A high-activity cerium oxide-based nano-abrasive and its preparation method and application
By adjusting the molar ratio and calcining conditions of the cerium source to yttrium nitrate hexahydrate and molten salt in the preparation of cerium oxide-based nano-abrasive particles, the problems of long periods and uneven sizes in the preparation of existing cerium oxide nano-abrasive particles were solved, and the problem of uneven sizes in the preparation of existing cerium oxide nano-abrasive particles was prepared. Highly reactive cerium oxide-based nano-abrasive particles are used in photocatalytic assisted chemical mechanical polishing, which significantly improves the material removal rate.
Patent Information
- Application Number
- CN202211629598.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-19
AI Technical Summary
The existing preparation methods for cerium oxide nanoparticles have long periods, abrasive particles agglomerate, uneven sizes, low photocatalytic activity, and it is difficult to balance chemical activity and mechanical properties.
The molar ratio of cerium source to yttrium nitrate hexahydrate and molten salt is 1: (0.01-0.2), and it is uniformly dispersed in anhydrous ethanol and magnetic stirring is followed by drying and calcining to obtain cerium oxide-based nano-abrasive particles. Adjust the roasting system to achieve controllable particle size, and combine deionized water washing and pH adjustment to prepare highly reactive ceria-based nano-abrasive particles.
The size controllable and high photocatalytic activity of ceria-based nano-abrasive particles is achieved. It is applied in photocatalytic assisted chemical mechanical polishing, which significantly improves the material removal rate and reaches 546.59nm/min.
Smart Images

Figure CN116002744B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photocatalytic assisted chemical mechanical polishing, and specifically relates to a high-activity cerium oxide-based nano-abrasive particle and a preparation method and application thereof. Background Art
[0002] In recent years, with the continuous improvement of the performance of electronic products such as mobile phones, tablet computers, and digital cameras, the surface quality of optical glass used in them has become more demanding. Chemical mechanical polishing, an ultra-precision processing technology based on the synergistic effect of mechanics and chemistry, is the only technology that can achieve global surface flattening in today's era. It has been widely used in the flattening of surfaces such as optical glass and wafers in integrated circuit manufacturing. Therefore, improving polishing performance has become the top priority of optical glass surface processing.
[0003] As one of the components of the chemical mechanical polishing system, polishing liquid is a key factor affecting the polishing quality and polishing efficiency. It is composed of deionized water, abrasive particles and other additives. Among them, abrasive particles are the most important component of polishing liquid, which has a direct impact on the performance of chemical mechanical polishing. Among them, CeO2 is considered to be one of the most effective abrasives because of its uniform tribochemical activity and chemical tooth effect. In addition, CeO2 has redox properties and variable valence state (Ce 4+ / Ce 3+ ), so it is also a rare earth semiconductor photocatalyst. However, in existing reports, the preparation method of cerium oxide nanoparticles has problems such as long cycle, abrasive agglomeration, uneven size, low photocatalytic activity, etc., and the existing synthesis method is difficult to balance between chemical activity and mechanical properties and photocatalytic performance. Therefore, it is of great practical significance to synthesize size-controlled, highly active cerium oxide-based nanoabrasives for photocatalytic assisted chemical mechanical polishing. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a high-activity cerium oxide-based nanoabrasive with a simple synthesis method, controllable size, and excellent photocatalytic assisted chemical mechanical polishing performance, as well as a preparation method and application thereof.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A highly active cerium oxide-based nano-abrasive and a preparation method thereof, comprising the following steps:
[0007] Step 1: according to the molar ratio of cerium source to yttrium nitrate hexahydrate being 1: (0.01-0.2), the molar ratio of the sum of cerium source and yttrium nitrate hexahydrate to molten salt being 1: (5-20), take the raw materials and grind them separately, then evenly disperse them in anhydrous ethanol, stir them magnetically for 30 minutes, and then dry them to obtain a mixed salt;
[0008] Step 2: Place the mixed salt obtained in step 1 into a muffle furnace for calcination treatment, heat it from room temperature to 500°C to 800°C at a rate of 2 to 5°C / min, keep it warm for 2 to 4 hours, then cool it to 400°C at a rate of 2 to 5°C / min, and then cool it naturally to room temperature. Wash the product after the reaction to obtain cerium oxide-based nano-abrasive particles.
[0009] The present invention also has the following technical features:
[0010] Preferably, the cerium source in step 1 is any one of cerium nitrate hexahydrate, cerium chloride hexahydrate, and cerium carbonate.
[0011] Preferably, the molten salt described in step one is two or more of potassium chloride, potassium nitrate, sodium chloride, sodium nitrate and lithium chloride.
[0012] Preferably, the drying treatment in step 1 is performed in a constant temperature drying oven at 50 to 80° C. for 4 to 5 hours.
[0013] Preferably, the washing agent in step 2 is repeatedly washed with deionized water for 3 to 5 times.
[0014] The present invention also protects a high-activity cerium oxide-based nano-abrasive grain prepared by the method as described above, wherein the grain size is 80-120 nm.
[0015] The present invention also protects the use of the above-mentioned highly active cerium oxide-based nano-abrasive particles in photocatalytically assisted chemical mechanical polishing.
[0016] Preferably, the following steps are used to prepare a highly active cerium oxide-based nano-abrasive polishing liquid:
[0017] Step 1, dispersing the obtained cerium oxide-based nano-abrasive particles in deionized water, and performing ball milling dispersion for 6 to 10 hours;
[0018] Step 2: Use a pH regulator to adjust the pH value of the dispersion prepared in step 1 to 6, and adjust the solid content to 0.5wt% to obtain a high-activity cerium oxide-based nano-abrasive polishing liquid for photocatalytically assisted chemical mechanical polishing.
[0019] Preferably, the pH adjuster is nitric acid and ammonium hydroxide.
[0020] Compared with the prior art, the present invention has the following technical effects:
[0021] The present invention uses Ce 3+ As raw material, Y 3+ As doping elements, potassium nitrate-potassium chloride is used as the molten salt system. The cerium oxide-based nano-abrasive particles synthesized by a simple molten salt method have a spherical or quasi-spherical microstructure. By adjusting the calcination system, the controllable preparation of 80-120nm abrasive particles can be achieved, and the size is controllable and the particle size distribution is uniform.
[0022] The quartz glass was surface processed by a polishing liquid used for photocatalytically assisted chemical mechanical polishing prepared by the cerium oxide-based nanoabrasive particles synthesized by the present invention, and the material removal rate reached 546.59 nm / min, thereby obtaining a high material removal rate. This is attributed to the high chemical activity and photocatalytic performance of the cerium oxide-based nanoabrasive particles synthesized by the present invention, which helps to improve the material removal rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The XRD spectrum of the cerium oxide-based nanoabrasive particles synthesized in Example 2;
[0024] Figure 2 This is a SEM image of the cerium oxide-based nanoabrasive particles synthesized in Example 2;
[0025] Figure 3 UV-visible absorption spectra of tetracycline solution degraded by cerium oxide-based nano-abrasive prepared in Example 2 at different times;
[0026] Figure 4 The material removal rate values of chemical mechanical polishing and photocatalytic assisted chemical mechanical polishing of the cerium oxide-based nano-abrasive polishing liquid prepared in Examples 1 to 4 and compared with Examples 1 to 4. DETAILED DESCRIPTION
[0027] The specific contents of the present invention are further explained in detail below in conjunction with embodiments.
[0028] Example 1
[0029] Step 1: Weigh 1.2701 g (0.002925 mol) of cerium nitrate hexahydrate, 0.0287 g (0.000075 mol) of yttrium nitrate hexahydrate, 0.2125 g (0.0027 mol) of potassium chloride, and 2.7449 g (0.0272 mol) of potassium nitrate, grind them separately, evenly disperse them in anhydrous ethanol, stir them magnetically for 30 min, and then dry them in a constant temperature drying oven at 50° C. for 5 h to obtain a mixed salt;
[0030] Step 2: Put the mixed salt obtained in step 1 into a crucible, place it in a muffle furnace, heat it from room temperature to 800°C at 5°C / min, keep it warm for 4 hours, calcine it, then cool it to 400°C at 2°C / min, and finally cool it naturally to room temperature. After washing it with deionized water for 5 times, disperse it in deionized water, and then ball-mill it for 8 hours to obtain Ce 0.975 Y 0.025 O2 nanoabrasive dispersion.
[0031] The Ce prepared in Example 1 of the present invention 0.975 Y 0.025 O2 nano-abrasive dispersion, adjust the solid content to 0.5wt%, and adjust the pH to 6.0 with nitric acid and ammonium hydroxide. The obtained polishing liquid is used for photocatalytic assisted chemical mechanical polishing of quartz glass. The polishing machine model is UNIPOL-1200S automatic pressure grinding and polishing machine, the polishing disk speed is 80r / min, the polishing head speed is 80r / min, the downward pressure is 3.0psi, the polishing time is 180s, the light source is a xenon lamp (model PLS-SXE300 / 300UV), the xenon lamp power is 300W, and the material removal rate is calculated by detecting the average value of the glass mass change before and after polishing.
[0032] Example 2
[0033] Step 1: Weigh 1.2375 g (0.00285 mol) of cerium nitrate hexahydrate, 0.0575 g (0.00015 mol) of yttrium nitrate hexahydrate, 0.2125 g (0.0027 mol) of potassium chloride, and 2.7449 g (0.0272 mol) of potassium nitrate, grind them separately, evenly disperse them in anhydrous ethanol, stir them magnetically for 30 min, and then dry them in a constant temperature drying oven at 60° C. for 4.5 h to obtain a mixed salt;
[0034] Step 2: Put the mixed salt obtained in step 1 into a crucible, place it in a muffle furnace, heat it from room temperature to 800°C at 5°C / min, keep it warm for 4 hours, calcine it, then cool it to 400°C at 2°C / min, and finally cool it naturally to room temperature. After washing it with deionized water for 5 times, disperse it in deionized water, and then ball-mill it for 8 hours to obtain Ce 0.95 Y 0.05 O2 nanoabrasive dispersion.
[0035] The Ce prepared in Example 2 of the present invention 0.95 Y 0.05O2 nano-abrasive dispersion, adjust the solid content to 0.5wt%, and adjust the pH to 6.0 with nitric acid and ammonium hydroxide. The obtained polishing liquid is used for photocatalytic assisted chemical mechanical polishing of quartz glass. The polishing machine model is UNIPOL-1200S automatic pressure grinding and polishing machine, the polishing disk speed is 80r / min, the polishing head speed is 80r / min, the downward pressure is 3.0psi, the polishing time is 180s, the light source is a xenon lamp (model PLS-SXE300 / 300UV), the xenon lamp power is 300W, and the material removal rate is calculated by detecting the average value of the glass mass change before and after polishing.
[0036] Example 3
[0037] Step 1: Weigh 1.1724 g (0.0027 mol) of cerium nitrate hexahydrate, 0.1149 g (0.0003 mol) of yttrium nitrate hexahydrate, 0.2125 g (0.0027 mol) of potassium chloride, and 2.7449 g (0.0272 mol) of potassium nitrate, grind them separately, evenly disperse them in anhydrous ethanol, stir them magnetically for 30 min, and then dry them in a constant temperature drying oven at 50° C. for 5 h to obtain a mixed salt;
[0038] Step 2: Put the mixed salt obtained in step 1 into a crucible, place it in a muffle furnace, heat it from room temperature to 800°C at 5°C / min, keep it warm for 4 hours, calcine it, then cool it to 400°C at 2°C / min, and finally cool it naturally to room temperature. After washing it with deionized water for 5 times, disperse it in deionized water, and then ball-mill it for 8 hours to obtain a cerium oxide-based nanoabrasive dispersion.
[0039] The Ce prepared in Example 3 of the present invention 0.90 Y 0.10 O2 nano-abrasive dispersion, adjust the solid content to 0.5wt%, and adjust the pH to 6.0 with nitric acid and ammonium hydroxide. The obtained polishing liquid is used for photocatalytic assisted chemical mechanical polishing of quartz glass. The polishing machine model is UNIPOL-1200S automatic pressure grinding and polishing machine, the polishing disk speed is 80r / min, the polishing head speed is 80r / min, the downward pressure is 3.0psi, the polishing time is 180s, the light source is a xenon lamp (model PLS-SXE300 / 300UV), the xenon lamp power is 300W, and the material removal rate is calculated by detecting the average value of the glass mass change before and after polishing.
[0040] Example 4
[0041] Step 1: Weigh 1.1073 g (0.00255 mol) of cerium nitrate hexahydrate, 0.1724 g (0.00045 mol) of yttrium nitrate hexahydrate, 0.2125 g (0.0027 mol) of potassium chloride, and 2.7449 g (0.0272 mol) of potassium nitrate, grind them separately, evenly disperse them in anhydrous ethanol, stir them magnetically for 30 min, and then dry them in a constant temperature drying oven at 80° C. for 4 h to obtain a mixed salt;
[0042] Step 2: Put the mixed salt obtained in step 1 into a crucible, place it in a muffle furnace, heat it from room temperature to 800°C at 5°C / min, keep it warm for 4 hours, calcine it, then cool it to 400°C at 2°C / min, and finally cool it naturally to room temperature. After washing it with deionized water for 5 times, disperse it in deionized water, and then ball-mill it for 8 hours to obtain Ce 0.85 Y 0.15 O2-based nanoabrasive dispersion.
[0043] The Ce prepared in Example 4 of the present invention 0.85 Y 0.15 O2 nano-abrasive dispersion, adjust the solid content to 0.5wt%, and adjust the pH to 6.0 with nitric acid and ammonium hydroxide. The obtained polishing liquid is used for photocatalytic assisted chemical mechanical polishing of quartz glass. The polishing machine model is UNIPOL-1200S automatic pressure grinding and polishing machine, the polishing disk speed is 80r / min, the polishing head speed is 80r / min, the downward pressure is 3.0psi, the polishing time is 180s, the light source is a xenon lamp (model PLS-SXE300 / 300UV), the xenon lamp power is 300W, and the material removal rate is calculated by detecting the average value of the glass mass change before and after polishing.
[0044] Example 5
[0045] Step 1: Weigh 1.2701 g (0.002925 mol) of cerium nitrate hexahydrate, 0.0112 g (0.000029 mol) of yttrium nitrate hexahydrate, 0.2457 g (0.0042 mol) of sodium chloride, and 0.8986 g (0.0106 mol) of sodium nitrate, grind them separately, evenly disperse them in anhydrous ethanol, stir them magnetically for 30 min, and then dry them in a constant temperature drying oven at 50° C. for 5 h to obtain a mixed salt;
[0046] Step 2: Put the mixed salt obtained in step 1 into a crucible, place it in a muffle furnace, heat it from room temperature to 500°C at 2°C / min, keep it warm for 3 hours, calcine it, then cool it to 400°C at 5°C / min, and finally cool it naturally to room temperature. After washing it with deionized water for 3 times, disperse it in deionized water, and then ball-mill it for 6 hours to obtain Ce 0.85 Y 0.15O2-based nanoabrasive dispersion.
[0047] The Ce prepared in Example 5 of the present invention 0.85 Y 0.15 O2 nano-abrasive dispersion, adjust the solid content to 0.5wt%, and adjust the pH to 6.0 with nitric acid and ammonium hydroxide. The obtained polishing liquid is used for photocatalytic assisted chemical mechanical polishing of quartz glass. The polishing machine model is UNIPOL-1200S automatic pressure grinding and polishing machine, the polishing disk speed is 80r / min, the polishing head speed is 80r / min, the downward pressure is 3.0psi, the polishing time is 180s, the light source is a xenon lamp (model PLS-SXE300 / 300UV), the xenon lamp power is 300W, and the material removal rate is calculated by detecting the average value of the glass mass change before and after polishing.
[0048] Example 6
[0049] Step 1: Weigh 1.1073 g (0.00255 mol) of cerium nitrate hexahydrate, 0.1954 g (0.00051 mol) of yttrium nitrate hexahydrate, 0.6795 g (0.009 mol) of potassium chloride, and 5.2722 g (0.0522 mol) of potassium nitrate, grind them separately, evenly disperse them in anhydrous ethanol, stir them magnetically for 30 min, and then dry them in a constant temperature drying oven at 80° C. for 4 h to obtain a mixed salt;
[0050] Step 2: Put the mixed salt obtained in step 1 into a crucible, place it in a muffle furnace, heat it from room temperature to 600°C at 3°C / min, keep it warm for 2h, calcine it, then cool it to 400°C at 3°C / min, and finally cool it naturally to room temperature. After washing it with deionized water for 3 times, disperse it in deionized water, and then ball-mill it for 10h to obtain Ce 0.85 Y 0.15 O2-based nanoabrasive dispersion.
[0051] The Ce prepared in Example 6 of the present invention 0.85 Y 0.15 O2 nano-abrasive dispersion, adjust the solid content to 0.5wt%, and adjust the pH to 6.0 with nitric acid and ammonium hydroxide. The obtained polishing liquid is used for photocatalytic assisted chemical mechanical polishing of quartz glass. The polishing machine model is UNIPOL-1200S automatic pressure grinding and polishing machine, the polishing disk speed is 80r / min, the polishing head speed is 80r / min, the downward pressure is 3.0psi, the polishing time is 180s, the light source is a xenon lamp (model PLS-SXE300 / 300UV), the xenon lamp power is 300W, and the material removal rate is calculated by detecting the average value of the glass mass change before and after polishing.
[0052] Comparative Example 1
[0053] The polishing liquid in Implementation 1 is applied to chemical mechanical polishing, the light source is removed, and the other polishing parameters are the same as in Example 1.
[0054] Comparative Example 2
[0055] The polishing liquid in Implementation 2 is applied to chemical mechanical polishing, the light source is removed, and the other polishing parameters are the same as in Example 2.
[0056] Comparative Example 3
[0057] The polishing liquid in Example 3 was applied to chemical mechanical polishing, the light source was removed, and the other polishing parameters were the same as in Example 3.
[0058] Comparative Example 4
[0059] The polishing liquid in Example 4 was applied to chemical mechanical polishing, the light source was removed, and the other polishing parameters were the same as in Example 4.
[0060] Comparative Example 5
[0061] The polishing liquid in Example 5 was applied to chemical mechanical polishing, the light source was removed, and the other polishing parameters were the same as in Example 5.
[0062] Comparative Example 6
[0063] The polishing liquid in Example 6 was applied to chemical mechanical polishing, the light source was removed, and the other polishing parameters were the same as in Example 6.
[0064] Figure 1 This is the XRD spectrum of the cerium oxide-based nano-abrasive prepared in Example 2. As shown in the figure, no second phase peak appears, and the crystallinity is high. Compared with the PDF card (#PDF 34-0394), it shows that the cerium oxide-based nano-abrasive with a cubic fluorite structure is successfully prepared.
[0065] Figure 2 This is a SEM image of the cerium oxide-based nanoabrasive prepared in Example 2. When the cerium oxide-based nanoabrasive synthesized in the present invention is used in photocatalytically assisted chemical mechanical polishing, if the nanoabrasive size is too large, the specific surface area of the nanoabrasive will be reduced, and the photocatalytic activity of the abrasive will be reduced; if the nanoabrasive size is too small, the polishing performance of the nanoabrasive will be reduced. Therefore, the appropriate abrasive size is the key to improving the photocatalytically assisted chemical mechanical polishing of cerium oxide-based nanoabrasives. As shown in the figure, the abrasive size synthesized in the present invention is 90-110nm, with a moderate size and uniform dispersion.
[0066] Figure 3The UV-visible absorption spectra of the tetracycline solution degraded by the cerium oxide-based nanoabrasive prepared in Example 2 at different times; 25 mg of cerium oxide-based nanoparticles were added to a 10 mg / L tetracycline (TC) solution, and the dark reaction lasted for 60 minutes, followed by a photodegradation reaction for 60 minutes. During this period, samples were taken every 15 minutes, and the absorbance of the supernatant was tested. Figure 3 As shown in the figure, after 30 min of photodegradation, TC has been almost completely degraded. This is because the prepared cerium oxide-based nanoabrasives form more oxygen vacancy defects. In order to balance the charge, more Ce 4+ Transformed to Ce 3+ , so that Ce 3+ The concentration is relatively high, and has higher chemical activity. It can be seen that the cerium oxide-based nanoparticles synthesized in the present invention have high photocatalytic activity.
[0067] Figure 4 The material removal rate values of chemical mechanical polishing and photocatalytic assisted chemical mechanical polishing of the cerium oxide-based nanoabrasive polishing liquids prepared in Examples 1 to 4 and Comparative Examples 1 to 4 show that the effect of the polishing liquid prepared with the cerium oxide-based nanoabrasives synthesized in the present invention in photocatalytic assisted chemical mechanical polishing is better than that of chemical mechanical polishing. This is because the cerium oxide-based nanoabrasives synthesized in the present invention have excellent photocatalytic activity, and therefore have higher polishing performance when applied to photocatalytic assisted chemical mechanical polishing.
[0068] Table 1 shows the polishing results corresponding to the polishing liquids prepared in Examples 1 to 4 and Comparative Examples 1 to 4:
[0069] Table 1
[0070]
[0071] The above specific embodiments are only selected examples to clearly illustrate the effects that can be achieved by the present invention, and cannot be simply considered as all implementation schemes of the present invention. For practitioners in the relevant field, other changes can be made on the basis of the above scheme description, which cannot be exhaustively listed here. Any changes in numerical values derived from the design principles of the present invention still fall within the scope of protection of the claims of the present invention.
Claims
1. Application of a highly active cerium oxide-based nano-abrasive in photocatalytically assisted chemical mechanical polishing. It is characterized in that The method for preparing highly active cerium oxide-based nano-abrasive particles comprises the following steps: Step 1: according to the molar ratio of cerium source to yttrium nitrate hexahydrate being 1: (0.01-0.2), the molar ratio of the sum of cerium source and yttrium nitrate hexahydrate to molten salt being 1: (5-20), take the raw materials and grind them separately, then evenly disperse them in anhydrous ethanol, stir them magnetically for 30 minutes, and then dry them to obtain a mixed salt; Step 2: Place the mixed salt obtained in step 1 into a muffle furnace for calcination, heat it from room temperature to 500°C to 800°C at a rate of 2 to 5°C / min, keep it warm for 2 to 4 hours, cool it to 400°C at a rate of 2 to 5°C / min, and then cool it naturally to room temperature. Wash the reaction product to obtain cerium oxide-based nano-abrasive particles with a particle size of 80 to 120 nm.
2. Use of the highly active cerium oxide-based nanoabrasive particles as claimed in claim 1 in photocatalytically assisted chemical mechanical polishing, It is characterized in that The cerium source described in step 1 is any one of cerium nitrate hexahydrate, cerium chloride hexahydrate, and cerium carbonate.
3. Use of the highly active cerium oxide-based nano-abrasive particles as claimed in claim 1 in photocatalytically assisted chemical mechanical polishing, It is characterized in that The molten salt described in step 1 is two or more of potassium chloride, potassium nitrate, sodium chloride, sodium nitrate and lithium chloride.
4. Use of the highly active cerium oxide-based nanoabrasive particles as claimed in claim 1 in photocatalytically assisted chemical mechanical polishing, It is characterized in that The drying process described in step 1 is to dry in a constant temperature drying oven at 50 to 80° C. for 4 to 5 hours.
5. Use of the highly active cerium oxide-based nano-abrasive particles as claimed in claim 1 in photocatalytically assisted chemical mechanical polishing, It is characterized in that The washing in step 2 is repeated 3 to 5 times using deionized water.
6. Use of the highly active cerium oxide-based nano-abrasive particles as claimed in claim 1 in photocatalytically assisted chemical mechanical polishing, It is characterized in that The following steps are used to prepare a highly active cerium oxide-based nano-abrasive polishing liquid: Step 1, dispersing the obtained cerium oxide-based nano-abrasive particles in deionized water, and performing ball milling dispersion for 6 to 10 hours; Step 2: Use a pH regulator to adjust the pH value of the dispersion prepared in step 1 to 6, and adjust the solid content to 0.5wt% to obtain a high-activity cerium oxide-based nano-abrasive polishing liquid for photocatalytically assisted chemical mechanical polishing.
7. Use of the highly active cerium oxide-based nano-abrasive particles as claimed in claim 6 in photocatalytically assisted chemical mechanical polishing, It is characterized in that The pH regulators are nitric acid and ammonium hydroxide.