Cubic deflected structure polymerized nitrogen and its preparation method and application
By filling the sample cavity of a diamond anvil cell with glassy carbon and liquid nitrogen, and using high temperature and high pressure treatment to form cubic deflection structure polymeric nitrogen encapsulated in diamond, the problem of difficulty in preservation at room temperature and pressure is solved, and high yield and long-term stable preservation are achieved.
Patent Information
- Application Number
- CN202211709768.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-29
AI Technical Summary
The cubic deflection structure polymeric nitrogen obtained by traditional preparation methods is difficult to store stably at room temperature and pressure, and the operation is complicated, with low yield and short storage time.
A diamond anvil cell sample chamber is filled with glassy carbon and liquid nitrogen. The sample is then processed under high temperature and pressure to form a cubic deflection structure polymer nitrogen, which is then encapsulated in diamond. The three-dimensional porous structure of glassy carbon is used to transform liquid nitrogen into diamond under high temperature and pressure, achieving stable preservation at room temperature and pressure.
Stable storage of cubic deflection structure polymeric nitrogen at room temperature and pressure was achieved, with long storage time. The preparation method is simple, has high yield, and is easy to operate.
Smart Images

Figure CN116002634B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of energetic materials, in particular to cubic deflected structure polymerized nitrogen and a preparation method and application thereof. Background Art
[0002] All-nitrogen compounds are promising candidates for high energy density materials (HEDM) such as propellants and explosives. Among all-nitrogen compounds, polymeric nitrogen, especially cubic deflected polymeric nitrogen (cg-N), has the highest energy. Theoretical calculations show that the density of cg-N is 3.9 g·cm -3 , with a specific impulse of 500s, and an explosion pressure more than ten times that of HMX (Octogen). Currently, cg-N is mainly prepared by pressurizing a diamond anvil cell (DAC) to 140GPa and compressing nitrogen at a high temperature of 2000K. However, the cg-N prepared by this preparation method cannot be stably stored at room temperature and pressure.
[0003] Although there are methods on the market for preparing polymerized nitrogen using carbon nanotubes or graphene materials, which can achieve stable storage of polymerized nitrogen at room temperature and pressure, the preparation method is complicated to operate, and the prepared polymerized nitrogen sample is nanoscale, with low yield, and the stable storage time at room temperature and pressure is very short, that is, the life span is basically on the order of 1 microsecond.
[0004] It can be seen from this that the polymerized nitrogen obtained by traditional preparation methods, especially cubic deflected structure polymerized nitrogen (cg-N), is still difficult to store stably at room temperature and pressure. Summary of the invention
[0005] Based on this, it is necessary to provide a cubic deflected structure polymerized nitrogen and its preparation method and application to address the above problems. The cubic deflected structure polymerized nitrogen obtained by the preparation method can be stably stored at room temperature and pressure and has a long storage time.
[0006] A method for preparing cubic deflected structure polymerized nitrogen comprises the following steps:
[0007] Provide a diamond anvil cell sample chamber;
[0008] The diamond anvil cell sample chamber is filled with glassy carbon, cooled to below -148°C, continuously filled with liquid nitrogen, then pressurized to above 100 GPa, heated to above 2100 K, and finally depressurized to normal pressure and cooled to room temperature to obtain cubic deflected structure polymerized nitrogen encapsulated in diamond.
[0009] In one embodiment, in the step of pressurizing, the pressure is increased to 100 GPa-120 GPa.
[0010] In one embodiment, in the cooling step, the temperature is cooled to -148°C to -196°C.
[0011] In one embodiment, the filling rate of the glassy carbon is selected from 60%-80%, and the filling rate of the liquid nitrogen is selected from 20%-40%.
[0012] In one embodiment, in the step of heating, the temperature is heated to 2100K-2500K.
[0013] In one embodiment, the method for preparing the diamond anvil cell sample chamber comprises the following steps:
[0014] Prepare the diamond anvil;
[0015] Pre-pressing the gasket using the diamond anvil to form an indentation;
[0016] A hole is punched at the center of the indentation, and the hole serves as a diamond anvil sample chamber.
[0017] In one embodiment, the diameter of the anvil surface of the diamond anvil is selected from 70 μm to 90 μm;
[0018] And / or, the diameter of the hole is selected from 30 μm-50 μm.
[0019] In one embodiment, the thickness of the gasket is selected from 240 μm to 260 μm, and the thickness of the gasket after pre-compression is selected from 10 μm to 30 μm;
[0020] And / or, the material of the gasket is selected from rhenium or tungsten.
[0021] A cubic deflected structure polymerized nitrogen prepared by the method for preparing cubic deflected structure polymerized nitrogen as described above.
[0022] An application of the cubic deflection structure polymerized nitrogen as described above in energetic materials.
[0023] In the present invention, glassy carbon is first filled into the diamond anvil sample chamber, and then liquid nitrogen is filled. Since the glassy carbon has pores, the filled liquid nitrogen will enter the pores of the glassy carbon and mix into the glassy carbon. Therefore, in a high-temperature and high-pressure environment formed by pressurization and heating treatment, the liquid nitrogen and the glassy carbon will simultaneously synthesize cubic deflected structure polymerized nitrogen and diamond under high temperature and high pressure, and when the glassy carbon is converted into diamond, the high-pressure cubic deflected structure polymerized nitrogen will be sealed inside, thereby obtaining the cubic deflected structure polymerized nitrogen encapsulated in the diamond. Therefore, when the pressure is released to normal pressure and the temperature is lowered to normal temperature, the cubic deflected structure polymerized nitrogen encapsulated in the diamond prepared by the present invention can be stably stored and has a long storage time. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1A schematic diagram of the preparation process of polymerized nitrogen encapsulated in a cubic deflected structure in diamond provided by the present invention;
[0025] Figure 2 This is the Raman spectrum of the polymerized nitrogen encapsulated in the diamond neutral cubic deflection structure prepared in Example 1 of the present invention at room temperature and pressure;
[0026] Figure 3 The 3D crystal structure diagram of the cubic deflected structure polymerized nitrogen prepared in Example 1 of the present invention;
[0027] Figure 4 This is the Raman spectrum of polymerized nitrogen prepared in Comparative Example 1 of the present invention;
[0028] Figure 5 This is the Raman spectrum of polymerized nitrogen prepared in Comparative Example 3 of the present invention;
[0029] Figure 6 This is the Raman spectrum of polymerized nitrogen prepared in Comparative Example 5 of the present invention;
[0030] Figure 7 This is the Raman spectrum of the cubic deflected structure polymerized nitrogen prepared in Example 1 of the present invention after being placed at room temperature and pressure for one week. DETAILED DESCRIPTION
[0031] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific implementation methods or embodiments, and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the combinations include any two related listed items, any more related listed items, or all related listed items.
[0033] See also Figure 1 , Figure 1 The schematic diagram of the preparation process of the cubic deflection structure polymerized nitrogen provided by the present invention, wherein A represents glassy carbon, B represents liquid nitrogen, C represents diamond, and D represents polymerized nitrogen. Figure 1As shown, liquid nitrogen and glassy carbon decompose and rebond under high temperature (above 2100K) and high pressure (above 100GPa) conditions to obtain cubic deflected structure polymerized nitrogen and diamond, and the cubic deflected structure polymerized nitrogen is encapsulated in diamond in a high-pressure form.
[0034] Specifically, the method for preparing cubic deflected structure polymerized nitrogen provided by the present invention comprises the following steps:
[0035] S1. Provide a diamond anvil cell sample chamber;
[0036] S2. Filling glassy carbon into the diamond anvil cell sample chamber, cooling it to below -148°C, continuously filling it with liquid nitrogen, then pressurizing it to above 100 GPa, and heating it to above 2100 K, and finally depressurizing it to normal pressure and cooling it to room temperature to obtain cubic deflected structure polymerized nitrogen encapsulated in diamond.
[0037] Glassy carbon is a non-graphitizable carbon that combines the properties of glass and ceramics. In contrast to crystalline graphite, it is an amorphous, nearly 100% sp 2 Hybrid carbon materials are formed by high-temperature sintering of polymerized organic precursors, such as phenolic resin, furfuryl alcohol resin, etc., in an inert gas atmosphere. Because it is black throughout and has a smooth surface similar to glass, it is called glassy carbon. Glassy carbon can be divided into two categories, type I and type II glassy carbon. Type I glassy carbon is formed by sintering polymerized organic matter at a temperature below 2000°C, and its interior is mainly composed of disordered curled graphene fragments; type II glassy carbon is sintered at a higher temperature (~2500°C), which is a disordered multilayer graphene three-dimensional matrix formed by stacking of nanoscale self-assembled fullerene-like spherical structures. It can be seen that compared with graphene materials, glassy carbon has a disordered structure and a three-dimensional pore structure.
[0038] In the present invention, glassy carbon is used as a three-dimensional porous structure, so that the liquid nitrogen filled in the sample cavity can enter the pores of the glassy carbon, that is, mixed in the glassy carbon, and the glassy carbon will be transformed into diamond under high temperature and high pressure. Therefore, the glassy carbon and liquid nitrogen filled in the sample cavity will be simultaneously transformed into corresponding diamond and cubic deflection structure polymerized nitrogen under the high temperature and high pressure environment formed by heating and pressurization, and the cubic deflection structure polymerized nitrogen is sealed in a small diamond cabin composed of diamond in a high pressure state. Therefore, when the pressure is released to normal pressure and the temperature is lowered to room temperature, the cubic deflection structure polymerized nitrogen encapsulated in the diamond can exist stably at room temperature and pressure, and the existence time is long.
[0039] In conventional preparation methods of polymerized nitrogen, such as the method of using carbon nanotubes and graphene materials to prepare polymerized nitrogen that can be stored at room temperature and pressure, the raw materials need to be dissolved, ultrasonicated, and then transferred to the carbon nanotubes or graphene materials, resulting in a complicated preparation method. In addition, the amount of nitrogen atoms transferred to the carbon nanotubes or graphene materials is relatively small, and the content is at the nanometer level, so that the yield of polymerized nitrogen is low, and the yield is basically about 1%; at the same time, the storage time is short.
[0040] The preparation method of cubic deflection structure polymerized nitrogen of the present invention does not need to consider the transfer of raw materials, and only needs to directly fill liquid nitrogen into the sample cavity containing glassy carbon, and the amount of liquid nitrogen and glassy carbon filled are both in the micrometer level, which is much larger than the nanometer level. Therefore, in the cubic deflection structure polymerized nitrogen encapsulated in diamond obtained under high temperature and high pressure, the yield of cubic deflection structure polymerized nitrogen is above 30%. Therefore, the preparation method of cubic deflection structure polymerized nitrogen of the present invention is simple, easy to operate, and has a high synthesis rate.
[0041] Considering the phase transition effect of glassy carbon and liquid nitrogen and the synthesis amount of cubic deflection structure polymerized nitrogen, in one embodiment, in step S1, the method for preparing the diamond anvil cell sample chamber comprises the following steps:
[0042] S11, preparing a diamond anvil;
[0043] S12, using the diamond anvil to pre-press the gasket to form an indentation;
[0044] S13, punching a hole at the center of the indentation, and the hole serves as a diamond anvil sample chamber.
[0045] Preferably, in step S11, the diameter of the anvil surface of the diamond anvil is selected from 70 μm-90 μm, and more preferably, the diameter of the anvil surface of the diamond anvil is selected from 80 μm. Such a setting can further ensure that the diamond anvil generates a high pressure of more than 100 GPa.
[0046] In one embodiment, in step S12, the thickness of the gasket is selected from 240 μm to 260 μm, and the thickness of the gasket after pre-compression is selected from 10 μm to 30 μm. This arrangement can ensure that the gasket has sufficient hardness after compression, which is convenient for subsequent use.
[0047] Preferably, the material of the gasket is selected from rhenium or tungsten. Further preferably, the gasket is selected from a rhenium sheet with a thickness of 250 μm and a size of 2.5 mm×2.5 mm.
[0048] In one embodiment, in step S13, an electric spark punch is used to punch a hole in the center of the indentation as a diamond anvil sample chamber, and the diameter of the hole is selected from 30 μm to 50 μm. This arrangement can further ensure that a sufficient high pressure is generated to facilitate the pressure for subsequent transformation of liquid nitrogen and glassy carbon, and at the same time, the synthesis amount of cubic deflection structure polymerized nitrogen can be increased.
[0049] It should be noted that after the diamond anvil sample cavity is formed, it can be reset into the diamond anvil.
[0050] In the present invention, the diamond anvil cell sample chamber is filled with glassy carbon and liquid nitrogen. Considering the synthesis rate and packaging effect of cubic deflection structure polymerized nitrogen, in one embodiment, the filling rate of the glassy carbon is selected from 60%-80%, and the filling rate of the liquid nitrogen is selected from 20%-40%.
[0051] It should be noted that in the preparation method of the present invention, liquid nitrogen is used as both a raw material and a pressure transmission medium, so that when pressurizing, there is no need to provide a pressure transmission medium.
[0052] Considering that liquid nitrogen will boil at room temperature, it is difficult to stably fill it into the diamond anvil cell sample cavity at room temperature, thereby affecting the synthesis rate of its cubic deflection structure polymerized nitrogen.
[0053] In one embodiment, in step S2, the temperature is lowered to -148°C to -196°C. This setting can better ensure that liquid nitrogen is stably filled in the diamond anvil sample chamber and better enters the pores of the glassy carbon, thereby increasing the synthesis rate of cubic deflection structure polymerized nitrogen.
[0054] Considering that both glassy carbon and liquid nitrogen need to be under high temperature and high pressure to undergo structural phase transition, and the control of temperature and pressure will affect the crystal structure obtained by the phase transition of glassy carbon and liquid nitrogen, in order to enable glassy carbon and liquid nitrogen to be better transformed into corresponding diamond and cubic deflected structure polymer nitrogen at the same time, in step S2, preferably, the pressure is increased to 100GPa-120GPa and heated to 2100K-2500K.
[0055] In one embodiment, in step S2, laser heating is performed to above 2100K by using a laser, and the laser wavelength is selected from 1060nm-1070nm. Preferably, the laser is a carbon dioxide laser. In this way, the present invention utilizes laser heating, which has high heating efficiency and can quickly reach a high temperature. The high temperature can cause liquid nitrogen to completely transform into cubic deflected structure polymerized nitrogen with a cubic network structure over a higher potential barrier, and make the cubic deflected structure polymerized nitrogen have better crystallinity.
[0056] The invention obtains a high-density cubic deflection structure polymerized nitrogen encapsulated in diamond which can stably exist at normal temperature and pressure by pressurizing and laser heating.
[0057] At the same time, the present invention also provides a cubic deflection structure polymerized nitrogen prepared by the method for preparing cubic deflection structure polymerized nitrogen as described above. The cubic deflection structure polymerized nitrogen is a high molecular polymer formed by nitrogen atoms being bonded by nitrogen-nitrogen single bonds, and the space group of the crystal structure of the cubic deflection structure polymerized nitrogen is I213, and its energy density is as high as 10.33 KJ / g.
[0058] In addition, the present invention also provides an application of the cubic deflection structure polymerized nitrogen as described above in energetic materials.
[0059] In one embodiment, the energetic material may be a propellant, an explosive, a propellant, a detonator, a pyrotechnic agent, or the like.
[0060] Hereinafter, the cubic deflection structure polymerized nitrogen and its preparation method and application will be further described through the following specific embodiments.
[0061] It should be noted that in the specific embodiments of the present invention, the HORIBA HR EVOLUTION Raman spectrometer is used to detect the obtained cubic deflection structure polymerized nitrogen and polymerized nitrogen encapsulated in diamond, and the corresponding Raman spectra are obtained, wherein the spectrum scanning range is: 100cm -1 -1200cm -1 or 100cm -1 -1400cm -1 , laser wavelength: 532nm, resolution: 1cm -1 .
[0062] Example 1
[0063] A diamond anvil with an anvil surface of 80 μm is used to pre-press a rhenium sheet with a thickness of 250 μm and a size of 2.5 mm×2.5 mm to form an indentation. The thickness of the rhenium sheet after pre-pressing is 20 μm. Then, an electric spark puncher is used to form a hole with a diameter of 40 μm at the center of the indentation. The hole serves as a sample cavity of the diamond anvil. Glassy carbon is filled into the sample cavity, cooled to -150°C, and liquid nitrogen is continuously filled to fill the entire sample cavity. The Raman peak of diamond is used as a pressure calibration to calibrate the pressure in the sample cavity. The filling rate of the glassy carbon is 60%, and the filling rate of the liquid nitrogen is 40%. Then, the diamond anvil is sealed, pressure-loaded, pressurized to 110 GPa, and laser-heated to 2100 K. Finally, the pressure is released to normal pressure and cooled to room temperature to obtain cubic deflected structure polymerized nitrogen encapsulated in diamond. The yield of cubic deflection structure polymerized nitrogen encapsulated in diamond obtained in this example is 36%.
[0064] Raman analysis was performed on the cubic deflection structure polymerized nitrogen encapsulated in diamond in this embodiment. Figure 2 This is the Raman spectrum of cubic deflection structure polymerized nitrogen encapsulated in diamond under normal temperature and pressure conditions. Figure 3 3D crystal structure diagram of cubic deflected structure polymerized nitrogen prepared in Example 1. Figure 2 In the Raman spectrum shown in -1 The characteristic peak of cubic deflected structure polymerized nitrogen appeared, which is consistent with the theoretical calculation Raman peak position of cubic deflected structure polymerized nitrogen structure in theoretical prediction.
[0065] At the same time, the cubic deflection structure polymerized nitrogen prepared in this embodiment was analyzed. Figure 3 This is the 3D crystal structure diagram of the square-deflected structured polymerized nitrogen prepared in Example 1, and the lattice constant is 0.345 nm.
[0066] It can be seen that the present embodiment successfully obtains cubic deflected structure polymerized nitrogen encapsulated in diamond under high pressure and high temperature.
[0067] Example 2
[0068] A diamond anvil with an anvil surface of 80 μm is used to pre-press a rhenium sheet with a thickness of 250 μm and a size of 2.5 mm×2.5 mm to form an indentation. The thickness of the rhenium sheet after pre-pressing is 25 μm. Then, an electric spark puncher is used to form a hole with a diameter of 30 μm at the center of the indentation. The hole serves as a sample cavity of the diamond anvil. Glassy carbon is filled into the sample cavity, cooled to -180°C, and liquid nitrogen is continuously filled to fill the entire sample cavity. The Raman peak of diamond is used as a pressure calibration to calibrate the pressure in the sample cavity. The filling rate of the glassy carbon is 70%, and the filling rate of the liquid nitrogen is 30%. Then, the diamond anvil is sealed, pressure-loaded, pressurized to 120 GPa, and laser-heated to 2200 K. Finally, the pressure is released to normal pressure and cooled to room temperature to obtain cubic deflected structure polymerized nitrogen encapsulated in diamond. The yield of polymerized nitrogen from this cubic deflection structure encapsulated in diamond is 42%.
[0069] Example 3
[0070] A diamond anvil with an anvil surface of 80 μm is used to pre-press a tungsten sheet with a thickness of 250 μm and a size of 2.5 mm×2.5 mm to form an indentation. The thickness of the tungsten sheet after pre-pressing is 25 μm. Then, an electric spark puncher is used to form a hole with a diameter of 40 μm at the center of the indentation. The hole is used as a sample cavity of the diamond anvil. Glassy carbon is filled into the sample cavity, cooled to -170°C, and liquid nitrogen is continuously filled to fill the entire sample cavity. The Raman peak of diamond is used as a pressure calibration to calibrate the pressure in the sample cavity. The filling rate of the glassy carbon is 80%, and the filling rate of the liquid nitrogen is 20%. Then, the diamond anvil is sealed, pressure is loaded, pressurized to 100 GPa, and laser heated to 2300 K. Finally, the pressure is released to normal pressure and cooled to normal temperature to obtain cubic deflection structure polymerized nitrogen encapsulated in diamond. The yield of the cubic deflection structure polymerized nitrogen encapsulated in diamond is 48%.
[0071] Example 4
[0072] Compared with Example 1, the only difference is that in Example 4, the filling rate of the glassy carbon is 50%, and the filling rate of the liquid nitrogen is 50%. The yield of the cubic deflection structure polymerized nitrogen encapsulated in diamond obtained in this example is 30%.
[0073] Example 5
[0074] Compared with Example 1, the only difference is that in Example 5, a diamond anvil with an anvil surface of 70 μm is used to pre-press a rhenium sheet with a thickness of 240 μm and a size of 2.5 mm×2.5 mm to form an indentation. The thickness of the rhenium sheet after pre-pressing is 20 μm, and then an electric spark punch is used to form a hole with a diameter of 25 μm at the center of the indentation. The hole serves as the sample cavity of the diamond anvil. The yield of cubic deflection structure polymerized nitrogen encapsulated in diamond obtained in this example is 36%.
[0075] Comparative Example 1
[0076] Compared with Example 1, the only difference is that in Example 1, glassy carbon is filled into the sample cavity, the temperature is lowered to -130°C, and liquid nitrogen is continuously filled to fill the entire sample cavity.
[0077] The Raman spectrum of the polymerized nitrogen prepared in this comparative example is as follows Figure 4 As shown, the crystal structure of the polymerized nitrogen is not a cubic deflected structure of polymerized nitrogen.
[0078] Comparative Example 2
[0079] Compared with Example 1, the only difference is that in Comparative Example 2, glassy carbon is filled into the sample cavity, the temperature is lowered to 0° C., and liquid nitrogen is continuously filled to fill the entire sample cavity.
[0080] Comparative Example 3
[0081] Compared with Example 1, the only difference is that in Comparative Example 3, the pressure is increased to 90 GPa.
[0082] The Raman spectrum of the polymerized nitrogen prepared in this comparative example is as follows Figure 5 As shown, the crystal structure of the polymerized nitrogen is not a cubic deflected structure of polymerized nitrogen.
[0083] Comparative Example 4
[0084] Compared with Example 2, the only difference is that in Comparative Example 4, the pressure is increased to 95 GPa.
[0085] Comparative Example 5
[0086] Compared with Example 1, the only difference is that in Comparative Example 5, the heating temperature is 2000K.
[0087] The Raman spectrum of the polymerized nitrogen prepared in this comparative example is as follows Figure 6 As shown, the crystal structure of the polymerized nitrogen is not a cubic deflected structure of polymerized nitrogen.
[0088] In order to better illustrate that the cubic deflected polymerized nitrogen prepared by the preparation method of the present invention can be stably stored at room temperature and pressure for a long time, the applicant placed the cubic deflected polymerized nitrogen prepared in Example 1 at room temperature and pressure for one week and then performed Raman analysis on it. The results are shown in Figure 7 .Depend on Figure 7 It can be clearly concluded that the cubic deflected polymerized nitrogen prepared by the preparation method of the present invention can not only be stably stored at room temperature and pressure, but also have a long storage time.
[0089] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0090] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing cubic deflected structure polymerized nitrogen, characterized in that: The following steps are involved: Provide a diamond anvil cell sample chamber; Fill the diamond anvil sample chamber with glassy carbon, then cool it to -148°C to -196°C, continue to fill it with liquid nitrogen, then pressurize it to above 100GPa, heat it to above 2100K, and finally release the pressure to normal pressure and cool it to room temperature to obtain cubic deflected structure polymerized nitrogen encapsulated in diamond, wherein the filling rate of the glassy carbon is selected from 60%-80%, and the filling rate of the liquid nitrogen is selected from 20%-40%.
2. The method for preparing cubic deflection structure polymerized nitrogen according to claim 1, characterized in that: In the step of pressurizing, the pressure is increased to 100 GPa to 120 GPa.
3. The method for preparing cubic deflection structure polymerized nitrogen according to claim 1, characterized in that: In the heating step, heating is performed to 2100K-2500K.
4. The method for preparing cubic deflection structure polymerized nitrogen according to any one of claims 1 to 3, characterized in that: The method for preparing the diamond anvil cell sample chamber comprises the following steps: Prepare the diamond anvil; Pre-pressing the gasket using the diamond anvil to form an indentation; A hole is punched at the center of the indentation, and the hole serves as a diamond anvil sample chamber.
5. The method for preparing cubic deflection structure polymerized nitrogen according to claim 4, characterized in that: The diameter of the anvil surface of the diamond anvil is selected from 70 μm to 90 μm; And / or, the diameter of the hole is selected from 30 μm-50 μm.
6. The method for preparing cubic deflection structure polymerized nitrogen according to claim 4, characterized in that: The thickness of the gasket is selected from 240 μm to 260 μm, and the thickness of the gasket after pre-compression is selected from 10 μm to 30 μm; And / or, the material of the gasket is selected from rhenium or tungsten.
7. Cubic deflected structure polymerized nitrogen prepared by the method for preparing cubic deflected structure polymerized nitrogen according to any one of claims 1 to 6.