High-strength steel sheet with excellent formability and method for producing the same
By rationally selecting the element composition and heat treatment process in high-strength steel, controlling the microstructure of ferrite and martensite, the problem of poor formability of high-strength steel in stamping is solved, and high strength, high ductility and low Cost of steel plate manufacturing.
Patent Information
- Application Number
- CN202180043856.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-06-17
- Filing Date
- 2021-06-16
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-06-16
AI Technical Summary
Existing high-strength steels are prone to cracks and poor formability during the stamping process, making it difficult to achieve both high strength and high ductility, resulting in processing defects and increased costs.
It is composed of alloys of carbon, silicon, manganese, titanium, niobium, molybdenum, phosphorus, sulfur and other elements. Through specific heat treatment processes, including heating, hot finishing rolling, winding, cold rolling and continuous annealing, the ferrite and martensite are controlled. The fine structure of silica ensures the low yield ratio and high ductility of the steel plate.
It achieves excellent formability of high-strength steel plates, reduces cracks and wrinkle defects in stamping forming, is suitable for use in complex-shaped automotive structural parts, and improves processing quality and economy.
Smart Images

Figure CN116034176B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a steel suitable for an automobile material, and more particularly to a high-strength steel sheet having excellent formability and a method for manufacturing the same. Background Art
[0002] In recent years, due to various environmental regulations and energy use regulations, the use of high-strength steel is required to improve fuel efficiency or durability.
[0003] In particular, as the impact stability regulations of automobiles are expanded, high-strength steel with excellent strength is applied as a material for structural parts such as frame members, seat rails, and pillars for improving the impact resistance of the vehicle body. Such automobile parts have complex shapes for safety and design, and are mainly formed and manufactured using stamping dies, so high strength and a high level of formability are required.
[0004] However, the higher the strength of steel, the better it is at absorbing impact energy. However, as the strength increases, the elongation decreases, which leads to a problem of reduced formability. In addition, when the yield strength is too high, less material is introduced into the mold during forming, resulting in poor formability.
[0005] In addition, representative high-strength steels used as automotive materials include dual phase steel (DP steel), transformation induced plasticity steel (TRIP steel), complex phase steel (CP steel), ferrite bainite steel (FB steel), etc.
[0006] DP steel, as an ultra-high tensile steel, has a low yield strength ratio of about 0.5 to 0.6, so it is easy to process and has the advantage of high elongation second only to TRIP steel. Therefore, it is mainly used in outer doors, seat rails, seat belts, suspensions, arms, wheel discs, etc.
[0007] TRIP steel has a yield ratio in the range of 0.57 to 0.67, and thus has excellent formability (high ductility), and is therefore suitable for parts requiring high formability, such as frames, roofs, seat belts, and bumpers.
[0008] CP steel has a low yield strength ratio, high elongation and bending workability, so it is used in side panels, underbody reinforcements, etc., and FB steel has excellent hole expandability, so it is mainly used in suspension lower arms or wheel discs, etc.
[0009] Among them, DP steel is mainly composed of ferrite with excellent ductility and martensite with high strength, and there may be a trace of retained austenite. This DP steel has low yield strength and high tensile strength, thus having excellent properties such as low yield ratio (YR), high work hardening rate, high ductility, continuous yield behavior, room temperature aging resistance, and bake hardenability.
[0010] However, in order to ensure ultra-high tensile strength of 980 MPa or more, the fraction of hard phases such as martensite phases that contribute to improving strength needs to be increased. In this case, the yield strength increases, so there is a problem of defects such as cracks occurring during stamping.
[0011] Generally, DP steel for automobiles is manufactured by making slabs through steelmaking and continuous casting processes, and then subjecting the slabs to [heating-rough rolling-hot finishing rolling] to obtain hot-rolled coils, which are then annealed to produce the final product.
[0012] Among them, the annealing process is mainly a process carried out when manufacturing cold-rolled steel sheets. The cold-rolled steel sheets are manufactured as follows: the hot-rolled coils are pickled to remove the surface oxide scale, and cold-rolled at a specified reduction rate at room temperature, and then annealed and further flattened as needed.
[0013] The cold-rolled steel sheet (cold-rolled material) obtained by cold rolling is in a very hardened state and is not suitable for making parts that require workability. Therefore, the workability can be improved by softening it through heat treatment in a continuous annealing furnace as a subsequent process.
[0014] As an example, the annealing process is to heat a steel plate (cold rolled material) to about 650-850° C. in a heating furnace and then hold the steel plate for a certain period of time, thereby reducing hardness and improving workability through recrystallization and phase transformation phenomena.
[0015] The steel sheet that has not been annealed has high hardness, especially surface hardness, and insufficient workability. However, the steel sheet that has been annealed has a recrystallized structure, so that the hardness, yield point, and tensile strength are reduced, which can help improve the workability.
[0016] As a typical method for reducing the yield strength of DP steel, it is advantageous to make ferrite coarse in size and to make austenite fine and uniform in size during continuous annealing.
[0017] like Figure 1As shown, the continuous annealing process is carried out through the [heating zone-soaking zone-slow cooling zone-rapid cooling zone-overaging zone] in the annealing furnace. At this time, a fine ferrite phase is formed by sufficient recrystallization in the heating zone, and then a fine and uniform austenite phase is formed from the fine ferrite phase in the soaking zone. Then, during the cooling process, austenite forms fine bainite and martensite phases while the ferrite phase is recrystallized.
[0018] As a prior art for improving the workability of high-strength steel, Patent Document 1 proposes a method based on microstructure refinement, specifically, a method for dispersing fine precipitated copper particles with a particle size of 1-100 nm in the microstructure of a dual-phase steel plate mainly composed of a martensite phase. However, this technology requires the addition of 2-5% Cu to obtain good fine precipitated phase particles, so red hot brittleness caused by a large amount of Cu as described above may occur, and there is a problem of excessive increase in manufacturing costs.
[0019] Patent document 2 discloses a high-strength steel plate, which has a ferrite matrix structure and a structure containing 2-10% pearlite, and precipitation strengthening and grain refinement are achieved by adding carbonitride-forming elements (e.g., Ti, etc.). In the case of this technology, although it has the advantage of being easy to achieve high strength relative to low manufacturing costs, the recrystallization temperature rises sharply due to fine precipitation. Therefore, in order to ensure high ductility caused by sufficient recrystallization, it is known that heating at a relatively high temperature is required during continuous annealing. In addition, the existing precipitation-strengthened steel that strengthens the steel by precipitating carbonitrides on the ferrite matrix has limitations in obtaining high strengths of more than 600 MPa.
[0020] In addition, Patent Document 3 discloses the following technology: a steel material containing 0.18% or more carbon is continuously annealed and water-cooled to room temperature, and then aged at 120-300°C for 1-15 minutes to ensure a volume fraction of 80-97% martensite. Although this technology is beneficial for improving yield strength, the shape quality of the coil is deteriorated due to temperature deviations in the width and length directions of the steel plate during water cooling, so there are problems such as material defects in some parts and reduced operability during roll forming and other processing.
[0021] In view of the above-mentioned prior art, in order to improve the formability of high-strength steel, it is necessary to develop a method that can reduce the yield strength but increase the ductility.
[0022] (Patent Document 1) Japanese Patent Publication No. 2005-264176
[0023] (Patent Document 2) Korean Patent Publication No. 2015-0073844
[0024] (Patent Document 3) Japanese Patent Publication No. 1992-289120 Summary of the invention
[0025] Technical issues to be solved
[0026] One aspect of the present invention provides a high-strength steel sheet which has a low yield ratio and high strength and has excellent formability due to improved ductility, and a method for producing the same, as a material suitable for automobile structural parts and the like.
[0027] The technical problem of the present invention is not limited to the above content. The technical problem of the present invention can be understood from the overall content of this specification, and those skilled in the art of the present invention can easily understand the additional technical problem of the present invention.
[0028] Technical Solution
[0029] One aspect of the present invention provides a high-strength steel sheet having excellent formability, the steel sheet comprising, in weight percent, carbon (C): 0.05-0.15%, silicon (Si): 0.5% or less (except 0%), manganese (Mn): 2.0-3.0%, titanium (Ti): 0.2% or less (except 0%), niobium (Nb): 0.1% or less (except 0%), vanadium (V): 0.2% or less (except 0%), molybdenum (Mo): 0.5% or less (except 0%), phosphorus (P): 0.1% or less, sulfur (S): 0.01% or less, and the remainder Fe and unavoidable impurities,
[0030] The microstructure is composed of ferrite with an area fraction of 20-45%, and the remainder of martensite and bainite, wherein the unrecrystallized ferrite in the ferrite is present at a fraction of less than 25 area%, and the average aspect ratio (long diameter: short diameter) is 1.1 to 2:1.
[0031] Another aspect of the present invention provides a method for manufacturing a high-strength steel plate with excellent formability, characterized in that it includes the following steps: heating a steel billet having the above-mentioned alloy composition; hot finish rolling the heated steel billet at an outlet side temperature of Ar3 or more and 1000°C or less to manufacture a hot-rolled steel plate; coiling the hot-rolled steel plate within a temperature range of 400-700°C; cooling to room temperature after coiling; cold rolling at a reduction rate of 40-70% after cooling to manufacture a cold-rolled steel plate; continuously annealing the cold-rolled steel plate; after the continuous annealing, primary cooling is performed to cool to a temperature range of 650-700°C; and after the primary cooling, secondary cooling is performed to cool to a temperature range of 300-580°C.
[0032] The continuous annealing step is performed in a device provided with a heating zone, a soaking zone and a cooling zone, and the end temperature of the heating zone is higher than the end temperature of the soaking zone by more than 10°C.
[0033] Beneficial Effects
[0034] According to the present invention, it is possible to provide a steel sheet having high strength and improved formability by ensuring a low yield ratio and high ductility.
[0035] As described above, the steel sheet of the present invention having improved formability can prevent processing defects such as cracks and wrinkles during press forming, and thus has the effect of being suitable for use in parts for structures and the like that need to be processed into complex shapes. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a schematic diagram of the heat treatment of the conventional continuous annealing process (CAL).
[0037] Figure 2 is a schematic diagram of a continuous annealing process (CAL) according to one aspect of the present invention, and Figure 1 The graph of (grey line) is shown together.
[0038] Figure 3 A microstructure photograph of a comparative example according to one embodiment of the present invention is shown.
[0039] Figure 4 A microstructure photograph of an inventive example according to one embodiment of the present invention is shown.
[0040] Figure 5 Schematic diagram showing the aspect ratio of ferrite grains according to one embodiment of the present invention.
[0041] Best Mode for Carrying Out the Invention
[0042] The inventors of the present invention have conducted intensive studies to develop a material having a moldability at a level suitable for use in parts that need to be processed into a complex shape among automotive materials.
[0043] In particular, the present inventors have confirmed that the goal can be achieved by inducing sufficient recrystallization of the soft phase that affects the ductility of steel and ensuring the refinement and distribution of the hard phase that contributes to ensuring strength, thereby completing the present invention.
[0044] Hereinafter, the present invention will be described in detail.
[0045] A high-strength steel sheet with excellent formability according to one aspect of the present invention may contain, in terms of weight%, carbon (C): 0.05-0.15%, silicon (Si): 0.5% or less (except 0%), manganese (Mn): 2.0-3.0%, titanium (Ti): 0.2% or less (except 0%), niobium (Nb): 0.1% or less (except 0%), vanadium (V): 0.2% or less (except 0%), molybdenum (Mo): 0.5% or less (except 0%), phosphorus (P): 0.1% or less, and sulfur (S): 0.01% or less.
[0046] Hereinafter, the reasons for limiting the alloy composition of the steel sheet provided in the present invention as described above will be described in detail.
[0047] In addition, unless otherwise specified, the content of each element in the present invention is based on weight, and the proportion of the structure is based on area.
[0048] Carbon (C): 0.05-0.15%
[0049] Carbon (C) is an important element added for solid solution strengthening. This C combines with precipitation elements to form fine precipitates, thereby contributing to improving the strength of steel.
[0050] When the C content exceeds 0.15%, the hardenability increases, and since martensite is formed during the cooling process when manufacturing the steel, the strength increases excessively, and there is also a problem of causing a decrease in elongation. In addition, due to poor weldability, there is a possibility of welding defects when processing into parts. In addition, when the C content is less than 0.05%, it is difficult to ensure the target level of strength.
[0051] Therefore, the C content may be 0.05-0.15%. More preferably, the C content may be 0.06% or more and 0.13% or less.
[0052] Silicon (Si): 0.5% or less (except 0%)
[0053] Silicon (Si) is a ferrite stabilizing element and helps to ensure the target level of ferrite fraction by promoting ferrite transformation. In addition, due to its excellent solid solution strengthening ability, it is effective in improving the strength of ferrite and is an element that effectively ensures strength without reducing the ductility of steel.
[0054] When the Si content exceeds 0.5%, the solid solution strengthening effect is excessive, which in turn reduces ductility and causes surface scale defects, thereby adversely affecting the quality of the plated surface. In addition, there is a problem of hindering chemical treatability.
[0055] Therefore, the content of Si may be 0.5% or less, and 0% may be excluded. The content of Si may more preferably be 0.1% or more.
[0056] Manganese (Mn): 2.0-3.0%
[0057] Manganese (Mn) is an element that precipitates sulfur (S) in steel as MnS, thereby preventing hot brittleness due to the formation of FeS and contributing to solid solution strengthening of steel.
[0058] When the content of such Mn is less than 2.0%, not only the above-mentioned effects cannot be obtained, but also it is difficult to ensure the strength at the target level. On the other hand, when the content of Mn exceeds 3.0%, the possibility of problems such as weldability and hot rolling is high, and martensite is more likely to be formed due to the increase in hardenability, so ductility may be reduced. In addition, too many Mn bands (Bands) (Mn oxide bands) are formed in the structure, so there is a problem of increased risk of defects such as processing cracks. In addition, Mn oxides are dissolved from the surface during annealing, so there is a problem of greatly hindering the plating property.
[0059] Therefore, the Mn content may be 2.0-3.0%, and more preferably may be 2.2-2.8%.
[0060] Titanium (Ti): 0.2% or less (except 0%)
[0061] Titanium (Ti) is an element that forms fine carbides and helps to ensure yield strength and tensile strength. In addition, Ti precipitates N in steel as TiN, thereby having the effect of suppressing the formation of AlN caused by Al that inevitably exists in steel, and thus has the effect of reducing the possibility of cracking during continuous casting.
[0062] When the content of Ti exceeds 0.2%, coarse carbides are precipitated, and the strength and elongation may be reduced due to the reduction of the carbon content in the steel. In addition, there is a possibility of causing nozzle clogging during continuous casting. Therefore, the content of Ti may be 0.2% or less, and 0% is excluded.
[0063] Niobium (Nb): 0.1% or less (except 0%)
[0064] Niobium (Nb) is an element that segregates at austenite grain boundaries to suppress the coarsening of austenite grains during annealing heat treatment and forms fine carbides to contribute to improving strength.
[0065] When the Nb content exceeds 0.1%, coarse carbides are precipitated, and strength and elongation may be poor due to the reduction of carbon content in steel, and there is a problem of increased manufacturing cost. Therefore, the Nb content may be 0.1% or less, and 0% is excluded.
[0066] Vanadium (V): 0.2% or less (except 0%)
[0067] Vanadium (V) is an element that reacts with carbon or nitrogen to form carbonitrides, and is an important element that forms fine precipitates at low temperatures to increase the yield strength of steel.
[0068] When the V content exceeds 0.2%, coarse carbides are precipitated, and strength and elongation may be poor due to the reduction of carbon content in steel, and there is a problem of increased manufacturing cost. Therefore, the V content may be 0.2% or less, and 0% is excluded.
[0069] Molybdenum (Mo): 0.5% or less (except 0%)
[0070] Molybdenum (Mo) is an element that forms carbides in steel, and when added in combination with carbonitride-forming elements such as Ti, Nb, and V, it maintains the size of fine precipitates, thereby helping to improve the yield strength and tensile strength of steel. In addition, Mo delays the transformation of austenite into pearlite while having the effect of refining ferrite and improving strength. This Mo forms martensite finely at the grain boundary by improving the hardenability of steel, and therefore has the advantage of being able to control the yield ratio. However, the Mo is an expensive element, and as its content increases, the manufacturing cost increases, which is disadvantageous to the economy, so it is preferred to appropriately control its content.
[0071] In order to fully obtain the above effects, up to 0.5% Mo can be added. When the Mo content exceeds 0.5%, the alloy cost increases sharply, thereby reducing economic efficiency, and due to excessive grain refinement and solid solution strengthening effects, there is a problem of reducing the ductility of steel.
[0072] Therefore, the Mo content may be 0.5% or less, except for 0%.
[0073] Phosphorus (P): 0.1% or less
[0074] Phosphorus (P) is a substitutional element with the greatest solid solution strengthening effect, and is an element that improves in-plane anisotropy without significantly reducing formability while ensuring strength. However, when too much P is added, the possibility of brittle failure increases significantly, resulting in an increased possibility of plate breakage during hot rolling, and there is a problem of hindering the surface properties of the plated surface.
[0075] Therefore, in the present invention, the P content may be controlled to be less than 0.1%, except for 0% in consideration of the level that is inevitably added.
[0076] Sulfur (S): 0.01% or less
[0077] Sulfur (S) is an impurity element in steel and is an element that is inevitably added. Since it hinders ductility, it is preferable to control the sulfur content to a minimum. In particular, S has the problem of increasing the possibility of red-hot brittleness, so it is preferable to control the sulfur content to 0.01% or less. However, considering the level that is inevitably added during the manufacturing process, 0% may be excluded.
[0078] The remaining component of the present invention is iron (Fe). However, undesirable impurities may inevitably be mixed from the raw materials or the surrounding environment during the conventional manufacturing process, so this impurity cannot be excluded. These impurities are well known to technicians in the conventional manufacturing process, so all of them are not specifically described in this specification.
[0079] The steel sheet of the present invention having the above alloy composition has a fine structure composed of ferrite and a martensite phase and a bainite phase as hard phases. In this case, the area fraction of the ferrite may be 20-45%, and the rest of the structure may be a hard phase.
[0080] When the ferrite phase fraction is less than 20%, the ductility of the steel cannot be sufficiently ensured, and the formability deteriorates. On the other hand, when the ferrite phase fraction exceeds 45%, the hard phase fraction becomes relatively low, and the target level of strength and formability cannot be ensured.
[0081] The steel sheet of the present invention including the ferrite phase in the above-mentioned fraction range preferably contains unrecrystallized ferrite in the ferrite at a fraction of 25 area % or less and has an average aspect ratio of 1.1 to 2:1.
[0082] When the fraction of the non-recrystallized ferrite exceeds 25 area %, ductility decreases and it becomes difficult to ensure a target level of formability.
[0083] In addition, even if the non-recrystallized ferrite fraction is present at 25 area % or less, when the average aspect ratio exceeds 2 (long axis: short axis = more than 2:1), there is a problem that local deformation and stress are concentrated on the non-recrystallized ferrite stretched as described above, resulting in poor ductility. Although there is no need to particularly limit the lower limit of the average aspect ratio of the non-recrystallized ferrite, the lower limit of the average aspect ratio can be set to 1.1 or more in consideration of the shape of the non-recrystallized ferrite caused by processing.
[0084] In the present invention, the fraction of non-recrystallized ferrite is expressed based on the above-mentioned ferrite fraction, not on the total microstructure fraction of the steel plate.
[0085] The aspect ratio refers to the ratio of the longitudinal direction (long diameter) to the transverse direction (short diameter) of the crystal grain size relative to the rolling direction (long diameter: short diameter). For example, Figure 5 shown. Figure 5 (a) is a schematic diagram showing the crystal grain size of recrystallized ferrite, Figure 5 (b) is a schematic diagram showing the crystal grain size of non-recrystallized ferrite. In addition, in the present invention, the aspect ratio value refers to the average aspect ratio value of the non-recrystallized ferrite grains.
[0086] In addition, with regard to the martensite phase and bainite phase constituting the hard phase, although there is no specific limitation on their respective fractions, in order to ensure ultra-high strength of a tensile strength of 980 MPa or more, the martensite phase may be included in the total microstructure fraction at a fraction of 10 area % or less (except 0%).
[0087] The steel plate of the present invention having the above-mentioned fine structure has a tensile strength of 980 MPa or more, a yield strength of 680 MPa or less, an elongation (total elongation) of 13% or more, and a yield ratio of 0.8 or less, and thus can have the characteristics of high strength, high ductility and low yield ratio.
[0088] Hereinafter, a method for producing a high-strength steel sheet having excellent formability according to another aspect of the present invention will be described in detail.
[0089] In short, the present invention can manufacture the desired steel plate through the process of [steel billet heating-hot rolling-coiling-cold rolling-continuous annealing], and each process is described in detail below.
[0090] [Heating of steel billet]
[0091] First, a steel billet satisfying the above-mentioned alloy composition may be prepared and then heated.
[0092] This process is carried out in order to smoothly carry out the subsequent hot rolling process and fully obtain the desired physical properties of the steel plate. In the present invention, there is no particular restriction on the conditions of this heating process, as long as it is a common condition. As an example, the heating process can be carried out in a temperature range of 1100-1300°C.
[0093] [Hot rolling]
[0094] The steel slab heated as described above may be hot rolled to produce a hot rolled steel sheet, and at this time, hot finish rolling may be performed at an outlet side temperature of Ar3 or more and 1000° C. or less.
[0095] When the outlet temperature during the hot finish rolling is lower than Ar3, the thermal deformation resistance increases sharply, and the top, tail and edge of the hot rolled coil become single-phase regions, so the in-plane anisotropy increases, which may deteriorate the formability. In addition, when the outlet temperature during the hot finish rolling exceeds 1000°C, the rolling load is relatively reduced, which is beneficial to productivity, but there is a possibility of generating thick oxide scale.
[0096] More specifically, the hot finish rolling may be performed within a temperature range of 760-940°C.
[0097] [Collect]
[0098] The hot-rolled steel sheet manufactured as described above can be rolled into a coil shape.
[0099] The coiling can be performed in the temperature range of 400-700°C. When the coiling temperature is lower than 400°C, excessive martensite or bainite is formed, causing excessive increase in the strength of the hot-rolled steel sheet, so that problems such as shape defects caused by load may occur during subsequent cold rolling. On the other hand, when the coiling temperature exceeds 700°C, there is a problem of deterioration in pickling properties due to the increase in surface oxide scale.
[0100] [cool down]
[0101] Preferably, the coiled hot-rolled steel sheet is cooled to room temperature at an average cooling rate of 0.1°C / s or less (except 0°C / s). At this time, the coiled hot-rolled steel sheet may be cooled after being transported, placed, etc., and the process before cooling is not limited thereto.
[0102] As described above, by cooling the coiled hot-rolled steel sheet at a predetermined speed, a hot-rolled steel sheet in which carbides serving as nucleation sites of austenite are finely dispersed can be obtained.
[0103] [Cold Rolling]
[0104] The hot-rolled steel sheet coiled as described above may be cold-rolled to manufacture a cold-rolled steel sheet.
[0105] At this time, the cold rolling can be performed at a cold rolling reduction rate of 40-70%. When the cold rolling reduction rate is less than 40%, the recrystallization driving force is weakened, and it is difficult to obtain good recrystallized grains. On the other hand, when the cold rolling reduction rate exceeds 70%, there is a high possibility of cracks at the edge of the steel plate, and there is a possibility that the rolling load increases sharply.
[0106] The present invention can perform pickling treatment on the hot-rolled steel plate before the cold rolling, and the pickling treatment process can be performed by a conventional method.
[0107] [Continuous annealing]
[0108] Preferably, the cold rolled steel sheet manufactured as described above is subjected to a continuous annealing process. As an example, the continuous annealing process can be performed in a continuous annealing furnace (CAL).
[0109] Generally, a continuous annealing furnace (CAL) is composed of [heating zone - soaking zone - cooling zone (slow cooling zone and rapid cooling zone) - overaging zone], and goes through the following process: a cold-rolled steel sheet is loaded into the continuous annealing furnace, then heated to a specific temperature in the heating zone, and maintained in the soaking zone for a specified time after reaching the target temperature.
[0110] In the present invention, in order to obtain recrystallized ferrite and fine martensite and bainite phases as the final fine structure, a method is established to apply sufficient heat input to the steel sheet in the heating zone consisting of [heating zone-soaking zone] during continuous annealing.
[0111] Specifically, in a conventional continuous annealing process, the final temperature of the heating zone and the temperature of the soaking zone are controlled to be the same temperature, whereas the present invention has a feature of independently controlling the temperature of the heating zone and the temperature of the soaking zone.
[0112] That is, in a conventional continuous annealing process, the starting temperature and the ending temperature of the soaking zone are controlled to be the same temperature, which means that the ending temperature of the heating zone and the starting temperature of the soaking zone are the same.
[0113] In contrast, the present invention can further promote the recrystallization of ferrite in the heating zone by controlling the temperature of the heating zone to be higher than the temperature of the soaking zone, thereby inducing the formation of fine ferrite, so that the austenite formed at the ferrite grain boundary can also be formed finely and uniformly.
[0114] Preferably, in the present invention, the termination temperature of the heating zone is controlled to be 10° C. or higher than the termination temperature of the soaking zone, and more preferably, the following relationship can be satisfied.
[0115] [Relational formula]
[0116] 10≤End temperature of heating zone - End temperature of soaking zone (℃)≤40
[0117] That is, the present invention controls the termination temperature of the heating zone to be higher than the termination temperature of the soaking zone, but when the temperature difference is lower than 10°C, the recrystallization of ferrite is delayed, so it is difficult to obtain a fine and uniform austenite phase. On the other hand, when the temperature difference exceeds 40°C, the subsequent cooling process cannot be fully carried out due to the excessive temperature difference, so there is a possibility of forming a coarse martensite phase or a coarse bainite phase in the final structure.
[0118] In the present invention, the termination temperature of the heating zone can be 790-830°C. When the termination temperature of the heating zone is lower than 790°C, sufficient heat input for recrystallization cannot be applied. On the other hand, when the termination temperature of the heating zone exceeds 830°C, productivity decreases and excessive austenite phase is formed, so that the fraction of hard phase after subsequent cooling is greatly increased, and there is a possibility that the ductility of the steel will deteriorate.
[0119] In addition, the end temperature of the soaking zone may be 760-790°C. When the end temperature of the soaking zone is lower than 760°C, excessive cooling is required at the end temperature of the heating zone, which is disadvantageous in economy and the heat for recrystallization may be insufficient. On the other hand, when the end temperature of the soaking zone exceeds 790°C, the fraction of austenite is too large, and the fraction of the hard phase exceeds during cooling, so there is a possibility that the formability is reduced.
[0120] In addition, in the present invention, the temperature difference between the termination temperature of the heating zone and the termination temperature of the soaking zone can be achieved by turning off the heating means from the time point when the heating zone process is completed to the time point when the soaking zone process is completed. As an example, furnace cooling treatment can be carried out in this interval.
[0121] [Stage cooling]
[0122] The desired structure is formed by cooling the cold-rolled steel sheet that has been subjected to the continuous annealing treatment as described above. In this case, it is preferable to perform cooling in steps.
[0123] In the present invention, the segmented cooling may consist of primary cooling-secondary cooling. Specifically, after the continuous annealing, primary cooling may be performed at an average cooling rate of 1-10°C / second to a temperature range of 650-700°C, and then secondary cooling may be performed at an average cooling rate of 5-50°C / second to a temperature range of 300-580°C.
[0124] At this time, the primary cooling is performed more slowly than the secondary cooling, so that defects in the sheet shape caused by a rapid temperature drop during the secondary cooling which is the subsequent relatively rapid cooling period can be suppressed.
[0125] When the final temperature during the primary cooling is lower than 650°C, the carbon diffusion activity is low due to the too low temperature, and the carbon concentration in the ferrite increases. On the other hand, since the carbon concentration in the austenite becomes low, the fraction of the hard phase is too large, and the yield ratio increases, thereby increasing the tendency of cracks to occur during processing. In addition, since the cooling speed in the soaking zone and the slow cooling zone is too fast, the shape of the plate becomes uneven.
[0126] When the end temperature exceeds 700°C, there is a disadvantage that an excessively fast cooling rate is required during the subsequent cooling (secondary cooling). In addition, when the average cooling rate during the primary cooling exceeds 10°C / second, carbon diffusion may not be fully performed. In addition, considering productivity, the primary cooling process may be performed at an average cooling rate of 1°C / second or more.
[0127] As described above, after completing the above-mentioned primary cooling, rapid cooling can be performed at a cooling rate of a certain value or higher. At this time, when the secondary cooling termination temperature is lower than 300°C, cooling deviations occur in the width and length directions of the steel plate, and there is a possibility that the plate shape may deteriorate. On the other hand, when the secondary cooling termination temperature exceeds 580°C, the hard phase cannot be fully ensured, and the strength may be reduced. In addition, when the average cooling rate during the secondary cooling is less than 5°C / second, there is a possibility that the fraction of the hard phase is too high. On the other hand, when the average cooling rate during the secondary cooling exceeds 50°C / second, there is a possibility that the hard phase is opposite and insufficient.
[0128] In addition, as required, after the staged cooling is completed, an aging treatment may be performed.
[0129] The over-aging treatment is a process of maintaining the coil for a certain period of time after the secondary cooling is terminated, and uniform heat treatment is performed along the width and length of the coil, thereby improving the shape quality. To this end, the over-aging treatment can be performed for 200-800 seconds.
[0130] The over-aging treatment temperature is lower than the secondary cooling termination temperature. As a non-limiting example, the over-aging treatment may be performed in a temperature range of 280-400°C.
[0131] The high-strength steel sheet of the present invention manufactured as described above is composed of a hard phase and a soft phase as a microstructure, and in particular, the recrystallization of ferrite is maximized through an optimized annealing process, so that a structure in which a bainite phase and a martensite phase as hard phases are uniformly distributed on a finally recrystallized ferrite matrix can be obtained.
[0132] Therefore, the steel sheet of the present invention can ensure excellent formability by ensuring a low yield ratio and high ductility even if it has a high strength of 980 MPa or more in tensile strength.
[0133] Hereinafter, the present invention will be described in more detail by way of examples. However, the description of these examples is only for illustrating the implementation of the present invention, and the present invention is not limited to the description of these examples. This is because the scope of the present invention is determined by the contents described in the claims and the contents reasonably derived therefrom. DETAILED DESCRIPTION
[0134] (Example)
[0135] Steel billets having the alloy composition shown in Table 1 below were manufactured, and then each steel billet was heated at 1200°C for 1 hour, and then hot-rolled at a finishing temperature of 880-920°C to manufacture hot-rolled steel sheets. Afterwards, each hot-rolled steel sheet was cooled at a cooling rate of 0.1°C / second and coiled at 650°C. Afterwards, the coiled hot-rolled steel sheet was cold-rolled at a reduction rate of 50% to manufacture a cold-rolled steel sheet. Under the temperature conditions shown in Table 2 below, each cold-rolled steel sheet was continuously annealed, then staged cooled (1st cooling-2nd cooling), and then aged at 360°C for 520 seconds to manufacture the final steel sheet.
[0136] At this time, the primary cooling in the step cooling was performed at an average cooling rate of 3° C. / sec, and the secondary cooling was performed at an average cooling rate of 20° C. / sec.
[0137] The microstructure of each of the steel sheets produced as described above was observed, and the mechanical properties and plating properties were evaluated, and the results are shown in Table 3 below.
[0138] At this time, the tensile test on each test piece was performed by sampling a tensile test piece of JIS No. 5 size in a direction perpendicular to the rolling direction and performing a tensile test at a strain rate of 0.01 / sec.
[0139] In addition, the unrecrystallized ferrite in the organizational phase was observed by SEM at 5000 times after nital etching. At this time, from the grain shape of the observed ferrite phase, sub grains observed in the conventional unrecrystallized ferrite or particles extending along the rolling direction were analyzed as unrecrystallized ferrite, and their fractions were measured. For the other phases, the fractions were also measured by SEM and image analyzer after nital etching.
[0140] [Table 1]
[0141]
[0142] [Table 2]
[0143]
[0144]
[0145] [Table 3]
[0146]
[0147] As shown in Tables 1 to 3, it can be confirmed that in Invention Examples 1 to 7, the steel alloy composition and manufacturing conditions, especially the continuous annealing process, all meet the conditions proposed in the present invention, and the desired fine structure is formed, so that it has high strength and excellent elongation, thereby ensuring formability.
[0148] On the other hand, in the process of manufacturing the steel sheet, the same continuous annealing process as the conventional continuous annealing process was applied, that is, the end temperature of the heating zone and the end temperature of the soaking zone were the same, but the recrystallization of ferrite was insufficient during the annealing in Comparative Examples 1 to 4 and Comparative Examples 8 to 10, and thus the desired physical properties in the present invention were not satisfied. Among them, the elongation of Comparative Examples 1 to 2 and Comparative Examples 8 to 9, which had relatively low annealing temperatures, was poor, and the yield strength of Comparative Examples 3 to 4 and Comparative Example 10, which had high annealing temperatures, exceeded the target level compared to Comparative Examples 1 to 2.
[0149] In Comparative Example 5, in which the end temperature of the heating zone during continuous annealing in the process of manufacturing the steel sheet was too high and the temperature difference from the end temperature of the soaking zone was 60°C, sufficient ferrite phase was not formed, but too much hard phase (especially bainite phase) was formed, so the elongation decreased.
[0150] The temperature difference between the end temperature of the heating zone and the end temperature of the soaking zone during continuous annealing was 20° C., but the elongation of Comparative Example 6 in which the end temperature of the soaking zone was too low was also poor.
[0151] In Comparative Example 7, the temperature of the soaking zone was higher than that of the heating zone, and thus high ductility could not be ensured.
[0152] Figure 3 The microstructure photograph of Comparative Example 2 is shown. Figure 4 A microstructure photograph of Inventive Example 2 is shown.
[0153] In Comparative Example 2, it was confirmed that an excessive amount of unrecrystallized ferrite phase was formed, whereas in Inventive Example 2, it was confirmed that a martensite phase and a bainite phase were formed on a relatively sufficient fraction of a recrystallized ferrite matrix.
Claims
1. A high-strength steel sheet having excellent formability, which comprises, in terms of weight %, excluding Fe and unavoidable impurities: carbon (C): 0.05-0.15%, silicon (Si): 0.5% or less and 0% or less, manganese (Mn): 2.0-3.0%, titanium (Ti): 0.2% or less and 0% or less, niobium (Nb): 0.1% or less and 0% or less, vanadium (V): 0.2% or less and 0% or less, molybdenum (Mo): 0.5% or less and 0% or less, phosphorus (P): 0.1% or less, sulfur (S): 0.01% or less, The microstructure is composed of ferrite with an area fraction of 20-45%, and the rest of martensite and bainite. The non-recrystallized ferrite in the ferrite is present at a fraction of 25 area % or less, and the average aspect ratio, i.e., major axis:minor axis, is 1.1 to 2:
1.
2. The high-strength steel sheet having excellent formability according to claim 1, in, The area fraction of the martensite is 10% or less, excluding 0%.
3. The high-strength steel sheet having excellent formability according to claim 1, in, The steel plate has a tensile strength of 980 MPa or more, a yield strength of 680 MPa or less, and an elongation of 13% or more.
4. The high-strength steel sheet having excellent formability according to claim 1, in, The yield strength ratio of the steel plate is less than 0.
8.
5. A method for manufacturing a high-strength steel sheet having excellent formability, It is characterized in that The following steps are involved: The steel slab is heated, and the steel plate contains, in terms of weight %, excluding Fe and inevitable impurities, carbon (C): 0.05-0.15%, silicon (Si): 0.5% or less and 0% or less, manganese (Mn): 2.0-3.0%, titanium (Ti): 0.2% or less and 0% or less, niobium (Nb): 0.1% or less and 0% or less, vanadium (V): 0.2% or less and 0% or less, molybdenum (Mo): 0.5% or less and 0% or less, phosphorus (P): 0.1% or less, sulfur (S): 0.01% or less, The heated steel slab is subjected to hot finish rolling at an outlet side temperature of Ar3 or higher and 1000° C. or lower to produce a hot rolled steel sheet; The hot rolled steel sheet is coiled at a temperature ranging from 400 to 700° C. Cooling to room temperature after winding; After cooling, cold rolling is performed at a reduction rate of 40-70% to produce a cold-rolled steel sheet; Continuously annealing the cold-rolled steel sheet; After the continuous annealing, cooling is performed once to a temperature range of 650-700° C.; and After the primary cooling, secondary cooling is performed to cool the mixture to a temperature range of 300-580°C. The continuous annealing step is carried out in a device provided with a heating zone, a soaking zone and a cooling zone, and the termination temperature of the heating zone is higher than the termination temperature of the soaking zone by more than 10°C.
6. The method for producing a high-strength steel sheet having excellent formability according to claim 5, in, The termination temperature of the heating zone and the termination temperature of the soaking zone satisfy the following relationship: 10≤the termination temperature of the heating zone-the termination temperature of the soaking zone≤40, wherein the unit of temperature is ℃.
7. The method for producing a high-strength steel sheet having excellent formability according to claim 5, in, The termination temperature of the heating zone is 790-830°C, and the termination temperature of the soaking zone is 760-790°C.
8. The method for producing a high-strength steel sheet having excellent formability according to claim 5, in, The step of heating the steel billet is carried out within a temperature range of 1100-1300°C.
9. The method for producing a high-strength steel sheet having excellent formability according to claim 5, in, The post-coiling cooling step is performed at an average cooling rate of 0.1° C. / sec or less and excluding 0° C. / sec.
10. The method for producing a high-strength steel sheet having excellent formability according to claim 5, in, The primary cooling is carried out at an average cooling rate of 1-10°C / second. The secondary cooling is performed at an average cooling rate of 5-50°C / sec.
11. The method for producing a high-strength steel sheet having excellent formability according to claim 5, in, After the secondary cooling, the step of performing an aging treatment is also included. The overaging treatment is performed for 200-800 seconds.