Organic-inorganic composite dispersion and method for producing the same

By polymerizing methacrylamide monomers under specific reaction conditions to form large-particle organic and inorganic composite particles, the problem of insufficient membrane-forming properties and water resistance of the dry coating of cell culture substrates in the prior art is solved, and the problem of insufficient membrane-forming properties and water resistance of the cell culture substrate in the prior art is realized. Excellent cell culture substrate performance.

CN116018357BInactive Publication Date: 2024-12-06FUJIFILM CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202180054512.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-04
Filing Date
2021-09-02
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, the dry coating used in cell culture substrates has insufficient performance in terms of membrane-forming properties and water resistance, and it is difficult to meet the stability requirements under culture conditions.

Method used

By polymerizing the methacrylamide monomer under specific reaction conditions, organic and inorganic composite particles with large particle size are formed, and dispersed in an aqueous medium to form an organic and inorganic composite dispersion liquid to obtain excellent film making Dry coating with water resistance.

Benefits of technology

Good membrane-forming properties and water resistance for the dry coating of the cell culture substrate are achieved, ensuring the stability and performance of the cell culture substrate during use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004107108210000201
    Figure BDA0004107108210000201
Patent Text Reader

Abstract

The present invention aims to provide an organic-inorganic composite dispersion liquid which is used to form a dry film of a cell culture substrate and can form a dry film having good film forming properties and water resistance. The problem is solved by the following organic-inorganic composite dispersion liquid: in the organic-inorganic composite dispersion liquid, organic-inorganic composite particles (X) formed by forming a three-dimensional grid by a polymer (P) of a monomer including a (meth)acrylamide-based monomer (a) and one or more inorganic materials (B) selected from water-swellable clay minerals and silica are dispersed in an aqueous medium (C), and the average particle size of the organic-inorganic composite particles (X) is 100 nm or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an organic-inorganic composite dispersion in an aqueous medium (C), which is obtained by forming a three-dimensional mesh of an organic-inorganic composite particle (X) of a polymer (P) of (meth)acrylamide monomer (a) and a water-swellable clay mineral (B). Background Technology

[0002] An organic-inorganic composite dispersion is known to be formed by a polymer (P) containing a monomer (a) of (meth)acrylamide and one or more inorganic materials (B) selected from water-swellable clay minerals and silica, forming a three-dimensional mesh, and the resulting organic-inorganic composite particles (X) are dispersed in an aqueous medium (C) (for example, see Patent Document 1).

[0003] Furthermore, the aforementioned Patent Document 1 describes the following: the dried coating of organic-inorganic complex particles (X) obtained by drying the organic-inorganic complex dispersion is used as a cell culture medium.

[0004] Existing technical documents

[0005] Patent documents

[0006] Patent Document 1: Japanese Patent Application Publication No. 2011-144236 Summary of the Invention

[0007] The technical problem to be solved by the invention

[0008] For cell culture media having a dry coating obtained by coating the aforementioned organic-inorganic composite particles (X) and drying it, which serves as the substrate for culturing cells—that is, the substrate that becomes the platform for culturing cells—it is required that it does not undergo modification under culture conditions. For example, when various culture media are added to the cell culture media during cell culture, the cell culture media must be water-resistant to prevent modification such as dissolution of the cell culture media.

[0009] However, the cell culture medium with a dry film obtained from a dry organic-inorganic complex dispersion described in the above-mentioned reference 1 cannot be said to have sufficient performance in terms of film-forming properties and water resistance, and there is room for improvement.

[0010] Therefore, the object of the present invention is to provide an organic-inorganic composite dispersion for forming a dry coating of cell culture medium and capable of forming a dry coating exhibiting good film-forming properties and water resistance.

[0011] means for solving technical problems

[0012] As a result of in-depth research conducted by the inventors to solve the above-mentioned problems, it was discovered that by polymerizing (meth)acrylamide monomers (a) under specific reaction conditions, large-particle-size organic-inorganic composite particles (X) can be obtained. When the organic-inorganic composite dispersion (X) is dispersed in an aqueous medium (C) to form a dry film, a dry film with excellent film-forming properties and water resistance can be formed, thereby solving the above-mentioned problems and thus completing the present invention.

[0013] That is, the present invention includes the following methods.

[0014] [1] An organic-inorganic complex dispersion, wherein,

[0015] Organic-inorganic composite particles (X), obtained by forming a three-dimensional mesh of a polymer (P) containing a monomer (a) of (meth)acrylamide type (a) and one or more inorganic materials (B) selected from water-swellable clay minerals and silica, are dispersed in an aqueous medium (C).

[0016] The average particle size of the organic-inorganic composite particles (X) is above 100 nm.

[0017] [2] According to the organic-inorganic complex dispersion described in [1], wherein,

[0018] The mass ratio ((B) / (P)) of the polymer (P) to one or more inorganic materials (B) selected from water-swellable clay minerals and silica is in the range of 0.01 to 10.

[0019] [3] The organic-inorganic complex dispersion according to [1] or [2], wherein,

[0020] The (meth)acrylamide monomer (a) is selected from one or more (meth)acrylamide monomers selected from N-substituted (meth)acrylamide derivatives, N,N-disubstituted (meth)acrylamide derivatives, and N,N'-methylenebisacrylamide.

[0021] [4] An organic-inorganic complex dispersion according to any one of [1] to [3], wherein,

[0022] The water-swellable clay mineral is at least one clay mineral selected from water-swellable lithium montmorillonite, water-swellable montmorillonite, water-swellable saponite, and water-swellable synthetic mica, which is layered into 1 to 10 layers in the aqueous medium (C), and the silica is colloidal silica with water dispersibility.

[0023] [5] A dry coating, which is a dry coating of said organic-inorganic complex particles (X) obtained by drying an organic-inorganic complex dispersion as described in any one of [1] to [4].

[0024] [6] A cell culture medium having the dry coating described in [5] on its surface.

[0025] [7] The cell culture medium according to [6] has a support and the dry coating laminated on the support.

[0026] [8] A method for manufacturing an organic-inorganic composite dispersion, wherein,

[0027] In the organic-inorganic complex dispersion, the organic-inorganic complex particles (X) are dispersed in an aqueous medium (C).

[0028] The method for manufacturing the organic-inorganic composite dispersion includes:

[0029] The process of forming organic-inorganic composite particles (X) by polymerizing (meth)acrylamide monomer (a) after mixing (meth)acrylamide monomer (a), one or more inorganic materials (B) selected from water-swellable clay minerals and silica, polymerization initiator (D), and aqueous medium (C).

[0030] The concentration (mass%) of one or more inorganic materials (B) selected from water-swellable clay minerals and silica in the aqueous medium (C) is within the range expressed by the following formula (1) or formula (2).

[0031] When polymerizing the (meth)acrylamide monomer (a), polymerization is carried out after the temperature conditions of the aqueous medium (C) are set above the LCST (lower critical solution temperature) of the organic-inorganic composite dispersion.

[0032] When Ra < 0.19 in equation (1),

[0033] The concentration (mass%) of inorganic material (B) is <12.4Ra + 0.05.

[0034] When Ra≥0.19 in equation (2),

[0035] The concentration (mass%) of inorganic material (B) is <0.87Ra + 2.17.

[0036] (In the formula, the concentration (mass%) of inorganic material (B) is obtained by dividing the mass of inorganic material (B) by the total mass of aqueous medium (C) and inorganic material (B) and then multiplying by 100. Ra is the mass ratio of inorganic material (B) to polymer (P) ((B) / (P)).)

[0037] [9] According to the method for manufacturing the organic-inorganic composite dispersion described in [8], wherein,

[0038] The temperature condition of the aqueous medium (C) is above 10°C of the LCST of the organic-inorganic composite dispersion.

[0039]

[10] The method for manufacturing the organic-inorganic complex dispersion according to [8] or [9], wherein,

[0040] When polymerizing the (meth)acrylamide monomer (a), the (meth)acrylamide monomer (a) is polymerized by a polymerization reaction based on heating or ultraviolet irradiation.

[0041]

[11] The method for manufacturing an organic-inorganic complex dispersion according to any one of [8] to

[10] , wherein,

[0042] When polymerizing the (meth)acrylamide monomer (a), the temperature conditions of the aqueous medium (C) are set to 45°C to 55°C. Potassium persulfate and N,N,N',N'-tetramethylethylenediamine are used as polymerization initiators or catalysts, and the (meth)acrylamide monomer (a) is polymerized through a heating-based polymerization reaction.

[0043] Invention Effects

[0044] According to the present invention, an organic-inorganic composite dispersion is provided for forming a dry coating of cell culture medium and is capable of forming a dry coating exhibiting good film-forming properties and water resistance. Detailed Implementation

[0045] The present invention will now be described in detail. Furthermore, the following description of the constituent elements is for illustrative purposes only and the present invention is not limited to these contents.

[0046] Furthermore, the description of "(meth)acrylamide monomers" indicates both acrylamide monomers and methacrylamide monomers.

[0047] (Organic-inorganic complex dispersion)

[0048] The organic-inorganic complex dispersion is formed by dispersing organic-inorganic complex particles (X) in an aqueous medium (C).

[0049] Organic-inorganic composite particles (X) are obtained by forming a three-dimensional mesh from polymer (P) and inorganic material (B).

[0050] The polymer (P) is obtained by polymerizing a monomer containing a (meth)acrylamide monomer (a).

[0051] The inorganic material (B) is composed of one or more selected from water-swellable clay minerals and silica.

[0052] The average particle size of the organic-inorganic complex particles (X) in the organic-inorganic complex dispersion is greater than 100 nm.

[0053] The following is a detailed description of each component that makes up the organic-inorganic complex dispersion.

[0054] <(meth)acrylamide monomers (a)>

[0055] As a (meth)acrylamide monomer (a), it can be appropriately used as long as its polymer (P) can interact with the inorganic material (B) to form organic-inorganic composite particles. Among them, N-substituted (meth)acrylamide derivatives such as N-methyl (meth)acrylamide, N-ethyl (meth)acrylamide, and N-isopropyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-disubstituted (meth)acryloylmorpholine, N,N'-methylenebisacrylamide, and N,N-dimethylaminoethyl (meth)acrylate can be used. Two or more of these monomers (a) can be used in combination.

[0056] In the case of polymers (P) with LCST (lower critical solution temperature) among the monomers (a) above, for example, if N-isopropylacrylamide is used, a dispersion with energy-saving dimming function in which the transparency of the dispersion changes with the ambient temperature can be obtained.

[0057] <Polymer (P)>

[0058] The polymer (P) is obtained by polymerizing a monomer containing the above-mentioned (meth)acrylamide monomer (a).

[0059] In addition to the (meth)acrylamide monomer (a) described above, other polymeric monomers can be used simultaneously as needed to impart a balance of hydrophilicity and hydrophobicity or functional groups to the organic-inorganic complex. That is, the polymer (P) can be obtained by polymerizing the (meth)acrylamide monomer (a) described above with other polymeric monomers.

[0060] For example, as other polymerization monomers, (meth)acrylate monomers with anionic groups such as sulfone and carboxyl groups can be used simultaneously; (meth)acrylate monomers with cationic groups such as quaternary ammonium groups; (meth)acrylate monomers with zwitterionic groups containing quaternary ammonium and phosphate groups; (meth)acrylate monomers with amino acid residues containing carboxyl and amino groups; (meth)acrylate monomers with sugar residues; (meth)acrylate monomers with hydroxyl groups; (meth)acrylate monomers with polyethylene glycol and polypropylene glycol chains; amphiphilic (meth)acrylate monomers with both hydrophilic chains such as polyethylene glycol and hydrophobic groups such as nonylphenyl; polyethylene glycol diacrylate; methoxyethyl (meth)acrylate; etc.

[0061] <Inorganic Materials (B)>

[0062] The inorganic material (B) used in this invention is selected from one or more inorganic materials selected from water-swellable clay minerals and silica.

[0063] Examples of water-swellable clay minerals include swellable clay minerals that can be peeled off in layers. Clay minerals that can swell and disperse uniformly in water or a mixture of water and an organic solvent are preferred. Inorganic clay minerals that can be uniformly dispersed in water at a molecular (monolayer) level or close to that level are particularly preferred.

[0064] Furthermore, the water-swellable clay mineral is preferably a clay mineral that has been exfoliated into 1 to 10 layers in an aqueous medium (C).

[0065] Specifically, examples of water-swellable clay minerals include water-swellable lithium montmorillonite, water-swellable montmorillonite, water-swellable saponite, and water-swellable synthetic mica, all of which contain sodium as an interlayer ion. These clay minerals can be used in combination.

[0066] As the silica (SiO2) used in this invention, colloidal silica can be cited as an example. Colloidal silica that can be uniformly dispersed in aqueous solution and has a particle size of 10 nm to 500 nm is preferred. Colloidal silica with a particle size of 10 to 50 nm is particularly preferred.

[0067] By using inorganic material (B), a dry coating with good stability and coating formation ability of organic-inorganic composite dispersion and excellent anti-fogging properties can be obtained.

[0068] In this invention, from the viewpoint of obtaining organic-inorganic composite particles (X) with a more desirable particle size, water-swellable clay minerals are preferred over silica.

[0069] <Organic-inorganic complex particles (X)>

[0070] The organic-inorganic composite particles (X) are obtained by forming a three-dimensional mesh from the above-mentioned polymer (P) and the above-mentioned inorganic material (B).

[0071] The mass ratio of polymer (P) to inorganic material (B) ((B) / (P)) is preferably 0.01 to 10, more preferably 0.03 to 5, and particularly preferably 0.05 to 3.

[0072] If the mass ratio ((B) / (P)) is within this range, the obtained organic-inorganic composite dispersion has excellent stability and can easily produce a smooth film with strong adhesion to the substrate.

[0073] As described above, the average particle size of the organic-inorganic composite particles (X) dispersed in the organic-inorganic composite dispersion is 100 nm or more. Thus, the organic-inorganic composite particles (X) of the present invention exhibit a large average particle size of 100 nm or more. Consequently, as shown in the following examples, the dry coating obtained by coating the organic-inorganic composite dispersion of the present invention, which disperses such large-sized organic-inorganic composite particles, exhibits excellent film-forming properties and water resistance.

[0074] In order to form the organic-inorganic composite particles (X) of the particle size specified in this invention, it is necessary to consider the types and amounts of polymerization catalysts and initiators used when polymerizing monomers containing (meth)acrylamide monomers (a), the types and amounts of various components constituting the organic-inorganic composite particles (X), and the amount of aqueous medium (C), etc., and to polymerize monomers containing (meth)acrylamide monomers (a) under specific polymerization temperature conditions. The method for preparing organic-inorganic composite particles (X) including polymerization temperature conditions will be described in detail in the section below (Method for Preparing Organic-Inorganic Composite Dispersion).

[0075] The average particle size of the organic-inorganic composite particles (X) is 100 nm or more, preferably 150 nm or more, and more preferably 200 nm or more. If it is 100 nm or more, film-forming properties and water resistance can be obtained. If it is 200 nm or more, it is envisioned that the film-forming properties will be even higher.

[0076] Furthermore, taking into account dispersibility, transparency of the coating, etc., the average particle size of the organic-inorganic composite particles (X) is preferably 1,000 nm or less, more preferably 800 nm or less, and even more preferably 700 nm or less.

[0077] [Method for determining the average particle size of organic-inorganic complex particles (X)]

[0078] The average particle size of latex particles can be determined by the 50% median particle size measured by dynamic light scattering, for example, by the 50% median particle size measured by a volume reference device (e.g., HORIBA, Ltd. Dynamic Light Scattering Particle Size Distribution Measurement Device LB-550).

[0079] <Water Medium (C)>

[0080] The aqueous medium (C) used in the manufacturing method of the present invention can contain (meth)acrylamide monomers (a), inorganic materials (B), etc., and is not particularly limited as long as a dispersion of organic-inorganic complex with good physical properties can be obtained. For example, it can be water, or an aqueous solution containing solvents and / or other compounds that are miscible with water, and can also contain preservatives or antibacterial agents, colorants, fragrances, enzymes, proteins, sugars, amino acids, cells, DNA, salts, water-soluble organic solvents, surfactants, polymers, leveling agents, etc.

[0081] <Characteristics of Organic-Inorganic Complex Dispersions>

[0082] The water resistance of the dried film can be evaluated by performing a gel fraction determination test using a dried film obtained by coating the organic-inorganic composite dispersion of the present invention into a film and then drying it.

[0083] The dried film obtained using the organic-inorganic composite dispersion of the present invention exhibits a high gel fraction, thus demonstrating excellent film-forming properties and water resistance.

[0084] The gel fraction of the dried film obtained using the organic-inorganic composite dispersion of the present invention is preferably 80% or more, more preferably 90% or more, and even more preferably 95% or more.

[0085] [Method for determining the gel fraction of organic-inorganic complex dispersions]

[0086] As shown in the following examples, the gel fraction of the dried film obtained using the organic-inorganic composite dispersion of the present invention can be determined by preparing the film and measuring the weight reduction rate of the film.

[0087] The organic-inorganic composite dispersion is cast onto a PP tray of approximately 15cm × 20cm until the thickness reaches 10–500μm. After drying at room temperature, it is dried at 130°C for 1 hour to obtain a dry coating film (hereinafter referred to as the dry coating film).

[0088] Approximately 0.2 g of the dried coating obtained by wrapping it with a 200-mesh stainless steel mesh was dried at 130°C for 2 hours and its weight was measured. Afterward, the coating, along with the mesh, was placed in water at approximately 23°C for 20–24 hours. It was then removed and dried in a hot air dryer at 130°C for 2 hours, and its weight was measured again. Based on the measured weights, the weight loss rate before and after standing in water was determined. This value was taken as the gel fraction (%).

[0089] It can be said that the higher the gel fraction (%) value, the higher the water resistance of the dried coating film, and the less likely it is to dissolve due to water or culture medium when it is made into a dried culture medium.

[0090] (Preparation method of organic-inorganic complex dispersion)

[0091] The method for manufacturing an organic-inorganic complex dispersion in which organic-inorganic complex particles (X) are dispersed in an aqueous medium (C) is described in detail below.

[0092] The method for manufacturing the organic-inorganic composite dispersion of the present invention includes a step of polymerizing the (meth)acrylamide monomer (a), one or more inorganic materials (B) selected from water-swellable clay minerals and silica, a polymerization initiator (D) and an aqueous medium (C) to form organic-inorganic composite particles (X).

[0093] As a preferred embodiment of the method for manufacturing the organic-inorganic complex dispersion of the present invention, a method for manufacturing the organic-inorganic complex dispersion including the following steps (I) to (II) can be cited:

[0094] (I) A process of mixing (meth)acrylamide monomers (a), one or more inorganic materials (B) selected from water-swellable clay minerals and silica, a polymerization initiator (D), and an aqueous medium (C); and

[0095] (II) The process of polymerizing (meth)acrylamide monomers (a).

[0096] The following is a detailed description of each process.

[0097] <(I) Process: Mixed Process>

[0098] The (meth)acrylamide monomer (a), one or more inorganic materials selected from water-swellable clay minerals and silica (B), and a polymerization initiator (D) are mixed and dissolved or uniformly dispersed in an aqueous medium (C).

[0099] In addition, regarding the (meth)acrylamide monomer (a), one or more inorganic materials selected from water-swellable clay minerals and silica as components of the mixture (B), and the aqueous medium (C), as described in the above items (organic-inorganic composite dispersion).

[0100] <<Polymerization Initiator (D)>>

[0101] As the polymerization initiator (D) that can be used in the manufacturing method of the present invention, a known free radical polymerization initiator can be selected as appropriate. It is preferable to have water dispersibility, and it is preferable to use a polymerization initiator that is uniformly contained throughout the system. Specifically, examples of polymerization initiators include water-soluble peroxides (e.g., potassium persulfate and ammonium persulfate), water-soluble azo compounds (e.g., VA-044, V-50, V-501 (all manufactured by FUJIFILM Wako Pure Chemical Corporation), photopolymerization initiators (Irg184, etc.), and Fe... 2+ Mixtures with hydrogen peroxide, etc.

[0102] As a catalyst, N,N,N',N'-tetramethylethylenediamine, as a tertiary amine compound, is preferred. However, the use of a catalyst is not always necessary.

[0103] On the other hand, photopolymerization initiators are preferred because they are less susceptible to oxygen inhibition and have a fast polymerization rate. Specifically, examples include acetophenones such as p-tert-butyltrichloroacetophenone, benzophenones such as 4,4'-bis(dimethylamino)benzophenone, ketones such as 2-methylthioxanthone, benzoin ethers such as benzoin methyl ether, α-hydroxy ketones such as hydroxycyclohexylphenyl ketone, phenyl glyoxylates such as methyl benzoate, and metallocenes.

[0104] The photopolymerization initiator is preferably water-insoluble. Water-insoluble here means that the initiator's solubility in water is less than 0.5% by mass. By using a water-insoluble initiator, the initiator is more likely to exist near the inorganic material (B), increasing the number of reaction sites near the inorganic material (B), resulting in a narrower particle size distribution of the obtained organic-inorganic composite and higher dispersion stability, which is preferable. Regarding film-forming properties and water resistance, any polymerization method can be used. Regarding particle size, for example, compared to UV photopolymerization of Irg184, thermal polymerization using potassium persulfate tends to result in larger particle sizes, and the particle size tends to become even larger when using amine catalysts such as potassium persulfate and N,N,N',N'-tetramethylethylenediamine. It is considered that UV polymerization is not easily mass-produced, while thermal polymerization is easier to mass-produce and is a more preferred method.

[0105] Preferably, the photopolymerization initiator is dissolved in a solvent (F) that is miscible with the aqueous medium (C) and added to the aqueous medium (C). This method allows for more uniform dispersion of the photopolymerization initiator, resulting in composite particles with more uniform particle size.

[0106] As the solvent (F) of this invention, a water-soluble solvent capable of dissolving the non-water-soluble photopolymerization initiator, or (meth)acrylamide monomers (a) and other water-soluble acrylic monomers (a') can be used. Examples of water-soluble solvents include amides such as dimethylacetamide and dimethylformamide, alcohols such as methanol and ethanol, dimethyl sulfoxide, and tetrahydrofuran. These solvents can be used in combination.

[0107] Furthermore, examples of (meth)acrylamide monomers (a) or water-soluble acrylic monomers (a') that can be used as solvents (F) include, for example, polypropylene glycol diacrylates such as tripropylene glycol diacrylate, polyethylene glycol diacrylates, polypropylene glycol acrylates such as pentapropylene glycol acrylate, polyethylene glycol acrylates, methoxyethyl acrylates, methoxytriethylene glycol acrylates such as methoxy polyethylene glycol acrylate, nonylphenoxy polyethylene glycol acrylate, N-substituted acrylamides such as dimethacrylamide, hydroxyethyl acrylate, and hydroxypropyl acrylate. Two or more of these acrylic monomers can be used in combination.

[0108] The water-soluble solvent mentioned here is preferably one that can dissolve more than 50g of water in 100g of water. Within this range, the non-water-soluble photopolymerization initiator (D) disperses well in the aqueous medium (C), the obtained organic-inorganic composite particles have uniform particle size, and the dispersion has good stability.

[0109] The mass ratio (D) / (F) of the photopolymerization initiator (D) to the solvent (F) in the solution of the non-water-soluble photopolymerization initiator (D) is preferably 0.001 to 0.1, more preferably 0.01 to 0.05. If it is 0.001 or higher, the amount of free radicals generated based on energy ray irradiation can be sufficiently obtained, and thus the polymerization reaction can be carried out appropriately. If it is 0.1 or lower, the color development and odor caused by the initiator will not occur substantially, and the cost can be reduced.

[0110] In any of the above-mentioned acrylic monomers (a') and water-soluble solvents, the amount of solution in which the photopolymerization initiator (D) is dissolved in the solvent (F) is preferably 0.1% to 5% by mass, more preferably 0.2% to 2% by mass, relative to the total mass of the (meth)acrylamide monomer (a), inorganic material (B), aqueous medium (C), polymerization initiator (D), and solvent (F). If the amount added is 0.1% by mass or more, polymerization can be sufficiently initiated; if it is less than 5% by mass, the generation of odor caused by the increase of polymerization initiator in the organic-inorganic composite particles (X) can be reduced, and problems such as re-agglomeration of temporarily dispersed photopolymerization initiators can be reduced, resulting in a uniform organic-inorganic composite dispersion, which is therefore preferred.

[0111] Furthermore, in the method for manufacturing the organic-inorganic composite dispersion of the present invention, the concentration (mass%) of one or more inorganic materials (B) selected from water-swellable clay minerals and silica in the aqueous medium (C) is expressed as a range by the following formula (1) or formula (2).

[0112] When Ra < 0.19 in equation (1),

[0113] The concentration (mass%) of inorganic material (B) is < 12.4Ra + 0.05

[0114] When Ra≥0.19 in equation (2),

[0115] The concentration (mass%) of inorganic material (B) is <0.87Ra+2.17

[0116] (In the formula, the concentration (mass%) of inorganic material (B) is obtained by dividing the mass of inorganic material (B) by the total mass of aqueous medium (C) and inorganic material (B) and then multiplying by 100; Ra is the mass ratio of inorganic material (B) to polymer (P) ((B) / (P)).)

[0117] By satisfying formula (1) or formula (2) above, the particulate organic-inorganic composite is uniformly dispersed in an aqueous medium, forming a good latex without gelling. If the concentration (mass%) of the inorganic material (B) in the aqueous medium is above the above range, the entire reaction system will gel due to polymerization, or the organic-inorganic composite dispersion will become uneven, thus making it impossible to produce a good organic-inorganic composite dispersion.

[0118] <(II) Process: The process of polymerizing (meth)acrylamide monomer (a)>

[0119] The method for manufacturing the organic-inorganic composite dispersion of the present invention is characterized in that, when polymerizing the (meth)acrylamide monomer (a), if the polymer uses a monomer having a lower critical solution temperature (LCST), the temperature conditions of the aqueous medium (C) are set to be above the LCST (lower critical solution temperature) of the organic-inorganic composite dispersion before polymerization.

[0120] The inventors have discovered that when polymerizing (meth)acrylamide monomers (a), if the polymerization temperature is set to a high temperature above the LCST (lower critical solution temperature) of the organic-inorganic composite dispersion, as described above, organic-inorganic composite particles (X) with a large particle size of 100 nm or more can be obtained. This is much larger than the particle size of previously known organic-inorganic composite particles. The reason for obtaining such large-sized organic-inorganic composite particles (X) is speculated as follows: It is believed that since the organic-inorganic composite particles (X) obtained in this invention inherently possess temperature-responsive properties, the physical properties of the polymer differ when polymerization is carried out at higher temperatures versus at temperatures below room temperature. Therefore, it is believed that by raising the temperature above the LCST during polymerization, the polymers interact with each other, easily entangle, and polymerize in an entangled state to obtain large-sized organic-inorganic composite particles. Furthermore, it is believed that by increasing the temperature, free radical movement occurs and cross-linking occurs, thereby increasing the particle size through polymerization in a three-dimensional polymer manner, such as branched polymers.

[0121] Furthermore, it is believed that the excellent film-forming properties and water resistance of the dried coating obtained by using an organic-inorganic composite dispersion with such large particle size are due to the increased crosslinking density caused by the increased number of crosslinking points in the organic-inorganic composite particles, which in turn leads to higher water resistance during film formation.

[0122] The LCST (lower critical solution temperature) of an organic-inorganic complex dispersion varies depending on the LCST of polymer P, the types of various components constituting the organic-inorganic complex particles (X), etc., and can be determined by the following measurements.

[0123] [Method for determining LCST of organic-inorganic complex dispersions]

[0124] Using a temperature-variable UV-Vis spectrophotometer with LCST, the temperature of the tank containing the organic-inorganic complex dispersion is increased at a rate of 10°C / 60 minutes while the temperature is observed, and the turbidity initiation temperature (LCST) of the organic-inorganic complex dispersion is determined. For example, the transmittance at 600 nm is measured, and the temperature at which the transmittance becomes below 50% and turbidity occurs is read.

[0125] The polymerization temperature condition for polymerizing (meth)acrylamide monomers (a), i.e., the temperature condition of the aqueous medium (C), is above the LCST of the organic-inorganic composite dispersion, and more preferably at a temperature 10°C or higher than the LCST.

[0126] Furthermore, more specifically, the temperature condition of the aqueous medium (C) for polymerizing the (meth)acrylamide monomer (a) is preferably 35°C or higher, more preferably 40°C or higher. Also, as the same temperature condition, to prevent side reactions in the water, it is preferably 90°C or lower, more preferably 80°C or lower, and even more preferably 70°C or lower.

[0127] Therefore, the polymerization temperature conditions for polymerizing (meth)acrylamide monomers (a) are preferably 35°C to 90°C, more preferably 40°C to 80°C, and even more preferably 40°C to 70°C.

[0128] In a dispersion (E) comprising (meth)acrylamide monomer (a), inorganic material (B), polymerization initiator (D), and aqueous medium (C), the polymerization method for (meth)acrylamide monomer (a) is not particularly limited and can be a polymerization method based on heating or a polymerization method based on energy ray irradiation (e.g., ultraviolet irradiation).

[0129] However, from the viewpoint that larger organic-inorganic composite particles (X) can be obtained, heating-based polymerization is preferred.

[0130] Examples of polymerization methods using the aforementioned photopolymerization initiator include irradiation with high-energy rays, such as electron beams, gamma rays, X-rays, ultraviolet light, and visible light. Among these, ultraviolet light is preferred for ease of use and operation. The intensity of the irradiated ultraviolet light is preferably 10–500 mW / cm². 2 The irradiation time is usually around 0.1 seconds to 200 seconds.

[0131] In typical heated free radical polymerization, oxygen acts as a polymerization inhibitor. However, in this invention, solution preparation and energy-based irradiation polymerization do not necessarily have to be carried out in an oxygen-blocking atmosphere; these operations can be performed in an air atmosphere. Nevertheless, ultraviolet irradiation in an inert gas atmosphere can further accelerate the polymerization rate and is therefore sometimes preferred.

[0132] Whether it is a polymerization method based on heating or a polymerization method based on energy irradiation (e.g., ultraviolet irradiation), it is preferred to carry out the polymerization under an inert gas atmosphere.

[0133] As a method for manufacturing the organic-inorganic complex dispersion of the present invention, for example, when (meth)acrylamide monomer (a) is polymerized by a heating-based polymerization reaction, the following manufacturing method is preferably exemplified.

[0134] For example, a method for manufacturing an organic-inorganic complex dispersion can be described as follows: when polymerizing a (meth)acrylamide monomer (a), the temperature conditions of the aqueous medium (C) are set to a temperature above the LCST (lower critical solution temperature) of the organic-inorganic complex dispersion (e.g., 45°C to 50°C), and a polymerization initiator or catalyst (e.g., potassium persulfate (KSP), or potassium persulfate (KSP) and N,N,N',N'-tetramethylethylenediamine (TEMED)) is used to polymerize the (meth)acrylamide monomer (a) through a heating-based polymerization reaction.

[0135] As a further preferred embodiment, for example, a method for manufacturing an organic-inorganic composite dispersion can be described as follows: After stirring and mixing (meth)acrylamide monomer (a) and pure water (C) at room temperature, an inorganic material is added. Under a nitrogen atmosphere, the inorganic material is dispersed in a mixed solution heated to 50°C. Next, potassium persulfate (KSP) and N,N,N',N'-tetramethylethylenediamine (TEMED) are added. Then, under a nitrogen atmosphere, the (meth)acrylamide monomer (a) is reacted in the mixed solution at 50°C for 0.5 to 3 hours to form a polymer (P). Thus, an organic-inorganic composite dispersion in which organic-inorganic composite particles (X) formed by the polymer (P) and inorganic material (B) dispersing in an aqueous medium (C) can be manufactured.

[0136] As a method for manufacturing the organic-inorganic composite dispersion of the present invention, for example, when (meth)acrylamide monomer (a) is polymerized by a polymerization reaction based on ultraviolet irradiation, the following manufacturing method is preferably exemplified.

[0137] For example, a method for manufacturing an organic-inorganic complex dispersion can be described as follows: when polymerizing a (meth)acrylamide monomer (a), the temperature conditions of the aqueous medium (C) are set to a temperature above the LCST (lower critical solution temperature) of the organic-inorganic complex dispersion (e.g., 45°C to 50°C), and a photopolymerization initiator (e.g., 1-hydroxycyclohexylphenyl ketone (Irg184)) is used to polymerize the (meth)acrylamide monomer (a) through a polymerization reaction based on ultraviolet irradiation.

[0138] As a further preferred embodiment, for example, a method for manufacturing an organic-inorganic composite dispersion can be described as follows: Inorganic material (B), (meth)acrylamide monomer (a), and pure water (C) are mixed, and these components are dispersed in a mixed solution heated to 45–50°C under a nitrogen atmosphere. Next, 1-hydroxycyclohexylphenyl ketone (Irg184) dissolved in methanol is added. Then, the (meth)acrylamide monomer (a) is reacted by irradiating the mixed solution at 45–50°C with ultraviolet light for 3 minutes under a nitrogen atmosphere to form a polymer (P). This allows the production of an organic-inorganic composite dispersion in an aqueous medium (C), in which organic-inorganic composite particles (X) formed by the polymer (P) and inorganic material (B) creating a three-dimensional network.

[0139] (Utilization of organic-inorganic complex dispersions)

[0140] <Drying and Coating>

[0141] By drying the organic-inorganic composite dispersion of the present invention, a transparent dried film with good flexibility and mechanical properties can be obtained. This dried film can be attached to a support (substrate) (coating) or a separate film without a support. The thickness of the dried film can be adjusted arbitrarily according to the application. For a dry film as a separate film, a thickness of 0.01 mm to 2 mm is preferred for ease of handling. Within this range, the dried film has sufficient strength, is easy to process, and easily produces a dried film with high surface smoothness. Furthermore, the thickness of the dried film attached to a support is not particularly limited; as long as it is 0.001 μm or more, it can be appropriately processed. Considering the absence of the influence of a support, a thickness of 0.005 μm or more is preferred.

[0142] The organic-inorganic composite dispersion of the present invention can be used directly as a coating, or it can be used after a purification process such as water washing. Furthermore, in order to impart functional properties such as coatability, surface smoothness of the dried film, gloss adjustment properties, and anti-fogging properties, leveling agents or surfactants, polymer compounds, colorants, etc., can be further added to the organic-inorganic composite dispersion.

[0143] A laminate can be manufactured by coating the organic-inorganic composite dispersion of the present invention onto a support to form a dried film. When coating the support, it is also possible to coat it into a pattern of a specific shape as needed. Examples of methods for patterning the organic-inorganic composite dispersion onto the support include printing methods where the dispersion is coated onto a patterned plate and then transferred to the support; patterned coating where uncoated portions are pre-masked on the support and the masked portions are removed after coating; and dispersion coating methods based on inkjet printing.

[0144] The dried coating obtained by coating and drying the organic-inorganic composite dispersion of the present invention can be used as a cell culture medium, temperature-sensitive membrane, etc., according to its temperature response characteristics.

[0145] <Cell Culture Materials>

[0146] After the organic-inorganic composite dispersion of the present invention is coated onto a support (e.g., a polystyrene container) and dried, and then washed as needed, it is dried while still attached to the support, thereby enabling its use as a cell culture medium with good cell adhesion and proliferation. Furthermore, by selecting the polymer (P), it can also be used as a culture medium in which cells can be cultured in a floating state without adhering to the culture surface (low cell adhesion).

[0147] The shape of the cell culture medium of the present invention is not particularly limited as long as it can culture cells and the cultured cells can be easily detached through low-temperature treatment. Examples include membrane-like, dish-like, bottle-like, tubular, linear or rod-like with a diameter of 5 nm to 5 mm, bag-like, porous plate-like, microfluidic, porous membrane-like or mesh-like (e.g., Transwell, CellStrainer), and spherical with a particle size preferably of 10 to 2,000 μm, more preferably 100 to 500 μm.

[0148] The cell culture medium of the present invention can be used as a single unit, but is preferably used as a cell culture apparatus on which a substrate is formed on a support. This is because, as a cell culture apparatus, it not only offers excellent convenience in transportation and storage, but can also be directly used as a culture container or culture carrier.

[0149] The material of the support used in this invention is not particularly limited, as long as it can adequately adhere to the cell culture medium and allow cells to be cultured on the adhered cell culture medium, and the cultured cells can be easily detached through low-temperature treatment. For example, styrene-based resins such as polystyrene, polyolefin-based resins such as polypropylene, polyurethane-based resins, polycarbonate, polyethylene terephthalate (PET), polysulfone-based resins, fluorinated resins, polysaccharide-based natural polymers such as cellulose, inorganic materials such as glass and ceramics, and metallic materials such as stainless steel and titanium can be appropriately used.

[0150] The shape of the support is not particularly limited, as long as it can serve as a support for the cell culture medium of the present invention. Examples include membrane-like, plate-like, spherical, polygonal, rod-like, disc-like, bottle-like, tubular, needle / filament-like, fibrous, bag-like, porous plate-like, microfluidic, porous membrane-like, or mesh-like (e.g., Transwell, CellStrainer). It can be a combination of these shapes, or it can be an irregularly shaped support without a specific shape.

[0151] Moreover, the cell culture medium of the present invention can not only be integrated with the support and used as a cell culture device, but can also be detached from the support and used separately.

[0152] Example

[0153] The present invention will be further described in detail below with reference to embodiments, but the scope of the present invention is not limited to these embodiments.

[0154] (Example 1)

[0155] [Preparation of reaction solution (E) containing (meth)acrylamide monomer (a), water-swellable clay mineral (B), photopolymerization initiator (D), and aqueous medium (C)]

[0156] 1.13 g of N-isopropylacrylamide (NIPAM) (manufactured by Kohjin Co., Ltd.) as a (meth)acrylamide monomer (a), 0.08 g of Laponite XLG (manufactured by Rockwood Additives Ltd.) as a clay mineral (B), and 40 g of ultrapure water as an aqueous medium (C) were mixed and heated to 45–50 °C under a nitrogen atmosphere.

[0157] Next, reaction solution (E1) was prepared by mixing 200 μL of Irg184 solution as a non-water-soluble photopolymerization initiator (D). The Irg184 solution refers to a methanol solution with a concentration of 2% by mass of Irg184.

[0158] [Preparation of a dispersion of organic-inorganic complex X]

[0159] Under a nitrogen atmosphere, the above reaction solution (E1) heated to 45°C was stirred with a magnetic stirrer while being irradiated with ultraviolet light at a intensity of 40 mW / cm at 365 nm. 2 The (meth)acrylamide monomer (a) was subjected to ultraviolet light for 3 minutes to induce polymerization, and a slightly turbid organic-inorganic complex dispersion (1) of organic-inorganic complex X was prepared (hereinafter also referred to as dispersion (1)).

[0160] The concentrations of Ra and inorganic material (B) in the reaction system are as follows.

[0161] Ra = 0.07, the concentration (mass%) of inorganic material (B) = 0.20 (%) < 12.4Ra + 0.05 = 0.92

[0162] The container with the above dispersion (1) was placed in a water bath, and the temperature of the water bath was increased from room temperature at a rate of 10°C / 60 minutes. The LCST of the dispersion (1) was measured.

[0163] When the above dispersion (1) was manufactured, the reaction conversion rate of (meth)acrylamide monomer (a) was 97%.

[0164] The residual monomer content is quantified by HPLC, and the reaction conversion rate is calculated based on the amount of feed.

[0165] Regarding the above dispersion (1), the particle size of the organic-inorganic composite particles was measured using a dynamic light scattering particle size distribution measuring device (e.g., HORIBA, Ltd. LB-550 dynamic light scattering particle size distribution measuring device), and the average particle size was 132 nm. Using the organic-inorganic composite dispersion (1) obtained in Example 1, the organic-inorganic composite dispersion was cast on a PP tray of approximately 15 cm × 20 cm until the thickness reached 50 μm. After drying at room temperature, it was dried at 130 °C for 1 hour, thereby obtaining a dried coating film.

[0166] Approximately 0.2 g of a dried coating was obtained by wrapping it with a 200-mesh stainless steel mesh. The coating was dried at 130°C for 2 hours, and its weight was measured. Afterward, the coating, along with the mesh, was placed in water at approximately 23°C for 20 hours. It was then removed and dried in a hot air dryer at 130°C for 2 hours, and its weight was measured again. Based on the measured weights, the weight loss rate before and after standing in water was determined. This value was taken as the gel fraction (%).

[0167] As a result, the gel fraction of the dried culture medium coated with the organic-inorganic complex dispersion (1) was 93%.

[0168] The evaluation results of the organic-inorganic complex dispersion (1) of Example 1 are shown in Table 1 below.

[0169] (Examples 2-3)

[0170] In Example 1, the content of water-swellable clay mineral (B) was changed to that shown in Table 1 below. Otherwise, reaction solutions (E2) to (E3) were prepared using the same method as in Example 1.

[0171] The concentrations of Ra and inorganic material (B) in the reaction system of the reaction solution (E2) are as follows.

[0172] Ra = 0.14, the concentration (mass%) of inorganic material (B) = 0.40 (%) < 12.4Ra + 0.05 = 1.79

[0173] The concentrations of Ra and inorganic material (B) in the reaction system of the reaction solution (E3) are as follows.

[0174] Ra = 0.28, the concentration (mass%) of inorganic material (B) = 0.80 (%) < 12.4Ra + 0.05 = 3.52

[0175] The evaluation results of the organic-inorganic complex dispersions (2) to (3) of Examples 2 to 3 are shown in Table 1 below.

[0176] (Example 4)

[0177] [Preparation of reaction solution (E) containing (meth)acrylamide monomer (a), water-swellable clay mineral (B), polymerization initiator (D), and aqueous medium (C)]

[0178] 1.13 g of N-isopropylacrylamide (manufactured by Kohjin Co., Ltd.) as a (meth)acrylamide monomer (a) and 40 g of pure water as an aqueous medium (C) were mixed and stirred at room temperature. Next, 0.16 g of Laponite XLG (manufactured by Rockwood Additives Ltd.) was mixed as a clay mineral (B), and these components were heated to 50°C and stirred for 10 minutes under a nitrogen atmosphere.

[0179] Next, as the polymerization initiator (D), 0.82 mL of potassium persulfate (KPS) solution was mixed to prepare the reaction solution (E4). Here, KPS solution refers to an aqueous solution with a KPS concentration of 2% by mass.

[0180] [Preparation of a dispersion of organic-inorganic complex X]

[0181] The above reaction solution (E4) was heated to 70°C under a nitrogen atmosphere and stirred with a magnetic stirrer while the (meth)acrylamide monomer (a) was polymerized for 0.5 hours to prepare a slightly turbid organic-inorganic complex dispersion (4) of organic-inorganic complex X.

[0182] The evaluation results of the organic-inorganic complex dispersion (4) of Example 4 are shown in Table 1 below.

[0183] (Example 5)

[0184] [Preparation of reaction solution (E) containing (meth)acrylamide monomer (a), water-swellable clay mineral (B), polymerization initiator (D), and aqueous medium (C)]

[0185] 1.13 g of N-isopropylacrylamide (manufactured by Kohjin Co., Ltd.) as a (meth)acrylamide monomer (a) and 40 g of pure water as an aqueous medium (C) were mixed and stirred at room temperature. Next, 0.08 g of Laponite XLG (manufactured by Rockwood Additives Ltd.) was mixed as a clay mineral (B), and these components were heated to 50°C and stirred for 10 minutes under a nitrogen atmosphere.

[0186] Next, 0.41 mL of potassium persulfate (KPS) solution as polymerization initiator (D) and 0.5 mL of N,N,N',N'-tetramethylethylenediamine (TEMED) solution as catalyst were mixed to prepare reaction solution (E5). Here, KPS solution refers to an aqueous solution with a KPS concentration of 2% by mass, and TEMED solution refers to an aqueous solution with a TEMED concentration of 2% by mass.

[0187] [Preparation of a dispersion of organic-inorganic complex X]

[0188] The above reaction solution (E5) was heated to 50°C under a nitrogen atmosphere, and the (meth)acrylamide monomer (a) was polymerized for 1 hour while being stirred with a magnetic stirrer, thus producing a slightly turbid organic-inorganic complex dispersion (5) of organic-inorganic complex X.

[0189] The evaluation results of the organic-inorganic complex dispersion (5) of Example 5 are shown in Table 1 below.

[0190] (Examples 6-7)

[0191] In Example 5, the content of water-swellable clay mineral (B) was changed to that shown in Table 1 below. Otherwise, reaction solutions (E6) to (E7) were prepared using the same method as in Example 5.

[0192] The evaluation results of the organic-inorganic complex dispersions (6) to (7) of Examples 6 and 7 are shown in Table 1 below.

[0193] (Comparative Example 1)

[0194] In Example 1, the contents of each component and the heating temperature of the reaction solution under polymerization conditions were changed to those recorded in Table 1 below. Otherwise, the reaction solutions (Comparative E1 to Comparative E4) were prepared in the same manner as in Example 1.

[0195] The evaluation results of the organic-inorganic complex dispersions of Comparative Examples 1 to 4 (Comparative Examples 1 to 4) are shown in Table 1 below.

[0196]

[0197] Based on the above examples and comparative examples, it is known that when (meth)acrylamide monomer (a) is polymerized, if the polymerization reaction is carried out at a high temperature, organic-inorganic composite particles (X) with a large particle size of 100 nm or more can be obtained. Furthermore, it is known that by coating a dispersion of the organic-inorganic composite containing these large-particle-size organic-inorganic composite particles (X) into a film and then drying it, a dried film exhibits a high gel fraction and excellent film-forming properties and water resistance.

[0198] Furthermore, organic-inorganic composite particles (X) with a particle size of 300 nm or larger can be obtained by thermal polymerization. From the viewpoint of obtaining organic-inorganic composite particles (X) with a larger particle size, thermal polymerization is preferred over UV polymerization.

[0199] Therefore, according to the present invention, it is possible to provide an organic-inorganic composite dispersion for forming a dry coating suitable for cell culture media, etc., and capable of forming a dry coating exhibiting good film-forming properties and water resistance.

Claims

1. A method for producing an organic-inorganic composite dispersion, wherein: In the organic-inorganic composite dispersion, the organic-inorganic composite particles (X) are dispersed in the aqueous medium (C). The method for preparing the organic-inorganic composite dispersion comprises: A step of mixing a (meth)acrylamide monomer (a), one or more inorganic materials (B) selected from water-swellable clay minerals and silica, a polymerization initiator (D) and an aqueous medium (C), and then polymerizing the (meth)acrylamide monomer (a) to form organic-inorganic composite particles (X); The concentration of the at least one inorganic material (B) selected from water-swellable clay minerals and silica in the aqueous medium (C) is within the range represented by the following formula (1) or (2), When polymerizing the (meth)acrylamide monomer (a), the temperature condition of the aqueous medium (C) is set to be 45° C. to 55° C. or higher than the LCST (lower critical solution temperature) of the organic-inorganic composite dispersion, and potassium persulfate and N,N,N',N'-tetramethylethylenediamine are used as polymerization initiators or catalysts to polymerize the (meth)acrylamide monomer (a) by a polymerization reaction based on heating. Formula (1) When Ra<0.19, The concentration of inorganic material (B) is less than 12.4Ra+0.05, When Ra≥0.19 in formula (2), The concentration of inorganic material (B) is less than 0.87Ra+2.17, In the formula, the concentration of the inorganic material (B) is the value obtained by dividing the mass of the inorganic material (B) by the total mass of the aqueous medium (C) and the inorganic material (B) and multiplying the result by 100, Ra is the mass ratio of the inorganic material (B) to the polymer (P) ((B) / (P)), The unit of the concentration is mass %.

2. The method for producing an organic-inorganic composite dispersion according to claim 1, wherein: The temperature of the aqueous medium (C) is 10° C. or higher than the LCST of the organic-inorganic composite dispersion.

Citation Information

Patent Citations

  • Organic inorganic composite dispersion and process for producing the same

    JP2011144236A

  • Organic and inorganic composite hydrogel and its producing method

    JP2002053762A

  • Inorganic-particles-containing water-soluble polymer dispersion, its production method, and its use

    JP2003096113A

  • Polymer gel composition and optical element, resin composition and optical film using the same

    JP2005060448A

  • Cell culture substrate and cell culture method

    JP2005110604A