A fast deep curing weather-resistant silicone sealant and its preparation method and application
By introducing phenyl and highly reactive reactive groups into the crosslinking agent, the crosslinking agent structure is designed, and the shortcomings of single-component room-temperature vulcanized silicone rubber in rapid deep curing and weather resistance are solved, and the conditions of high temperature and high humidity are achieved Excellent properties and long-term weathering resistance.
Patent Information
- Application Number
- CN202211727523.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-27
AI Technical Summary
The existing single-component room temperature vulcanized silicone rubber has shortcomings in rapid deep curing and weather resistance, and cannot be improved simultaneously, limiting its application efficiency and performance under high temperature and high humidity conditions.
Using a phenyl-containing alkoxysilane crosslinking agent and a coupling agent hydrolyzate of highly reactive reactive groups as crosslinking agents, combining highly reactive amino groups, acyloxy groups or epoxy groups, the crosslinking agent structure is designed to design the crosslinking agent structure in Fast deep curing is achieved under small amounts of water vapor and the weather resistance of sealants is improved.
It achieves rapid deep curing with a curing depth of more than 1.5mm within 4 hours and a curing depth of more than 6mm within 7 days. At the same time, it maintains excellent humidity and heat resistance with a cohesion failure degree of more than 90% for 1500 hours under 85℃ and 85% R.H. humidity conditions. .
Smart Images

Figure CN115975591B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of organic silicon, in particular to a fast deep-curing weather-resistant organic silicon sealant and a preparation method and application thereof. Background Art
[0002] Single-component room temperature vulcanized silicone rubber has excellent bonding and mechanical properties, low cost, and is easy to automatically dispense. It is widely used in construction, electronics, industry and other fields due to its outstanding high and low temperature resistance, electrical insulation and weather resistance.
[0003] However, since single-component room temperature vulcanized silicone rubber needs to be exposed to water vapor in the air and cure from the surface to the inside, its curing depth is greatly limited. Existing single-component room temperature vulcanized silicone rubber requires at least 24 hours to assemble the structure, which greatly reduces the efficiency of automation. With the rapid development of related industries, higher requirements are put forward for rapid assembly, including requiring single-component room temperature vulcanized silicone rubber to dry quickly and cure deeply. At the same time, with the increasing application of single-component room temperature vulcanized silicone rubber, the requirements for its weather-resistant bonding under high temperature and high humidity conditions are also getting higher and higher.
[0004] At present, most of the methods to improve the curing rate and bonding performance of sealants are to modify the cross-linking agent or add curing / bonding accelerators. For example, patent CN111704864A discloses that oligomers formed by hydrolysis and cross-linking of multiple coupling agents containing n-octyltriethoxysilane are added to silane-modified polyether sealants as bonding accelerators, which are more active and can promote the deep curing of the sealant, but it does not pay attention to the weather resistance of the sealant. For example, patent CN109486467A adds a coupling agent having both hydrophobic alkyl and highly reactive organic groups (such as amino and epoxy groups) to silicone sealants, which can improve the deep curing speed of the sealant, enhance the wettability of the sealant and the substrate, and enhance the bonding strength of the product, but it also does not mention the weather resistance of the sealant. As for the weather resistance of sealants, there are patents (such as patent CN102746486A) that improve the weather resistance of sealants by introducing long-chain fatty chains with excellent moisture-barrier capabilities into the main chain of the silicone matrix. However, since single-component room temperature vulcanized silicone rubber needs to come into contact with water vapor in the air to cross-link, and the long-chain fatty chains block moisture, they will in turn block the contact between silicone rubber and water vapor to a certain extent, resulting in limited improvement in the deep curing ability of the sealant.
[0005] Therefore, it is necessary to develop a silicone sealant that has both fast deep-layer curing ability and weather resistance. Summary of the invention
[0006] The purpose of the present invention is to overcome the defect that the deep curing ability and weather resistance of the existing silicone sealant cannot be improved at the same time, and to provide a silicone sealant with both fast deep curing ability and weather resistance. The present invention uses a hydrolyzate of a phenyl-containing alkoxysilane crosslinking agent and a coupling agent containing a highly active reactive group as a crosslinking agent, which can react quickly under the condition of a small amount of water vapor to achieve the purpose of fast curing and deep curing. At the same time, the highly active amino, acyloxy or epoxy group is evenly distributed in the sealant system, so that the sealant has long-term weather resistance and weather-resistant bonding performance.
[0007] Another object of the present invention is to provide a method for preparing the fast deep-curing weather-resistant silicone sealant.
[0008] Another object of the present invention is to provide the application of the fast deep-curing weather-resistant silicone sealant in the fields of construction, electronics, industry or corrosion protection.
[0009] To achieve the above object, the present invention adopts the following technical solution:
[0010] A fast deep-curing weather-resistant silicone sealant comprises the following components in parts by weight:
[0011]
[0012] Wherein, the cross-linking agent has a structural formula as shown in Formula I:
[0013]
[0014] In Formula I, n=3 to 13; R 1 Selected from C 1~2 The alkyl group;
[0015] R 2 , R 3 , R 4 , R 5 Independently selected from phenyl (—C 6 H 5 ), methyl (—CH 3 ), vinyl (—CH=CH 2 ), aminopropyl (—(CH2)3NH2), C 1~2 Alkoxy (—OCH 3 , —OCH 2 CH 3 ), at least one of an epoxy-containing alkoxy group and an acrylate-containing alkyl group, and R 2 , R 3 , R 4 , R 5 Contains at least one phenyl group;
[0016] R 6 Selected from methyl, vinyl, aminopropyl, C 1~2 At least one of an alkoxy group, an alkoxy group containing an epoxy group, and an alkyl group containing an acrylate group.
[0017] The present invention uses the hydrolysis product of phenyl-containing alkoxysilane and a coupling agent containing a highly active reactive group as a crosslinking agent, which can react quickly in the presence of a small amount of water vapor to achieve the purpose of rapid curing and deep solidification. At the same time, the highly active amino, acyloxy or epoxy group is evenly distributed in the sealant system, so that the sealant has long-term weather resistance and weather-resistant bonding properties.
[0018] Due to its large volume and conjugation effect, phenyl can significantly improve the weather resistance of sealants, especially its moisture and heat resistance. However, due to the steric effect of phenyl, the activity of the cross-linkable active groups near it will be reduced. Therefore, by designing the cross-linker structure and controlling the degree of polymerization, the phenyl content in the cross-linker can be effectively controlled, thereby achieving a good balance between curing performance and weather resistance.
[0019] At the same time, the inventors of the present invention have also found through extensive research that when a phenyl group is connected to the end of a crosslinking agent, on the one hand, due to the steric hindrance of the phenyl group, the activity of the crosslinkable active groups near it is reduced, which can prevent the sealant surface from forming a dense crosslinking degree too quickly, which is conducive to the penetration of water vapor from the surface to the inside, thereby improving the deep curing ability of the sealant; on the other hand, the crosslinking agent after hydrolysis polymerization contains a certain degree of polymerization, and the reaction between macromolecules will reduce the dependence on moisture content, and the structure contains a large number of amino, acyloxy or epoxy hydrophilic groups, which is also conducive to the penetration of moisture from the surface to the inside. In addition, the highly active amino, acyloxy or epoxy groups are concentrated in the middle part of the crosslinking agent molecular chain, most of the active groups are less affected by the phenyl group, and the distribution uniformity of the active groups in the sealant system will not cause local poor bonding, further improving the bonding performance and weather-resistant bonding of the sealant.
[0020] Preferably, the epoxy-containing alkoxy group includes
[0021] Preferably, the alkyl group containing an acrylate group comprises —(CH2)3OOC(CH 3 )C=CH 2 .
[0022] Preferably, in the formula I, n=6 to 10. In the crosslinking agent, as the degree of polymerization n increases, the proportion of hydrophilic groups of the crosslinking agent increases, which is conducive to deep curing, but the proportion of phenyl groups decreases, resulting in poor weather resistance of the system. When the degree of polymerization n decreases, the proportion of hydrophilic groups of the crosslinking agent is small, and the content of phenyl groups is too high, which reduces the permeability of moisture, thereby reducing deep curing. Therefore, when the n value is within the above range, the obtained sealant has excellent rapid deep curing performance and weather resistance.
[0023] Conventional polydimethylsiloxanes can be used in the present invention, including but not limited to at least one of α,ω-dihydroxy polydimethylsiloxane, methyldimethoxy-terminated polydimethylsiloxane, trimethoxy-terminated polydimethylsiloxane and vinyldimethoxy-terminated polydimethylsiloxane.
[0024] Preferably, the dynamic viscosity of the polydimethylsiloxane at 25° C. is 1000 to 80000 mPa.s. As the viscosity increases, the deep curing performance and weather resistance of the obtained sealant are improved. However, when the viscosity of the polydimethylsiloxane is too high, the construction performance of the sealant deteriorates. Therefore, when the viscosity of the polydimethylsiloxane is within the above-mentioned appropriate range, the weather resistance and bonding properties of the obtained sealant are both good.
[0025] The filler is a reinforcing filler, and its function is to improve the mechanical strength of the sealant. Conventional reinforcing fillers for silicone sealants can be used in the present invention. The filler includes but is not limited to at least one of calcium carbonate, talc, zinc borate, titanium dioxide, silicon powder, quartz powder, aluminum hydroxide, aluminum oxide, white carbon black, carbon black, magnesium oxide, zinc oxide, barium carbonate, diatomaceous earth and kaolin.
[0026] Conventional catalysts can also be used in the present invention, and the catalysts include organic tin catalysts and / or titanate organic catalysts. The organic tin catalysts include but are not limited to at least one of dioctyltin diacetate, dioctyltin dilaurate, dioctyltin dioctoate, dibutyltin diacetate, dibutyltin dilaurate, and dibutyltin dioctoate; the titanate organic catalysts include but are not limited to at least one of isopropyl titanate, n-butyl titanate, ethyl acetoacetate chelate of isopropyl titanate, and acetylacetone chelate of isopropyl titanate.
[0027] The present invention also protects a method for preparing the above-mentioned fast deep-curing weather-resistant silicone sealant, which comprises the following steps:
[0028] S1. Preparation of cross-linking agent
[0029] According to the structure shown in formula I, the reaction monomers of the organosilicon crosslinking agent and the coupling agent are prepared into a mixed solution, and a hydrolysis reaction is carried out in an inert atmosphere at -10 to 50° C., and finally a phenyl-containing siloxane is added, and after the reaction is complete, the by-products are removed to obtain the crosslinking agent;
[0030] S2. Preparation of silicone sealant
[0031] The fast deep-curing weather-resistant organic silicone sealant can be obtained by uniformly mixing polydimethylsiloxane, filler, cross-linking agent and catalyst under vacuum conditions.
[0032] In the reaction monomers described in step S1, the organosilicon crosslinking agent is selected from at least one of vinyl trimethoxysilane, vinyl triethoxysilane, methyl trimethoxysilane, methyl triethoxysilane, and tetramethoxysilane; the coupling agent is selected from at least one of γ-aminopropyl triethoxysilane, γ-aminopropyl trimethoxysilane, 3-aminopropyl methyl dimethoxysilane, 3-aminopropyl methyl diethoxysilane, 3-(methacryloyloxy) propyl trimethoxysilane, and γ-[(2,3)-epoxypropyl] propyl trimethoxysilane. The type and amount of the reaction monomers are selected according to the structure shown in Formula I.
[0033] The phenyl-containing siloxane includes, but is not limited to, at least one of phenyltrimethoxysilane and diphenyldimethoxysilane.
[0034] The inert atmosphere in step S1 is an atmosphere formed by mixing at least one of nitrogen, helium or argon.
[0035] In step S2, in order to further improve the dispersion uniformity of each component in the sealant, the polydimethylsiloxane and the filler can be stirred and mixed evenly, and then dehydrated under vacuum conditions of 80 to 150°C and -0.097 to -0.092Mpa. After cooling to ≤40°C, a cross-linking agent and a catalyst are added, and the mixture is continued to be stirred and mixed in a closed manner under vacuum conditions of 80 to 150°C and -0.097 to -0.092Mpa for 20 to 40 minutes until it is evenly mixed.
[0036] The application of the above-mentioned fast deep-curing weather-resistant silicone sealant in the fields of construction, electronics, industry or corrosion protection is also within the protection scope of the present invention.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] The invention improves the weather resistance, especially the moisture and heat resistance, of the sealant by introducing phenyl into the crosslinking agent; at the same time, the molecular structure of the crosslinking agent is designed to reduce the influence of the phenyl on the reduction of the activity of the crosslinkable active group. By designing the crosslinking agent structure and controlling the degree of polymerization, the content of the phenyl in the crosslinking agent can be effectively controlled, thereby achieving a good balance between the curing performance and the weather resistance, so that the obtained organosilicon sealant has both rapid deep curing performance and excellent weather resistance and weather resistance bonding performance.
[0039] The curing depth of the organic silicon sealant of the present invention after 4 hours is more than 1.5 mm, and the curing depth after 7 days is more than 6 mm, which can be as high as 10 mm. It also has excellent moisture and heat resistance. After being placed under 85° C. and 85% RH humidity conditions for 1500 hours, the degree of cohesive failure is still more than 90%. DETAILED DESCRIPTION
[0040] To better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. Unless otherwise specified, the reagents and materials used in the present invention are commercially available.
[0041] The following raw materials are used in the examples and comparative examples of the present invention:
[0042] Dimethicone:
[0043] 1#: α,ω-dihydroxy polydimethylsiloxane, dynamic viscosity at 25°C is 20000mPa.s;
[0044] 2#: α,ω-dihydroxy polydimethylsiloxane, dynamic viscosity at 25°C is 80000mPa.s;
[0045] 3#: α,ω-dihydroxypolydimethylsiloxane, dynamic viscosity at 25°C is 1000mPa.s;
[0046] 4#: trimethoxy-terminated polydimethylsiloxane, dynamic viscosity at 25°C is 20000mPa.s;
[0047] 5#: Vinyl dimethoxy-terminated polydimethylsiloxane, dynamic viscosity at 25°C is 20000mPa.s;
[0048] Crosslinking agent:
[0049] Cross-linking agent I, the structural formula is as follows:
[0050]
[0051] Prepared according to a method comprising the following steps:
[0052] After 2 mol of methyltrimethoxysilane and 1 mol of γ-aminopropyltrimethoxysilane are mixed evenly, 1 mol of water is added to fully dissolve to obtain a mixed reaction solution containing monomers, and the mixture is reacted at 10° C. for 30 min under a nitrogen protection environment. Then 1 mol of phenyltrimethoxysilane is added and the mixture is reacted for 30 min. The temperature is then raised to 100° C. and the mixture is evacuated to -0.095 MPa and maintained for 30 min. The by-products are removed to obtain the crosslinking agent I.
[0053] Crosslinker II:
[0054] It was prepared according to the method of crosslinker I, except that the reaction raw material methyltrimethoxysilane in crosslinker I was replaced by vinyltrimethoxysilane in equal moles, and γ-aminopropyltrimethoxysilane was replaced by 3-(methacryloyloxy)propyltrimethoxysilane in equal moles. The structural formula is shown below:
[0055]
[0056] Crosslinker III:
[0057] It was prepared according to the method of crosslinker I, except that the methyltrimethoxysilane in the crosslinker I was replaced by tetramethoxysilane in equal moles, the γ-aminopropyltrimethoxysilane was replaced by γ-[(2,3)-epoxypropyl]propyltrimethoxysilane in equal moles, and the phenyltrimethoxysilane was replaced by diphenyldimethoxysilane. The structural formula is shown below:
[0058]
[0059] Cross-linking agent IV:
[0060] It was prepared according to the method of crosslinker I, except that the reaction raw material γ-aminopropyltrimethoxysilane in crosslinker I was replaced by an equimolar mixture of γ-aminopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane and γ-[(2,3)-epoxypropyl]propyltrimethoxysilane (molar ratio 1:1:1), and the structural formula is shown below:
[0061]
[0062] Crosslinker V:
[0063] It was prepared according to the method of crosslinker I, except that the molar ratio of the reaction raw materials in crosslinker I was replaced by methyltrimethoxysilane:γ-aminopropyltrimethoxysilane:water:phenyltrimethoxysilane=1:1:2:2, and the degree of polymerization n=6.
[0064] Crosslinker VI:
[0065] It was prepared according to the method of crosslinker I, except that the reaction was carried out at -10°C for 80 minutes under a nitrogen protection environment, and then 1 mol of phenyltrimethoxysilane was added and reacted for 30 minutes. The degree of polymerization of the obtained crosslinker IV was n=10.
[0066] Crosslinker VII:
[0067] It was prepared according to the method of crosslinker I, except that the reaction was carried out at 50° C. for 10 minutes under a nitrogen protection environment, and then 1 mol of phenyltrimethoxysilane was added and reacted for 30 minutes. The degree of polymerization of the obtained crosslinker V was n=13.
[0068] Crosslinker VIII:
[0069] It was prepared according to the method of crosslinker I, except that the reaction was carried out at 50° C. for 20 minutes under a nitrogen protection environment, and then 1 mol of phenyltrimethoxysilane was added and reacted for 30 minutes. The degree of polymerization of the obtained crosslinker VI was n=18.
[0070] Crosslinker IX:
[0071] It was prepared according to the method of crosslinker I, except that the reaction was carried out at -10°C for 15 minutes under a nitrogen protection environment, and then 1 mol of phenyltrimethoxysilane was added and reacted for 30 minutes. The degree of polymerization of the obtained crosslinker VII was n=2.
[0072] Crosslinker X:
[0073] Prepared according to a method comprising the following steps:
[0074] After 2 mol of methyltrimethoxysilane, 1 mol of γ-aminopropyltrimethoxysilane and 1 mol of phenyltrimethoxysilane are mixed evenly, 1 mol of water is added to fully dissolve to obtain a mixed reaction solution containing monomers. Under a nitrogen protection environment, the mixture is reacted at 100° C. for 30 minutes, and then the vacuum is evacuated to -0.095 MPa and maintained for 30 minutes to remove the by-products. The obtained cross-linking agent has a random block copolymer structure.
[0075] Examples 1 to 15, Comparative Examples 1 to 4
[0076] A series of silicone sealants are provided, which are prepared according to a method comprising the following steps:
[0077] According to the raw material formula in Tables 1 and 2, polydimethylsiloxane and filler are stirred evenly, and then moisture is removed under vacuum conditions of 100°C and -0.095Mpa, and then the temperature is lowered to below 40°C, and a cross-linking agent and a catalyst are added. After being stirred evenly in a closed state at -0.095Mpa (about 30 minutes), the silicone sealant can be obtained by discharging the material.
[0078] Table 1 Formula of organic silicon sealant of embodiment 1~9 (weight parts)
[0079]
[0080] Table 2 Formulas of silicone sealants of Examples 10 to 13 and Comparative Examples 1 to 4 (parts by weight)
[0081]
[0082] Performance Testing
[0083] The performance of the organic silicon sealant obtained in the above examples and comparative examples was characterized, and the specific test items, test methods and results are as follows:
[0084] 1. Surface drying time: obtained according to the test of GB / T 13477 1992. The test results are shown in Table 3.
[0085] 2. Curing depth: Use a polytetrafluoroethylene test plate with a wedge-shaped groove of 5 cm in length, 5 cm in width and 20 mm in depth, and evenly pour the prepared silicone sealant into the wedge-shaped groove of the polytetrafluoroethylene test plate. Then place the test plate at a temperature of (23±2)°C and a relative humidity of 55% to cure to form a test sample. After 4h and 7d, peel off the test sample from the test plate and compare the curing depth. The test results are shown in Table 3.
[0086] 3.Performance after curing:
[0087] 3.1 Tensile strength and hardness: Use a polytetrafluoroethylene container with a wedge-shaped groove with a depth of 2mm, a length of 25cm and a width of 20cm to evenly pour the prepared silicone sealant into the polytetrafluoroethylene container, then place the prepared sample at a temperature of (23±2)℃ and a relative humidity of 55% for curing for 7 days, take it out, and prepare the test sample. Then test the tensile strength of the sample according to GB / T 528-2009, and test the hardness of the sample according to GB / T531.1-2008. The test results are shown in Table 3;
[0088] 3.2 Weathering resistance bonding test: The prepared silicone sealant was evenly applied on the surface of 3003 series aluminum material with a bonding area of 25mm x 12.5mm and a thickness of 1mm. The prepared sample was then placed at a temperature of (23±2)°C and a relative humidity of 55% for curing for 7 days. It was then taken out and aged at a temperature of 85°C and a relative humidity of 85% for 0h and 1500h. It was then cooled to room temperature to compare the bonding conditions (expressed by the degree of interface damage. The higher the proportion of interface damage, the better the bonding performance). The test results are shown in Table 3.
[0089] Table 3 Performance test results of the silicone sealants obtained in the examples and comparative examples
[0090]
[0091] From the above results we can see that:
[0092] The curing depth of the prepared materials is above 1.5 mm after 4 hours, above 6 mm after 7 days, and up to 9.93 mm. The materials also have excellent heat and humidity resistance. After being placed under the conditions of 85°C and 85% RH for 1500 hours, the degree of cohesive failure is still above 80%. The materials also have good tensile strength and hardness, and can meet the use requirements.
[0093] The results of Examples 1 to 3 show that under the above dosage range and raw material selection of the present invention, the obtained sealant has excellent comprehensive performance.
[0094] The results of Example 1 and Examples 4 to 7 show that conventional polydimethylsiloxane can be used in the present invention, and as the viscosity increases, the weather resistance of the obtained sealant is improved. However, when the viscosity of the polydimethylsiloxane is too high, the construction performance of the sealant deteriorates. Therefore, when the viscosity of the polydimethylsiloxane is within the above-mentioned appropriate range, the weather resistance and bonding properties of the obtained sealant are better.
[0095] The results of Examples 1 and 8 to 9 show that conventional inorganic fillers and catalysts can be used in the present invention and have little effect on the performance of the sealant.
[0096] The results of Examples 1 and 10 to 12 show that conventional crosslinking agents and coupling agents, with adjustable ratios, are suitable for use in the present invention.
[0097] The results of Example 1, Examples 13 to 15, and Comparative Examples 1 to 2 show that as the degree of polymerization n in the crosslinker increases, the proportion of hydrophilic groups in the crosslinker increases, which is conducive to deep curing, but the proportion of phenyl groups decreases, resulting in poor weather resistance of the system. When the degree of polymerization n decreases, the proportion of hydrophilic groups in the crosslinker is small, and the content of phenyl groups is too high, which reduces the permeability of moisture, thereby reducing deep curing (i.e., curing depth). Therefore, when the n value is within the above range, the obtained sealant has excellent rapid deep curing performance.
[0098] The cross-linking agent in Comparative Example 3 is a random block copolymer, and the activity of the cross-linkable active groups is affected by the phenyl group, so the 4h curing depth and the performance and bonding performance after 7d of curing are significantly reduced; the cross-linking agent in Comparative Example 4 is a simple physical blend without pre-hydrolysis, and the curing performance is significantly reduced.
[0099] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A fast and deep curing weather-resistant silicone sealant. It is characterized in that The composition comprises the following components in parts by weight: 100 parts of polydimethylsiloxane; Filler 80~150 parts; 3-15 parts of cross-linking agent; Catalyst 0.1~8 parts; Wherein, the preparation method of the cross-linking agent comprises the following steps: 2 mol of methyltrimethoxysilane and 1 mol of γ-aminopropyltrimethoxysilane were mixed evenly, and 1 mol of water was added to dissolve to obtain a mixed reaction solution, and a hydrolysis reaction was carried out under a nitrogen protection environment. Finally, 1 mol of phenyltrimethoxysilane was added, and the reaction was carried out for 30 minutes, and then the temperature was raised to 100° C., and the vacuum was evacuated to -0.095 MPa, and maintained for 30 minutes. The by-products were removed to obtain the cross-linking agent; The conditions of the hydrolysis reaction are: reaction at 10°C for 30 minutes; or reaction at -10°C for 80 minutes; or reaction at 50°C for 10 minutes.
2. The fast deep curing weather-resistant silicone sealant according to claim 1, It is characterized in that The filler includes at least one of calcium carbonate, talc, zinc borate, titanium dioxide, silicon powder, quartz powder, aluminum hydroxide, aluminum oxide, white carbon black, carbon black, magnesium oxide, zinc oxide, barium carbonate, diatomaceous earth and kaolin.
3. The fast deep curing weather-resistant silicone sealant according to claim 1, It is characterized in that The catalyst includes at least one of dioctyltin diacetate, dioctyltin dilaurate, dioctyltin dioctoate, dibutyltin diacetate, dibutyltin dilaurate, dibutyltin dioctoate, isopropyl titanate, n-butyl titanate, ethyl acetoacetate chelate of isopropyl titanate and acetylacetone chelate of isopropyl titanate.
4. The method for preparing the fast deep curing weather-resistant silicone sealant according to any one of claims 1 to 3, It is characterized in that The steps include: The fast deep-curing weather-resistant organic silicone sealant can be obtained by uniformly mixing polydimethylsiloxane, filler, cross-linking agent and catalyst under vacuum conditions.
5. Application of the fast deep curing weather-resistant silicone sealant according to any one of claims 1 to 3, It is characterized in that The fast deep-curing weather-resistant silicone sealant is used in the fields of construction, electronics or corrosion protection.
Citation Information
Cited By
Modified cross-linking agent, dealcoholized silicone sealant with high curing speed and good heat resistance and preparation method of dealcoholized silicone sealant
CN119978023A
A modified crosslinking agent and a fast-curing, heat-resistant, alcohol-free silicone sealant, and their preparation method.
CN119978023B