25 mm crushed stone, binder and cement are mixed and laid on the surface of the base material. By weight, the crushed stone with a size of 2 mm is 1.5 parts, the crushed stone with a size of 25 mm is 11 parts, the binder is 3 parts, and the cement is 32 parts. The water-cement ratio is 0.43. The mass ratio of hydroxypropyl methylcellulose, clay mineral powder and steel fiber in the binder is 1:8:0.3. The length of the steel fiber is 20 mm, and the aspect ratio is 1:60. The crushed stone with a size of 2 mm, cement and water are mixed and stirred for 3.5 minutes, and the crushed stone with a size of 25 mm and the binder are added and stirred for 9 minutes to obtain a slurry. The laying thickness of the slurry is 300 mm.

[0037] Comparative Example 1

[0038] (1) Mix crushed stone with an average size of 2 mm, a binder, and cement, wherein the crushed stone with an average size of 2 mm is 15 parts, the binder is 1 part, and the cement is 27 parts. The water-cement ratio is 0.36. The mass ratio of hydroxypropyl methylcellulose, clay mineral powder, and steel fiber in the binder is 1:4:0.5. The length of the steel fiber is 25 mm, and the aspect ratio is 1:60. Stir the crushed stone and 35% of the total water for 2.5 minutes, then add cement and stir for 55 seconds, and finally add the binder and the remaining water and stir for 3.5 minutes to obtain a base material. The laying thickness of the base material is 200 mm;

[0039] (2) After the base material has been laid for 2.5 hours, 25 mm crushed stone, binder and cement are mixed and laid on the surface of the base material. By weight, the crushed stone with a size of 25 mm is 11 parts, the binder is 3 parts, the cement is 32 parts, and the water-cement ratio is 0.43. The mass ratio of hydroxypropyl methylcellulose, clay mineral powder and steel fiber in the binder is 1:8:0.3. The length of the steel fiber is 20 mm, and the aspect ratio is 1:60. Mix 2 mm crushed stone, cement and water and stir for 3.5 minutes, add 25 mm crushed stone and binder and stir for 9 minutes to prepare slurry. The slurry is laid with a thickness of 400 mm.

[0040] Comparative Example 2

[0041] (1) Mix crushed stones with an average size of 2 mm and 14 mm, a binder, and cement, wherein the crushed stones with an average size of 2 mm are 6 parts, the crushed stones with an average size of 14 mm are 10 parts, the binder is 1 part, and the cement is 27 parts. The water-cement ratio is 0.36. The mass ratio of hydroxypropyl methylcellulose, clay mineral powder, and steel fiber in the binder is 1:10:1. The length of the steel fiber is 25 mm, and the aspect ratio is 1:60. Stir the crushed stones and 35% of the total water for 2.5 minutes, then add cement and stir for 55 seconds, and finally add the binder and the remaining water and stir for 3.5 minutes to obtain a base material. The laying thickness of the base material is 240 mm.

[0042] (2) After the base material has been laid for 2.5 hours, 2 mm and 25 mm crushed stone, binder and cement are mixed and laid on the surface of the base material. By weight, the crushed stone with a size of 2 mm is 1.5 parts, the crushed stone with a size of 25 mm is 11 parts, the binder is 3 parts, and the cement is 32 parts. The water-cement ratio is 0.43. The mass ratio of hydroxypropyl methylcellulose, clay mineral powder and steel fiber in the binder is 1:3:1. The length of the steel fiber is 20 mm, and the aspect ratio is 1:60. The crushed stone with a size of 2 mm, cement and water are mixed and stirred for 3.5 minutes, and the crushed stone with a size of 25 mm and the binder are added and stirred for 9 minutes to obtain a slurry. The slurry is laid with a thickness of 300 mm.

[0043] Test Example 1

[0044] The exposed aggregate concrete prepared in Examples 1-5 and Comparative Examples 1-2 was tested. The specimens were 400 mm in length, 400 mm in width, and the height was the same as the laying thickness of each embodiment and comparative example. The construction environment temperature was 43°C and the curing time was 28 days. The compressive strength and permeability coefficient were tested and whether slurry settling and stratification occurred were observed.

[0045] The compressive strength test standard is GB / T50081-2002, and the permeability coefficient is measured using the concrete permeability coefficient tester (NELD-PC370).

[0046] name Compressive strength(Mpa) Permeability coefficient (mm / s) Is there any sedimentation and stratification? Example 1 23.1 8.4 no Example 2 24.5 8.6 no Example 3 24.9 9.1 no Example 4 22.4 7.5 yes Example 5 20.7 7.7 yes Comparative Example 1 19.2 7.1 yes Comparative Example 2 21.2 6.7 yes

[0047] The experimental results show that the exposed aggregate concrete prepared by the present invention has good compression resistance and permeability. Example 4-5 changes the mixing method of raw materials in step (1) and step (2), resulting in a decrease in the performance of the exposed aggregate concrete. In the present invention, in step (1), when the size of the crushed stone is small, the crushed stone and water are first mixed to fully infiltrate the aggregate, so that the cement can fully adhere to the surface of the crushed stone, fill the pores on the surface of the aggregate and improve the bonding effect between the aggregates. In step (2), when the size of the crushed stone is large, the water-cement ratio is controlled to be 0.42-0.44, and the cement ash is mixed first and then the crushed stone is added. This can avoid exposing the aggregate and the poor bonding effect. More importantly, it improves the bonding effect of the slurry interface prepared in step (1) and step (2) to prevent cement slurry deposition and stratification fracture.

[0048] In Comparative Example 1, the paving thickness and the crushed stone size selection are changed, resulting in a decrease in the performance of the exposed aggregate concrete. In the present invention, the reasonable mixing of the crushed stone size and the paving thickness can improve the compressive strength and the permeability coefficient. In step (2) of Comparative Example 1, only larger-sized crushed stones are used for paving, which can increase the porosity of the concrete pavement and further improve the water penetration effect. However, the pore structure is large, resulting in a significant decrease in compressive strength, and cement deposition occurs at the same time, resulting in cracks at the joints, a decrease in the load-bearing effect of the base material, and deformation of the concrete material. In Comparative Example 2, the component ratio of the binder is adjusted, resulting in a decrease in the performance of the exposed aggregate concrete. The binder of the present invention can absorb the free water between the aggregates, avoid dehydration, and have a better bonding effect between the aggregates, avoiding the phenomenon of aggregate shedding.

[0049] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A construction method for exposed aggregate concrete, characterized in that: The following steps are involved: (1) Mix crushed stones with sizes of 2 mm and 14 mm, a binder, and cement. The crushed stones with sizes of 2 mm are 6 parts, the crushed stones with sizes of 14 mm are 10 parts, the binder is 1 part, and the cement is 27 parts. The water-cement ratio is 0.

36. The mass ratio of hydroxypropyl methylcellulose, clay mineral powder, and steel fiber in the binder is 1:4:0.

5. The length of the steel fiber is 25 mm, and the aspect ratio is 1:

60. Stir the crushed stones and 35% of the total water for 2.5 minutes, then add cement and stir for 55 seconds, and finally add the binder and the remaining water and stir for 3.5 minutes to obtain a base material. The laying thickness of the base material is 240 mm. (2) After the base material has been laid for 2.5 hours, 2 mm and 25 mm crushed stone, binder and cement are mixed and laid on the surface of the base material. By weight, the crushed stone with a size of 2 mm is 1.5 parts, the crushed stone with a size of 25 mm is 11 parts, the binder is 3 parts, and the cement is 32 parts. The water-cement ratio is 0.

43. The mass ratio of hydroxypropyl methylcellulose, clay mineral powder and steel fiber in the binder is 1:8:0.

3. The length of the steel fiber is 20 mm, and the aspect ratio is 1:

60. The crushed stone with a size of 2 mm, cement and water are mixed and stirred for 3.5 minutes, and the crushed stone with a size of 25 mm and the binder are added and stirred for 9 minutes to obtain a slurry. The slurry is laid with a thickness of 300 mm.