The high magnetic agent obtained through magnetic separation is used as raw material, and the dioxin decomposing agent is prepared by impregnation or ball milling, which solves the problems of complex catalytic cracking waste catalyst treatment process and low resource utilization rate, and achieves efficient resource utilization and economy. Improved efficiency.

CN116037609BActive Publication Date: 2024-10-15CHENGDU HUAYU ENVIRONMENTAL PROTECTION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310094674.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-10
Publication Date
2024-10-15
Estimated Expiration
2043-02-10

AI Technical Summary

Technical Problem

Existing treatment methods for spent catalytic cracking catalysts have problems such as complex treatment processes, low resource utilization, unfriendly environment and poor economic benefits, especially the inability to effectively utilize metals such as rare earths in high magnetic agents.

Method used

The low magnetic agent and the high magnetic agent are obtained through magnetic separation, and the dioxin decomposing agent is prepared by the impregnation method or the ball milling method. The transition metal and other components in the high magnetic agent are used to improve the recycling rate and economic benefits of the catalytic cracking spent catalyst.

Benefits of technology

It realizes the resource utilization of waste catalytic cracking catalyst, reduces production costs, reduces secondary pollution, and improves the comprehensive economic and social benefits of recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004071299710000031
    Figure BDA0004071299710000031
Patent Text Reader

Abstract

The present invention relates to the technical field of catalyst recycling, and provides a method for recycling catalytic cracking waste catalyst, comprising the following steps: step S1. subjecting the catalytic cracking waste catalyst to magnetic separation treatment to obtain a low magnetic agent and a high magnetic agent; step S2. using the high magnetic agent obtained in step S1 as a raw material, and adopting an impregnation method or a ball milling method to prepare a dioxin decomposer. The method for recycling catalytic cracking waste catalyst provided by the present invention uses the high magnetic agent obtained after magnetic separation of the catalytic cracking waste catalyst as a raw material, and adopts an impregnation method or a ball milling method to prepare a new dioxin decomposer, with low production cost and less secondary pollution, truly realizing the resource utilization of the catalytic cracking waste catalyst, and greatly improving the comprehensive economic and social benefits of recycling the catalytic cracking waste catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalyst recycling, and in particular to a method for recycling catalytic cracking waste catalyst. Background Art

[0002] Catalytic cracking is an important secondary processing technology for petroleum. Through catalytic cracking, heavy oil macromolecules with high boiling point and high molecular weight can be converted into high value-added products. In the process of catalytic cracking, catalysts play a pivotal role. Their application scale is large, and the annual consumption is more than hundreds of thousands of tons. Therefore, a large amount of catalytic cracking waste catalyst (FCC) is generated.

[0003] The common treatment methods for existing catalytic cracking waste catalysts are mainly the following:

[0004] The first is chemical regeneration, which has a complicated process. It cannot remove Ni, Fe, and V from the spent catalytic cracking catalyst at the same time, and it also requires the use of toxic Cl2 and H2S, which produces a lot of pollution. The activity of the regenerated catalyst is not as good as that of the new catalyst.

[0005] The second method is to use magnetic separation to reuse low-magnetic agents. Although this method is simple, only low-magnetic agents can be reused, and high-magnetic agents cannot be recycled.

[0006] Other treatment methods (such as underground burial) are equally simple, but they are not environmentally friendly and waste resources. At the same time, there are also methods of using catalytic cracking waste catalysts as ingredients for cement, asphalt, and bricks. However, such methods can only utilize the skeleton of catalytic cracking waste catalysts, and cannot reasonably utilize metals such as rare earths, and have low economic value.

[0007] In summary, it is urgent to develop a method for recycling catalytic cracking waste catalyst that is simple, has high utilization rate, is environmentally friendly, and has good economic benefits. Summary of the invention

[0008] The object of the present invention is to provide a method for recycling high magnetic agent obtained after magnetic separation of spent catalytic cracking catalyst, thereby effectively improving the recycling rate of spent catalytic cracking catalyst and the economic benefits generated by recycling spent catalytic cracking catalyst.

[0009] The purpose of the present invention is achieved through the following technical solutions:

[0010] The present invention provides a method for recycling spent catalytic cracking catalyst, comprising the following steps:

[0011] Step S1. subjecting the spent catalytic cracking catalyst to magnetic separation treatment to obtain a low magnetic agent and a high magnetic agent;

[0012] Step S2: using the high magnetic agent obtained in step S1 as a raw material, a dioxin decomposing agent is prepared by an impregnation method or a ball milling method.

[0013] In some possible embodiments, in step S2, the step of preparing the dioxin decomposition agent by the impregnation method includes:

[0014] Step S21. Take a certain amount of high magnetic agent and TiO2 powder and mix them evenly to obtain a mixture;

[0015] Step S22. Dry the mixture obtained in step S21 at 105° C. for 12 h, and weigh a certain amount of the mixture after cooling;

[0016] Step S23. dissolving a certain amount of ammonium metavanadate in oxalic acid and adding deionized water to prepare a V2O5 impregnation solution;

[0017] Step S24. Slowly pour the V2O5 impregnation solution obtained in step S23 into the mixture weighed in step S22, fully stir to form a paste, let the paste stand in an air atmosphere for 24 hours and then dry at 105°C to obtain a powder; wherein the drying time at 105°C is 12-72 hours.

[0018] Step S25: calcining the powder dried in step S24 in an air atmosphere to obtain a powdery dioxin decomposition agent.

[0019] In some possible embodiments, in step S21, the mass content of the high magnetic agent is 0.1%-90%, and the mass content of TiO2 is 0.1%-10%.

[0020] In some possible embodiments, in step S23, the molar amount of oxalic acid added is twice the molar amount of ammonium metavanadate added.

[0021] In some possible embodiments, in step S25, the calcination temperature is 200-800° C., and the calcination time is 1-48 hours.

[0022] In some possible embodiments, in step S2, the step of preparing the dioxin decomposition agent by ball milling includes:

[0023] Step S21' weigh a certain amount of high magnetic agent, V2O5 powder and TiO2 powder and mix them evenly to obtain a mixture;

[0024] Step S22'. The mixture obtained in step S21' is placed in a ball mill and ground to obtain a powder;

[0025] Step S23'. In an air atmosphere, the powder obtained in step S22' is calcined to obtain a powdered dioxin decomposer.

[0026] In some possible embodiments, in step S21', the mass fraction of the high magnetic agent is 0.1%-90%, the mass fraction of the V2O5 powder is 0.1%-10%, and the mass fraction of the TiO2 powder is 0.1%-10%.

[0027] In some possible embodiments, in step S22', there are two kinds of stainless steel balls in the ball mill, the diameters of the two kinds of stainless steel balls are 10 mm and 5 mm respectively, and the mass ratio of the two kinds of stainless steel balls is 1:1.

[0028] In some possible embodiments, in step S22', the mass ratio of the stainless steel balls in the ball mill to the mixture is 10:1-100:1, the rotation speed of the ball mill is 100-1000 rpm, and the ball milling time is 1-48 h.

[0029] In some possible embodiments, in step S23', the calcination temperature is 200-800°C, and the calcination time is 1-48h.

[0030] The technical solution of the embodiment of the present invention has at least the following advantages and beneficial effects:

[0031] The method for recycling catalytic cracking waste catalyst provided by the present invention uses the high magnetic agent obtained after magnetic separation of the catalytic cracking waste catalyst as a raw material, and adopts an impregnation method or a ball milling method to prepare a new dioxin decomposer, which has low production cost and less secondary pollution, truly realizes the resource utilization of catalytic cracking waste catalyst, and greatly improves the comprehensive economic and social benefits of recycling catalytic cracking waste catalyst. DETAILED DESCRIPTION

[0032] The present invention provides a method for recycling spent catalytic cracking catalyst, the method comprising the following steps:

[0033] Step S1. The spent catalytic cracking catalyst is subjected to magnetic separation treatment to obtain a low magnetic agent and a high magnetic agent.

[0034] It should be noted that the low magnetic agent obtained after magnetic separation of spent catalytic cracking catalyst can be directly reused as a balance agent to achieve the recovery and utilization of the low magnetic agent.

[0035] The following table 1 shows the partial metal contents in the high magnetic agent obtained after magnetic separation of catalytic cracking waste catalyst.

[0036] Table 1: Some metal contents in high magnetic agents

[0037]

[0038] According to the analysis, the high magnetic agent retains the complete skeleton and porous structure of ultrastable zeolite, and has stable physical and chemical properties. At the same time, combined with Table 1, it can be seen that the high magnetic agent contains a lot of transition metals, such as La, Ce, V, Ni, etc. Combined with the characteristics of the high magnetic agent, it is considered to use the high magnetic agent as a raw material to prepare a new dioxin decomposer.

[0039] Step S2. Using the high magnetic agent obtained in step S1 as a raw material, a new dioxin decomposer is prepared by an impregnation method or a ball milling method. The main chemical components of the dioxin decomposer include: a main active component is V2O5, the mass content of which is 0.1%-10%, a co-catalyst is TiO2, the mass content of which is 0.1%-10%, and a matrix is ​​a high magnetic agent, the mass content of which is 0.1%-90%.

[0040] A new dioxin decomposition agent for decomposing dioxins is prepared by using a high magnetic agent as a raw material, thereby realizing the recycling of the high magnetic agent and making more adequate resource utilization of the catalytic cracking waste catalyst.

[0041] It should be noted that in the actual preparation of dioxin decomposers, binders, dispersants, water retaining agents, lubricants and other additives should be appropriately added so that the prepared dioxin decomposer can have an excellent decomposition effect on dioxins at a lower temperature, thereby being suitable for industrial large-scale production.

[0042] In order to more clearly and intuitively understand the method for recycling catalytic cracking waste catalyst provided by the present invention, the process of preparing the dioxin decomposer by using the impregnation method or the ball milling method will be further described below in conjunction with specific embodiments.

[0043] Example 1

[0044] In step S2, the steps of preparing the dioxin decomposition agent by the impregnation method include:

[0045] Step S21. Take a certain amount of high magnetic agent and TiO2 powder and mix them evenly to obtain a mixture; wherein the mass content of the high magnetic agent is 90%, and the mass content of the TiO2 powder is 5%.

[0046] Step S22: Dry the mixture obtained in step S21 at 105° C. for 12 h, and weigh 95 g of the mixture after cooling.

[0047] Step S23. Dissolve 6.41 g of ammonium metavanadate in oxalic acid, and add an appropriate amount of deionized water to prepare a V2O5 impregnation solution; wherein the molar amount of oxalic acid added is about twice the molar amount of ammonium metavanadate added.

[0048] Step S24. Slowly pour the V2O5 impregnation solution obtained in step S23 into the mixture weighed in step S22, and stir thoroughly to form a paste. Let the paste stand in an air atmosphere for 24 hours and then dry it at 105°C for 24 hours to obtain a powder.

[0049] Step S25. calcining the powder dried in step S24 in an air atmosphere to obtain a powdered dioxin decomposer; wherein the calcination temperature is 400° C. and the calcination time is 9 hours.

[0050] Example 2

[0051] In step S2, the steps of preparing the dioxin decomposition agent by the impregnation method include:

[0052] Step S21. Take a certain amount of high magnetic agent and TiO2 powder and mix them evenly to obtain a mixture; wherein the mass content of the high magnetic agent is 80%, and the mass content of the TiO2 powder is 10%.

[0053] Step S22: Dry the mixture obtained in step S21 at 105° C. for 12 h, and weigh 90 g of the mixture after cooling.

[0054] Step S23. Dissolve 12.82 g of ammonium metavanadate in oxalic acid, and add an appropriate amount of deionized water to prepare a V2O5 impregnation solution; wherein the molar amount of oxalic acid added is about twice the molar amount of ammonium metavanadate added.

[0055] Step S24. Slowly pour the V2O5 impregnation solution obtained in step S23 into the mixture weighed in step S22, and stir thoroughly to form a paste. Let the paste stand in an air atmosphere for 24 hours and then dry it at 105°C for 48 hours to obtain a powder.

[0056] Step S25. calcining the powder dried in step S24 in an air atmosphere to obtain a powdered dioxin decomposer; wherein the calcination temperature is 450° C. and the calcination time is 6 hours.

[0057] Example 3

[0058] In step S2, the steps of preparing the dioxin decomposition agent by the impregnation method include:

[0059] Step S21. Take a certain amount of high magnetic agent and TiO2 powder and mix them evenly to obtain a mixture; wherein the mass content of the high magnetic agent is 80%, and the mass content of the TiO2 powder is 5%.

[0060] Step S22: Dry the mixture obtained in step S21 at 105° C. for 12 h, and weigh 85 g of the mixture after cooling.

[0061] Step S23. Dissolve 18.42 g of ammonium metavanadate in oxalic acid, and add an appropriate amount of deionized water to prepare a V2O5 impregnation solution; wherein the molar amount of oxalic acid added is about twice the molar amount of ammonium metavanadate added.

[0062] Step S24. Slowly pour the V2O5 impregnation solution obtained in step S23 into the mixture weighed in step S22, and stir thoroughly to form a paste. Let the paste stand in an air atmosphere for 24 hours and then dry it at 105°C for 72 hours to obtain a powder.

[0063] Step S25. calcining the powder dried in step S24 in an air atmosphere to obtain a powdered dioxin decomposer; wherein the calcination temperature is 600° C. and the calcination time is 3 hours.

[0064] Example 4

[0065] In step S2, the steps of preparing a dioxin decomposition agent by ball milling include:

[0066] Step S21'. Weigh 90g of high magnetic agent, 5g of V2O5 powder and 5g of TiO2 powder and mix them evenly to obtain a mixture.

[0067] Step S22'. The mixture obtained in step S21' is placed in a ball mill for grinding to obtain powder; wherein the ball mill has two kinds of stainless steel balls, the diameters of the two stainless steel balls are 10 mm and 5 mm respectively, and the mass ratio of the two stainless steel balls is 1:1, and the mass ratio of the stainless steel balls in the ball mill to the mixture is 10:1, and the rotation speed of the ball mill is controlled to be 1000 rpm, and the ball milling time is 48 hours.

[0068] Step S23'. After grinding, the powder obtained in step S22' is calcined in an air atmosphere to obtain a powdered dioxin decomposer; wherein the calcination temperature is 600°C and the calcination time is 3h.

[0069] Example 5

[0070] In step S2, the steps of preparing a dioxin decomposition agent by ball milling include:

[0071] Step S21'. Weigh 80g of high magnetic agent, 10g of V2O5 powder and 10g of TiO2 powder and mix them evenly to obtain a mixture.

[0072] Step S22'. The mixture obtained in step S21' is placed in a ball mill for grinding to obtain powder; wherein the ball mill has two kinds of stainless steel balls, the diameters of the two stainless steel balls are 10 mm and 5 mm respectively, and the mass ratio of the two stainless steel balls is 1:1, and the mass ratio of the stainless steel balls in the ball mill to the mixture is 50:1, and the rotation speed of the ball mill is controlled to be 500 rpm, and the ball milling time is 36 hours.

[0073] Step S23'. After grinding, the powder obtained in step S22' is calcined in an air atmosphere to obtain a powdered dioxin decomposer; wherein the calcination temperature is 500°C and the calcination time is 6h.

[0074] Example 6

[0075] In step S2, the steps of preparing a dioxin decomposition agent by ball milling include:

[0076] Step S21'. Weigh 95g of high magnetic agent, 3g of V2O5 powder and 2g of TiO2 powder and mix them evenly to obtain a mixture.

[0077] Step S22'. The mixture obtained in step S21' is placed in a ball mill for grinding to obtain powder; wherein the ball mill has two kinds of stainless steel balls, the diameters of the two stainless steel balls are 10 mm and 5 mm respectively, and the mass ratio of the two stainless steel balls is 1:1, and the mass ratio of the stainless steel balls in the ball mill to the mixture is 70:1, and the rotation speed of the ball mill is controlled to be 800 rpm, and the ball milling time is 24 hours.

[0078] Step S23'. After grinding, the powder obtained in step S22' is calcined in an air atmosphere to obtain a powdered dioxin decomposer; wherein the calcination temperature is 600°C and the calcination time is 6h.

[0079] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for recycling catalytic cracking spent catalyst, characterized in that: The following steps are involved: Step S1. subjecting the spent catalytic cracking catalyst to magnetic separation to obtain a low magnetic agent and a high magnetic agent; Step S2. Using the high magnetic agent obtained in step S1 as a raw material, a dioxin decomposition agent is prepared by an impregnation method or a ball milling method; In step S2, the steps of preparing the dioxin decomposition agent by the impregnation method include: Step S21. Take a certain amount of high magnetic agent and TiO2 powder and mix them evenly to obtain a mixture; Step S22. Drying the mixture obtained in step S21 at 105° C. for 12 h, cooling and weighing a certain amount of the mixture; Step S23. Dissolving a certain amount of ammonium metavanadate in oxalic acid and adding deionized water to prepare a V2O5 impregnation solution; Step S24. Slowly pour the V2O5 impregnation solution obtained in step S23 into the mixture weighed in step S22, and stir thoroughly to form a paste. Allow the paste to stand in an air atmosphere for 24 hours and then dry at 105° C. to obtain a powder. Step S25. The dried powder in step S24 is calcined in an air atmosphere to obtain a powdered dioxin decomposition agent; In step S2, the steps of preparing a dioxin decomposition agent by ball milling include: Step S21' weigh a certain amount of high magnetic agent, V2O5 powder and TiO2 powder and mix them evenly to obtain a mixture; Step S22'. The mixture obtained in step S21' is placed in a ball mill and ground to obtain a powder; Step S23'. In an air atmosphere, the powder obtained in step S22' is calcined to obtain a powdery dioxin decomposition agent.

2. The method for recycling catalytic cracking waste catalyst according to claim 1, characterized in that: In step S21, the mass content of the high magnetic agent is 0.1%-90%, and the mass content of TiO2 is 0.1%-10%.

3. The method for recycling catalytic cracking waste catalyst according to claim 1, characterized in that: In step S23, the molar amount of oxalic acid added is twice the molar amount of ammonium metavanadate added.

4. The method for recycling catalytic cracking waste catalyst according to claim 1, characterized in that: In step S25, the calcination temperature is 200-800°C, and the calcination time is 1-48h.

5. The method for recycling catalytic cracking waste catalyst according to claim 1, characterized in that: In step S21', the mass fraction of the high magnetic agent is 0.1%-90%, the mass fraction of the V2O5 powder is 0.1%-10%, and the mass fraction of the TiO2 powder is 0.1%-10%.

6. The method for recycling catalytic cracking waste catalyst according to claim 1, characterized in that: In step S22', there are two kinds of stainless steel balls in the ball mill, the diameters of the two kinds of stainless steel balls are 10 mm and 5 mm respectively, and the mass ratio of the two kinds of stainless steel balls is 1:

1.

7. The method for recycling catalytic cracking waste catalyst according to claim 1 or 6, characterized in that: In step S22', the mass ratio of the stainless steel balls in the ball mill to the mixture is 10:1-100:1, the rotation speed of the ball mill is 100-1000 rpm, and the ball milling time is 1-48 hours.