A porous graphite material produced from coal gasification residue and its preparation method and application
By mixing the gasified residue with additives and heating and sintering, porous graphite materials are prepared, which solves the problem of resource utilization of gasified residues, and efficient production of electrode materials is achieved, reducing costs and environmental pollution.
Patent Information
- Application Number
- CN202211636654.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-15
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-12-15
AI Technical Summary
The high content of residual carbon in the gasified residue hinders its application in the fields of cement and concrete, and its resource utilization is difficult to achieve, resulting in low environmental pollution and utilization.
Porous graphite material is prepared by mixing the gasified residue with water, additives, crosslinking agents, dispersants, foaming agents and catalysts, and after heating and sintering, a porous graphite material is prepared for use as a porous graphite electrode to increase water and electrodes. Contact area to improve electrolysis or power generation efficiency.
It realizes the effective utilization of coal gasified residues, produces high-value porous graphite electrodes, reduces production costs, improves electrolysis or power generation efficiency, and avoids the generation of large amounts of wastewater, significantly reduces the volume of powdered coal gasified residues, and realizes Comprehensive utilization of resources.
Smart Images

Figure CN116062743B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a porous graphite material produced from coal gasification residue and a preparation method and application thereof, belonging to the technical field of solid waste resource utilization. Background Art
[0002] Coal gasification technology is known as the leader of the modern coal chemical industry and can provide synthesis gas for the entire back-end chemical production. However, a large amount of coal gasification slag will inevitably be produced during the coal gasification process, which will cause great pollution to the ecological environment. Since coal gasification slag contains unburned carbon residue and metal oxide minerals under high-temperature reaction, it is urgent to effectively utilize the carbon residue and relatively rich silicon, aluminum, iron and other resources in the coal gasification slag.
[0003] Coal gasification is the process of introducing gasifying agents such as oxygen, water vapor or hydrogen into coal or coal coke at high temperature, and then chemically reacting to generate synthesis gas from the combustible part of the coal or coal coke. After the coal undergoes thermal conversion processes such as combustion and gasification in the gasifier, the minerals and other inorganic components in the coal successively undergo processes such as rupture, agglomeration and melting, and finally form ash with some coal or coal coke that do not participate in the reaction. Coal gasification slag is divided into coarse slag and fine slag. The gasification slag obtained from the slag outlet of the gasifier is usually called coarse slag, and the fly ash leaving with the synthesis gas is called fine slag.
[0004] The chemical composition of coal gasification slag is related to factors such as coal ash content, flux type and introduction amount, and gasification process. Coal gasification slag is mainly composed of SiO2, Al2O3, CaO, Fe2O3 and residual carbon. The coarse and fine slag produced by the entrained flow gasifier were analyzed. It was found that when the gasifier was running at full load, the residual carbon content in the fine slag could reach 60%, which was usually higher than that in the coarse slag. However, the structural morphology of the residual carbon in the two was similar, and large-sized unburned carbon existed. The residual carbon is the result of incomplete gasification of coal, and its high content hinders its application in cement and concrete additives. The residual carbon in the fine slag is mainly porous granular with a higher degree of order. Because the reaction activity of disordered carbon is higher than that of graphite carbon and it is gasified preferentially, the proportion of graphitized structural carbon in the fine slag increases. Temperature is one of the important factors affecting the carbonization of residual carbon. Under high temperature conditions, especially at high temperatures above 1400℃ in the gasifier, some disordered carbon undergoes graphitization transformation. Compared with the carbon residue in coal char, the carbon residue in ash has a higher specific surface area, richer pore structure, larger average pore size, more ordered carbon crystal structure and more active sites.
[0005] As an inevitable by-product of the coal gasification process, fine slag is usually simply piled up in the open air, occupying a large area. The low utilization rate limits its transportation or utilization, and it is very easy to cause environmental pollution. With the in-depth study of the characteristics of coal gasification ash, the full understanding of the pollution of fly ash produced by boiler combustion to human health, soil, atmosphere, water bodies, and heavy metal leaching, as well as the economic and environmental benefits brought by the recycling of fly ash, it is crucial to achieve "zero emissions" of gasification technology and strengthen the environmental safety utilization of fine slag, which will help reduce fuel consumption, reduce the need for landfill, and improve the overall economy of gasifier operation. Gasification fine slag is a low-value, difficult-to-separate solid waste. At present, flotation is mostly used to enrich and separate residual carbon. However, the resource recycling of coal gasification residues is still one of the problems to be solved in this field. Summary of the invention
[0006] In order to solve the above technical problems, the purpose of the present invention is to provide a porous graphite material produced from coal gasification residue and its preparation method and application. The porous graphite material provided by the present invention can be used as a porous graphite electrode. Compared with traditional natural graphite electrodes, it has lower cost, can greatly increase the contact area between water and electrodes, and improve the efficiency of electrolysis or power generation.
[0007] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a porous graphite material produced from coal gasification residue, which comprises the following steps:
[0008] (1) mixing coal gasification residue with water, additives, a cross-linking agent, a dispersant, a foaming agent, a polymerization agent and a catalyst and molding the mixture to obtain a molded coal gasification residue;
[0009] (2) heating the formed coal gasification residue to generate porous carbon;
[0010] (3) The porous carbon is sintered and cooled to obtain the porous graphite material.
[0011] In the above method, preferably, in step (1), the coal gasification residue is screened coal gasification residue, and the particle size of the screened coal gasification residue is less than 200 μm. More preferably, the coal gasification residue is screened by flotation. The specific operation steps of flotation can be conventional in the art, for example, flotation can be performed using a conventional flotation column or flotation machine in the art.
[0012] In the above method, preferably, in step (1), the additive includes one or a combination of paraffin, light mineral oil and aromatic hydrocarbons. More preferably, the light mineral oil can be a light mineral oil with polycyclic aromatic hydrocarbons (especially bicyclic and / or tricyclic polycyclic aromatic hydrocarbons) as the main component. More preferably, the aromatic hydrocarbons can include one or a combination of C6 to C20 monocyclic aromatic hydrocarbons, polycyclic aromatic hydrocarbons and condensed aromatic hydrocarbons; further preferably, the aromatic hydrocarbons include polycyclic aromatic hydrocarbons, especially bicyclic and / or tricyclic polycyclic aromatic hydrocarbons.
[0013] In the above method, preferably, in step (1), the crosslinking agent includes one or a combination of hydroxyethyl acrylate crosslinking agents, methacrylate crosslinking agents, and blocked isocyanate crosslinking agents. More preferably, the crosslinking agent includes polytriallyl isocyanurate. The polytriallyl isocyanurate is a homopolymer of triallyl isocyanurate (TAIC). TAIC undergoes a self-polymerization reaction when heated to above 140°C in air to obtain the homopolymer, which is a transparent, hard, heat-resistant, and electrically insulating resin.
[0014] In the above method, preferably, in step (1), the dispersant includes a turbid liquid formed by dispersing polyethylene glycol fatty acid ester in a solvent. More preferably, the solvent includes water, mineral oil or vegetable oil, etc. More preferably, in the turbid liquid, the weight ratio of the polyethylene glycol fatty acid ester to the solvent is (0.5-3):1. The polyethylene glycol fatty acid ester used in the present invention may include one or more combinations of polyethylene glycol stearate, polyethylene glycol laurate and polyethylene glycol oleate, etc. More preferably, the polyethylene glycol fatty acid ester includes one or more combinations of polyethylene glycol 400 distearate, polyethylene glycol 400 dioleate and polyethylene glycol 600 dioleate, etc.
[0015] In the above method, preferably, in step (1), the foaming agent includes one or a combination of waterborne polyurethane surfactants, carboxylic acid and salt surfactants, alkyl sulfonic acid and salt surfactants, phenolic surfactants, and pyridine surfactants, etc. More preferably, the foaming agent includes waterborne polyurethane surfactants.
[0016] In the above method, preferably, in step (1), the polymerization agent includes one or a combination of polyvinyl n-butyl ether, vinyl sulfite, and vinyl ethylene carbonate, etc. More preferably, the polymerization agent includes polyvinyl n-butyl ether, which has good viscosity-increasing properties and low-temperature properties.
[0017] In the above method, preferably, in step (1), the catalyst comprises one or a combination of iron, nickel, titanium, silicon, their carbides, their oxides, etc.
[0018] In the above method, preferably, in step (1), the weight ratio of the coal gasification residue to water is (1-5):10.
[0019] In the above method, preferably, in step (1), the weight ratio of the coal gasification residue to the additive is (2-5):1.
[0020] In the above method, preferably, in step (1), the weight ratio of the coal gasification residue to the cross-linking agent is (3-6):1.
[0021] In the above method, preferably, in step (1), the weight ratio of the coal gasification residue to the dispersant is (80-110):1.
[0022] In the above method, preferably, in step (1), the weight ratio of the coal gasification residue to the foaming agent is (100-300):1.
[0023] In the above method, preferably, in step (1), the weight ratio of the coal gasification residue to the polymerization agent is (10-20):1.
[0024] In the above method, preferably, in step (1), the weight ratio of the coal gasification residue to the catalyst is (4-10):1.
[0025] In the above method, in step (1), the forming can be performed by conventional mold forming. Preferably, the formed coal gasification residue can be a coal gasification residue sheet. More preferably, the thickness of the coal gasification residue sheet is 1-2 mm. The length and width of the coal gasification residue sheet can be designed according to the size of the electrolytic cell or fuel cell. More preferably, the length and width of the coal gasification residue sheet are generally less than 100 mm × 100 mm, that is, the length is less than 100 mm and the width is less than 100 mm.
[0026] In the above method, preferably, step (1) may specifically include: screening the coal gasification residue and mixing it with water; then adding additives, crosslinking agents and dispersants to obtain a mixture (suspension); adding a foaming agent to the mixture to generate foam, then adding a polymerizing agent and a catalyst, injecting it into a mold before forming a gel, and forming it into a sheet in the mold to obtain a coal gasification residue sheet. Among them, more preferably, the coal gasification residue can be washed with water after screening and then mixed with water. More preferably, under stirring conditions, additives, crosslinking agents and dispersants are added and mixed evenly to obtain a mixture; the stirring speed is preferably 500-700 rpm. More preferably, under stirring conditions, a foaming agent is added to generate foam; the stirring speed is preferably 200-300 rpm. More preferably, stirring is continued for a period of time after adding the polymerizing agent and the catalyst; the stirring speed is preferably 500-700 rpm.
[0027] In the above method, preferably, in step (2), the formed coal gasification residue is heated to 100-150° C. and kept warm for 2-3 hours under air-tight conditions (i.e., under inert gas protection), and then continued to be heated to 400-600° C. and kept warm for 1.5-2.5 hours (still maintaining air-tight conditions). The product obtained after heating in step (2) mainly includes the porous carbon, hydrocarbon oil and liquefied gas.
[0028] In the above method, preferably, in step (2), the porous carbon is a porous carbon sheet.
[0029] In the above method, more preferably, step (2) may specifically include:
[0030] The coal gasification residue pieces are heated to 100-150°C in an airtight condition and kept at this temperature for 2-3 hours to distill out water vapor, gaseous reactants and hydrocarbon vapor;
[0031] Continue heating and raising the temperature (still maintaining air isolation conditions, i.e., maintaining inert gas protection) to 400-600°C and keep warm for 1.5-2.5 hours to cause the high-boiling point macromolecular hydrocarbons in the coal gasification residue sheets to undergo thermal conversion reaction and crack into light hydrocarbons which are distilled out in the form of hydrocarbon vapor, and part of the residue is coked to form coke to obtain a porous carbon sheet.
[0032] In the above method, preferably, in step (2), the heating rate of the heating is 15-25°C / h.
[0033] In the above method, preferably, step (2) further comprises: subjecting the gaseous reactants and hydrocarbon vapor distilled during the heating process of the coal gasification residue flakes to oil and gas fractionation to obtain hydrocarbon oil and liquefied gas. The oil and gas fractionation can be carried out in a conventional oil and gas fractionation system. The gaseous reactants mainly include compound impurities containing O and / or S, etc., which are sent to the oil and gas fractionation system together with the hydrocarbon vapor and can be removed by steam stripping.
[0034] In the above method, preferably, step (2) further comprises: condensing the water vapor distilled during the heating of the coal gasification residue slices and sending it to a sewage treatment system for treatment. After being treated in the sewage treatment system, clean water and sludge are obtained.
[0035] In the above method, preferably, in step (3), the sintering temperature is 800-1500° C., the time is 2-5 hours, and the sintering is carried out in an air-tight condition (ie, under the protection of an inert gas).
[0036] In the above method, preferably, in step (3), the sintering is carried out by heating the temperature to the sintering temperature at a heating rate of 15-25° C. / h.
[0037] In the above method, preferably, in step (3), the porous graphite material is a porous graphite sheet.
[0038] In the above method, preferably, in step (2) and step (3), the process of heating the formed coal gasification residue (preferably coal gasification residue sheets) and the process of sintering the porous carbon (preferably porous carbon sheets) can be carried out using a fixed bed reactor.
[0039] According to a specific embodiment of the present invention, preferably, the above method further comprises: washing the screened coal gasification residue with clean water treated by a sewage treatment system.
[0040] According to a specific embodiment of the present invention, preferably, the above method further comprises: mixing the clean water treated by the sewage treatment system with the coal gasification residue in step (1).
[0041] According to a specific embodiment of the present invention, preferably, the above method further comprises: using the sludge obtained after treatment in the sewage treatment system as a raw material, mixing it with the coal gasification residue, water, additives, cross-linking agent, dispersant, foaming agent, polymerization agent and catalyst in step (1) and then molding it to obtain the molded coal gasification residue.
[0042] According to a specific embodiment of the present invention, preferably, the above method further comprises: performing oil-water separation on the waste liquid obtained from the coal gasification residue after water washing and screening to obtain sewage and waste oil, sending the sewage to the sewage treatment system for treatment, and sending the waste oil to the oil and gas fractionation system for oil and gas fractionation.
[0043] According to a specific embodiment of the present invention, preferably, the above method further comprises: sending the liquefied gas obtained after oil and gas fractionation by the oil and gas fractionation system to a liquefied gas storage tank for storage, and sending the hydrocarbon oil obtained after oil and gas fractionation by the oil and gas fractionation system to a hydrocarbon oil storage tank for storage.
[0044] According to a specific embodiment of the present invention, preferably, the above method further comprises: using the raw materials stored in the hydrocarbon oil storage tank and the liquefied gas storage tank as auxiliary fuel for heating in step (2) and / or step (3).
[0045] According to a specific embodiment of the present invention, preferably, the method further comprises: using coal gasification residue scraps or a mixture of coal gasification residue scraps and coal as the main fuel for heating in step (2) and / or step (3). Coal gasification residue scraps include, but are not limited to, sieved residues that do not meet the particle size requirements, coal gasification residue scraps that are trimmed according to length and width specifications, etc.
[0046] According to a specific embodiment of the present invention, preferably, the above-mentioned preparation method further comprises: the porous graphite material (preferably a porous graphite sheet) obtained in step (3) is subjected to surface processing and / or chemical modification by at least physical means to obtain a treated porous graphite material. Among them, more preferably, the chemical modification includes acid treatment and / or alkali treatment, etc., and preferably the porous graphite material is chemically modified by an acid-base method. The specific operation of the acid-base method can adopt the operating steps of the conventional graphite electrode acid-base purification and modification method in the art, and those skilled in the art can select and adjust according to actual conditions. The specific method of surface processing by physical means can be conventional in the art, such as but not limited to laser surface processing, electrophoresis, etc. More preferably, step (4) can further comprise: cutting the porous graphite material obtained in step (3), and then performing the physical surface processing and / or chemical modification; or firstly performing the surface processing and / or chemical modification of the porous graphite material obtained in step (3) by at least physical means, and then cutting; obtaining the treated porous graphite material. Those skilled in the art should understand that after physical surface processing and / or chemical modification, and / or after cutting, conventional operations such as cleaning and drying may be selectively performed. The present invention does not specifically limit these conventional operations, and those skilled in the art may make conventional adjustments based on actual conditions.
[0047] In the present invention, the porous graphite material (preferably a porous graphite sheet) obtained in step (3) of the above preparation method can be used as a porous graphite electrode, or can be used as a porous graphite electrode after being processed in step (4) above.
[0048] The method for preparing a porous graphite material produced from coal gasification residue provided by the present invention is a method for preparing a porous graphite material using coal gasification residue as a raw material by utilizing the characteristics of high residual carbon content in coal gasification residue and graphitization transformation at high temperature. In a preferred embodiment of the present invention, the method first separates coarse slag and fine slag from coal gasification residue by flotation, then mixes the fine slag with water, additives, crosslinking agents, dispersants, foaming agents, polymerizing agents and foaming agents, and after being molded into sheet-like coal gasification residue by a mold, is placed in a fixed bed reactor for heating and temperature raising to generate coke, and is sintered at high temperature, and a porous graphite material (preferably a porous graphite sheet) is obtained after cooling. At the same time, the method for preparing a porous graphite material produced from coal gasification residue provided by the present invention is also a combined process for extracting hydrocarbon oil from coal gasification residue and producing porous graphite material, which produces porous graphite material by a thermal conversion method, and simultaneously produces hydrocarbon oil as a byproduct. The porous graphite material (preferably a porous graphite sheet) can be used as a graphite electrode in an electrolytic cell or a fuel cell, which is beneficial to increase the contact area between water and the electrode and improve the efficiency of electrolysis or power generation.
[0049] A second aspect of the present invention provides a porous graphite material produced from coal gasification residue, which is prepared by the above-mentioned method for preparing a porous graphite material produced from coal gasification residue.
[0050] According to a specific embodiment of the present invention, preferably, the density of the porous graphite material is 0.5-0.9 g / cm 3 The present invention can control the density of the prepared porous graphite material to be 0.5-0.9 g / cm by controlling the dosage ratio of the additive, crosslinking agent, polymerization agent and catalyst mixed with the coal gasification residue in step (1). 3 .
[0051] According to a specific embodiment of the present invention, preferably, the specific surface area of the porous graphite material is 150-400m 2 / g.
[0052] According to a specific embodiment of the present invention, preferably, the pore size of the porous graphite material is 2-15 nm.
[0053] According to a specific embodiment of the present invention, preferably, the porous graphite material is a porous graphite sheet.
[0054] The porous graphite material (including the treated porous graphite material) provided by the present invention has a lower density than water, has gaps of different sizes and shapes inside, and has a larger specific surface area. Compared with traditional natural graphite electrodes, the material is used as a porous graphite electrode, which has a lower cost, can greatly increase the contact area between water and the electrode, and improve the efficiency of electrolysis or power generation.
[0055] A third aspect of the present invention provides a use of the porous graphite material produced from coal gasification residue as a graphite electrode.
[0056] According to a specific embodiment of the present invention, preferably, the application is: the porous graphite material is used as a graphite electrode in an electrolytic cell or a fuel cell.
[0057] The technical solution provided by the present invention realizes the effective utilization of coal gasification residues, can produce high-value product porous graphite electrodes, and can dry distill by-product hydrocarbon oil in the process of preparing graphite electrodes. Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:
[0058] 1. The technical solution provided by the present invention is lower in cost than the traditional graphite electrode preparation method. The prepared porous graphite electrode has a large specific surface area, which can greatly increase the contact area between water and the electrode and improve the electrolysis or power generation efficiency.
[0059] 2. The technical solution provided by the present invention mixes coal gasification residue with water, additives, cross-linking agents, dispersants, foaming agents, polymers and catalysts to form sheets and then heats them to generate coke. The coke is sintered at high temperature and cooled to obtain porous graphite electrode sheets. This process couples the two processes of thermal conversion of coal gasification residue and roasting of graphite electrode sheets to achieve the preparation of graphite electrode sheets. This process can produce hydrocarbon oil while producing graphite electrode sheets, and the produced hydrocarbon oil is of better quality than traditional water-washed coal gasification residue oil.
[0060] 3. The technical solution provided by the present invention avoids the generation of a large amount of waste water (the existing conventional method for utilizing coal gasification residue usually generates a large amount of waste water), significantly reduces the volume of powdered coal gasification residue, solves the problem that both water washing and coking cannot process powdered coal gasification residue, and realizes comprehensive utilization of resources.
[0061] 4. The technical solution provided by the present invention has small process investment, wide working conditions, strong applicability, easy operation, simple process, low cost, and has obvious economic, environmental and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 A flow chart of the method for producing porous graphite electrode sheets from coal gasification residue provided in Example 1 and Example 2.
[0063] Figure 2 The XRD detection spectrum of the porous graphite electrode provided in Example 2 and the graphite standard spectrum.
[0064] Figure 3 This is a comparison chart of discharge curves of the porous graphite electrode provided in Example 2 and the conventional graphite electrode at different current densities. DETAILED DESCRIPTION
[0065] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0066] A specific embodiment of the present invention provides a method for producing a porous graphite electrode sheet from coal gasification residue, wherein the method comprises:
[0067] (1) screening the coal gasification residue by flotation to obtain fine residue with a particle size of less than 200 μm, washing the screened coal gasification residue with water, and then adding additives, crosslinking agents and dispersants in sequence to form a suspension; adding a foaming agent to the suspension to generate foam, and then adding a polymerizing agent and a catalyst, injecting the suspension into a mold before forming a gel, and forming the suspension into a sheet in the mold to obtain a coal gasification residue sheet;
[0068] Wherein, the additive includes one or a combination of paraffin, light mineral oil and aromatic hydrocarbons;
[0069] The crosslinking agent includes one or a combination of hydroxyethyl acrylate crosslinking agent, methacrylate crosslinking agent and blocked isocyanate crosslinking agent; preferably, the crosslinking agent is polytriallyl isocyanurate;
[0070] The dispersant comprises a turbid liquid formed by dispersing polyethylene glycol fatty acid ester in a solvent; the solvent comprises water, mineral oil or vegetable oil; the weight ratio of the polyethylene glycol fatty acid ester to the solvent is (0.5-3):1;
[0071] The foaming agent includes one or a combination of waterborne polyurethane surfactants, carboxylic acid and salt surfactants, alkyl sulfonic acid and salt surfactants, phenolic surfactants and pyridine surfactants; preferably, the foaming agent is a waterborne polyurethane surfactant;
[0072] The polymerization agent includes one or a combination of polyvinyl n-butyl ether, vinyl sulfite, and vinyl ethylene carbonate, etc.; preferably, the polymerization agent is polyvinyl n-butyl ether;
[0073] The catalyst comprises one or a combination of iron, nickel, titanium, silicon, their carbides and their oxides;
[0074] The weight ratio of each component is:
[0075] Coal gasification residue: water = (1-5): 10
[0076] Coal gasification residue: additive = (2-5): 1
[0077] Coal gasification residue: cross-linking agent = (3-6): 1
[0078] Coal gasification residue: dispersant = (80-110): 1
[0079] Coal gasification residue: foaming agent = (100-300): 1
[0080] Coal gasification residue: polymerizer = (10-20): 1
[0081] Coal gasification residue: catalyst = (4-10): 1;
[0082] The thickness of the coal gasification residue sheet is 1-2 mm, preferably 1.25 mm;
[0083] The length and width of the coal gasification residue sheet can be determined according to the size of the porous graphite electrode to be prepared; for example, the length and width are 100 mm respectively;
[0084] (2) heating the coal gasification residue sheet to 100-150° C. at a heating rate of 15-25° C. / h and keeping the temperature for 2-3 hours in an air-tight condition (i.e., under the protection of an inert gas), and distilling out water vapor, gaseous reactants (the gaseous reactants mainly include compound impurities containing O and / or S, etc.) and light hydrocarbons (in the form of hydrocarbon vapor); continuing to heat at a heating rate of 15-25° C. / h (still maintaining the air-tight condition, i.e., maintaining the protection of an inert gas) to 400-600° C. and keeping the temperature for 1.5-2.5 hours, so that the high-boiling-point macromolecular hydrocarbons in the coal gasification residue sheet undergo a thermal conversion reaction and cracking to generate light hydrocarbons, which are distilled out in the form of hydrocarbon vapor, and part of the residue is coked to generate coke, thereby obtaining a porous carbon sheet;
[0085] (3) in an air-tight condition (i.e., under the protection of an inert gas), continue heating at a heating rate of 15-25° C. / h to sinter the porous carbon sheet at 800-1500° C. for 2-5 hours, and after cooling, obtain a porous graphite electrode sheet;
[0086] Wherein, in step (2) and step (3), the process of heating the coal gasification residue sheet and the process of sintering the porous carbon sheet can be carried out using a fixed bed reactor;
[0087] wherein the gaseous reactants and hydrocarbon vapor distilled out during the heating process of the fixed bed reactor are transported to the oil and gas fractionation system for oil and gas fractionation;
[0088] The water vapor distilled during the heating process of the fixed bed reactor is condensed and sent to the sewage treatment system for treatment; after being treated by the sewage treatment system, clean water and sludge are obtained;
[0089] wherein, the clean water treated by the sewage treatment system is used to wash the screened coal gasification residue in step (1); the waste liquid obtained by washing the screened coal gasification residue is subjected to oil-water separation to obtain sewage and waste oil, the sewage is sent to the sewage treatment system for treatment, and the waste oil is sent to the oil-gas fractionation system for oil-gas fractionation;
[0090] wherein the purified water treated by the sewage treatment system is mixed with the coal gasification residue in step (1);
[0091] wherein the sludge obtained after treatment in the sewage treatment system is used as a raw material (counted in the coal gasification residue), mixed with the coal gasification residue in step (1), water, additives, crosslinking agent, dispersant, foaming agent, polymerization agent and catalyst, and then molded to obtain the molded coal gasification residue;
[0092] (4) sending the liquefied gas obtained after the oil and gas fractionation system performs oil and gas fractionation to a liquefied gas storage tank for storage, and sending the hydrocarbon oil obtained after the oil and gas fractionation system performs oil and gas fractionation to a hydrocarbon oil storage tank for storage;
[0093] The raw materials stored in the hydrocarbon oil storage tank and the liquefied gas storage tank are used as auxiliary fuel for heating in step (2) and / or step (3); coal gasification residue or a mixture of coal gasification residue and coal is used as main fuel for heating in step (2) and / or step (3);
[0094] The method may further include: cutting the porous graphite electrode sheet prepared in step (3), optionally performing surface processing by physical means and / or chemical modification such as acid-base method as needed, and then cleaning and drying to obtain the porous graphite electrode sheet.
[0095] The density of the porous graphite electrode sheet prepared in the above specific embodiment is 0.5-0.9 g / cm 3 , with a specific surface area of 150-400m 2 / g, pore size is 2-15nm.
[0096] Example 1
[0097] This embodiment provides a method for producing a porous graphite electrode sheet from coal gasification residue, and the process is as follows: Figure 1 shown.
[0098] The method includes:
[0099] (1) screening the coal gasification residue by flotation to obtain fine residue with a particle size of less than 200 μm, washing the screened coal gasification residue with water and mixing it with water in a reactor, then adding additives, crosslinking agents and dispersants in sequence under stirring conditions at a speed of 500-700 rpm, mixing them evenly to obtain a suspension; adding a foaming agent to the suspension under stirring conditions at a speed of 200-300 rpm to generate foam, then adding a polymerization agent and a catalyst, continuing to stir for a period of time under stirring conditions at a speed of 500-700 rpm, injecting into a mold before forming a gel, and forming into a sheet in the mold to obtain a coal gasification residue sheet;
[0100] Wherein, the additive is light mineral oil; the light mineral oil is a light mineral oil with two-ring and / or three-ring polycyclic aromatic hydrocarbons as main components;
[0101] The cross-linking agent is polytriallyl isocyanurate;
[0102] The dispersant is a turbid liquid formed by dispersing polyethylene glycol 400 distearate in a solvent; the solvent is mineral oil; the weight ratio of the polyethylene glycol fatty acid ester to the solvent is 1:1;
[0103] The foaming agent is a water-based polyurethane surfactant;
[0104] The polymerization agent is polyvinyl n-butyl ether;
[0105] The catalyst is a Ni-Fe oxide catalyst (the catalyst is a conventional Ni-Fe oxide catalyst with Al2O3 as a carrier);
[0106] The weight ratio of each component is:
[0107] Coal gasification residue: water = 1:10
[0108] Coal gasification residue: additive = 3:1
[0109] Coal gasification residue: cross-linking agent = 3:1
[0110] Coal gasification residue: dispersant = 100:1
[0111] Coal gasification residue: foaming agent = 100:1
[0112] Coal gasification residue: polymerizer = 10:1
[0113] Coal gasification residue: catalyst = 4:1;
[0114] Among them, the thickness of the coal gasification residue sheet is 1.25mm;
[0115] Among them, the length and width of the coal gasification residue sheet are 100 mm respectively;
[0116] (2) placing the coal gasification residue sheet in a fixed bed reactor (a closed rotary kiln is used in this embodiment), and heating the temperature to 100°C at a heating rate of 15°C / h under air-tight conditions (i.e., under inert gas protection) for 3 hours to distill out water vapor, gaseous reactants (the gaseous reactants mainly include compound impurities containing O and / or S, etc.) and light hydrocarbons (in the form of hydrocarbon vapor); continuing to heat the temperature to below 400°C at a heating rate of 15°C / h to distill out the residual fuel fraction (in the form of hydrocarbon vapor); continuing to heat the temperature to 400°C-600°C at a heating rate of 15°C / h and keeping the temperature for 2 hours, so that the high-boiling-point macromolecular hydrocarbons in the coal gasification residue sheet undergo thermal conversion reaction and cracking to generate light hydrocarbons and distill them out (in the form of hydrocarbon vapor), and part of the residue is coked to generate coke, thereby obtaining a porous carbon sheet;
[0117] (3) in an air-tight condition (i.e., under the protection of an inert gas), the temperature is continuously raised to 1000° C. at a heating rate of 15° C. / h and kept at this temperature for 2 hours to sinter and graphitize the porous carbon sheet, and after cooling, a porous graphite electrode is obtained;
[0118] wherein the gaseous reactants and hydrocarbon vapors distilled out of the fixed bed reactor during the temperature increase process are transported to the oil and gas fractionation system for oil and gas fractionation;
[0119] The water vapor distilled from the fixed bed reactor during the heating process is condensed and sent to the sewage treatment system for treatment; after being treated by the sewage treatment system, clean water and sludge are obtained;
[0120] wherein, the clean water treated by the sewage treatment system is used to wash the screened coal gasification residue in step (1); the waste liquid obtained by washing the screened coal gasification residue is subjected to oil-water separation to obtain sewage and waste oil, the sewage is sent to the sewage treatment system for treatment, and the waste oil is sent to the oil-gas fractionation system for oil-gas fractionation;
[0121] wherein the purified water treated by the sewage treatment system is mixed with the coal gasification residue in step (1);
[0122] wherein the sludge obtained after treatment in the sewage treatment system is used as a raw material (counted in the coal gasification residue), mixed with the coal gasification residue in step (1), water, additives, crosslinking agent, dispersant, foaming agent, polymerization agent and catalyst, and then molded to obtain the molded coal gasification residue;
[0123] (4) sending the liquefied gas obtained after the oil and gas fractionation system performs oil and gas fractionation to a liquefied gas storage tank for storage, and sending the hydrocarbon oil obtained after the oil and gas fractionation system performs oil and gas fractionation to a hydrocarbon oil storage tank for storage;
[0124] The raw materials stored in the hydrocarbon oil storage tank and the liquefied gas storage tank are used as auxiliary fuel for heating in step (2) and step (3); coal gasification residue scraps or a mixture of coal gasification residue scraps and coal are used as main fuel for heating in step (2) and step (3); and the waste gas generated by the combustion of the fuel during heating in the fixed bed reactor is discharged into the atmosphere after tail gas treatment (the main component is CO2).
[0125] The density of the porous graphite electrode prepared in this example is 0.5 g / cm 3 , with a specific surface area of 200m 2 / g, and the average pore size is 8nm.
[0126] Example 2
[0127] This embodiment provides a method for producing a porous graphite electrode sheet from coal gasification residue, and the process is as follows: Figure 1 shown.
[0128] The method includes:
[0129] (1) screening the coal gasification residue by flotation to obtain fine residue with a particle size of less than 200 μm, washing the screened coal gasification residue with water and mixing it with water in a reactor, then adding additives, crosslinking agents and dispersants in sequence under stirring conditions at a speed of 500-700 rpm, mixing them evenly to obtain a suspension; adding a foaming agent to the suspension under stirring conditions at a speed of 200-300 rpm to generate foam, then adding a polymerization agent and a catalyst, continuing to stir for a period of time under stirring conditions at a speed of 500-700 rpm, injecting into a mold before forming a gel, and forming into a sheet in the mold to obtain a coal gasification residue sheet;
[0130] Wherein, the additive is light mineral oil; the light mineral oil is a light mineral oil with two-ring and / or three-ring polycyclic aromatic hydrocarbons as main components;
[0131] The cross-linking agent is polytriallyl isocyanurate;
[0132] The dispersant is a turbid liquid formed by dispersing polyethylene glycol 600 dioleate in a solvent; the solvent is mineral oil; the weight ratio of the polyethylene glycol fatty acid ester to the solvent is 2:1;
[0133] The foaming agent is a water-based polyurethane surfactant;
[0134] The polymerization agent is polyvinyl n-butyl ether;
[0135] The catalyst is a Ni-Fe oxide catalyst (same as in Example 1);
[0136] Wherein, the weight ratio of each component is:
[0137] Coal gasification residue: water = 1:5
[0138] Coal gasification residue: additive = 3:1
[0139] Coal gasification residue: cross-linking agent = 5:1
[0140] Coal gasification residue: dispersant = 100:1
[0141] Coal gasification residue: foaming agent = 150:1
[0142] Coal gasification residue: polymerizer = 15:1
[0143] Coal gasification residue: catalyst = 4:1;
[0144] Among them, the thickness of the coal gasification residue sheet is 1.25mm;
[0145] Among them, the length and width of the coal gasification residue sheet are 100 mm respectively;
[0146] (2) placing the coal gasification residue sheet in a fixed bed reactor (a closed rotary kiln is used in this embodiment), and heating the temperature to 150°C at a heating rate of 25°C / h under air-tight conditions (i.e., under inert gas protection) for 2 hours to distill out water vapor, gaseous reactants (the gaseous reactants mainly include compound impurities containing O and / or S, etc.) and light hydrocarbons (in the form of hydrocarbon vapor); continuing to heat the temperature to below 400°C at a heating rate of 25°C / h to distill out the residual fuel fraction (in the form of hydrocarbon vapor); continuing to heat the temperature to 400°C-600°C at a heating rate of 25°C / h and keeping the temperature for 2 hours, so that the high-boiling-point macromolecular hydrocarbons in the coal gasification residue sheet undergo thermal conversion reaction and cracking to generate light hydrocarbons and distill them out (in the form of hydrocarbon vapor), and part of the residue is coked to generate coke, thereby obtaining a porous carbon sheet;
[0147] (3) in an air-tight condition (i.e., under the protection of an inert gas), the temperature is continuously raised to 1500° C. at a heating rate of 25° C. / h and kept at this temperature for 2 hours to sinter and graphitize the porous carbon sheet, and after cooling, a porous graphite electrode is obtained;
[0148] wherein the gaseous reactants and hydrocarbon vapors distilled out of the fixed bed reactor during the temperature increase process are transported to the oil and gas fractionation system for oil and gas fractionation;
[0149] The water vapor distilled from the fixed bed reactor during the heating process is condensed and sent to the sewage treatment system for treatment; after being treated by the sewage treatment system, clean water and sludge are obtained;
[0150] wherein, the clean water treated by the sewage treatment system is used to wash the screened coal gasification residue in step (1); the waste liquid obtained by washing the screened coal gasification residue is subjected to oil-water separation to obtain sewage and waste oil, the sewage is sent to the sewage treatment system for treatment, and the waste oil is sent to the oil-gas fractionation system for oil-gas fractionation;
[0151] wherein the purified water treated by the sewage treatment system is mixed with the coal gasification residue in step (1);
[0152] wherein the sludge obtained after treatment in the sewage treatment system is used as a raw material (counted in the coal gasification residue), mixed with the coal gasification residue in step (1), water, additives, crosslinking agent, dispersant, foaming agent, polymerization agent and catalyst, and then molded to obtain the molded coal gasification residue;
[0153] (4) sending the liquefied gas obtained after the oil and gas fractionation system performs oil and gas fractionation to a liquefied gas storage tank for storage, and sending the hydrocarbon oil obtained after the oil and gas fractionation system performs oil and gas fractionation to a hydrocarbon oil storage tank for storage;
[0154] The raw materials stored in the hydrocarbon oil storage tank and the liquefied gas storage tank are used as auxiliary fuel for heating in step (2) and step (3); coal gasification residue scraps or a mixture of coal gasification residue scraps and coal are used as main fuel for heating in step (2) and step (3); and the waste gas generated by the combustion of the fuel during heating in the fixed bed reactor is discharged into the atmosphere after tail gas treatment (the main component is CO2).
[0155] The density of the porous graphite electrode prepared in this example is 0.9 g / cm 3 , with a specific surface area of 300m 2 / g, and the average pore size is 10nm.
[0156] Figure 2 The XRD detection spectrum of the porous graphite electrode provided in this embodiment and the graphite standard spectrum. Figure 2 It can be seen that the unit cell size and properties of the porous graphite electrode prepared in this embodiment are better than those of the graphite electrode. Figure 3 The discharge curve comparison diagram of the porous graphite electrode provided in this embodiment and the conventional graphite electrode at different current densities. Figure 3 In the figure, the dotted line represents a conventional graphite electrode, the solid line represents a porous graphite electrode of this embodiment, and a is the -2 Discharge curve under current density, b is at 0.15mA.cm -2Discharge curve under current density, c is at 0.1mA.cm -2 Discharge curve under current density. Figure 3 It can be seen that the porous graphite electrode prepared in this embodiment has a high specific surface area and a mesoporous structure compared to conventional graphite electrodes, and there is more space to accommodate discharge products, so the discharge capacity is greatly improved compared to conventional graphite electrodes.
[0157] Comparative Example 1
[0158] This comparative example provides a method for producing porous graphite electrode sheets from coal gasification residue.
[0159] The method includes:
[0160] (1) screening the coal gasification residue by flotation to obtain fine residue with a particle size of less than 200 μm, washing the screened coal gasification residue with water and mixing it with water in a reactor, and then adding additives, crosslinking agents and dispersants in sequence under stirring conditions at a speed of 500-700 rpm, mixing them evenly to obtain a suspension; adding a polymerizing agent and a catalyst to the suspension under stirring conditions at a speed of 200-300 rpm, continuing to stir for a period of time under stirring conditions at a speed of 500-700 rpm, injecting into a mold before forming a gel, and forming into a sheet in the mold to obtain a coal gasification residue sheet;
[0161] Wherein, the additive is light mineral oil; the light mineral oil is a light mineral oil with two-ring and / or three-ring polycyclic aromatic hydrocarbons as main components;
[0162] The cross-linking agent is polytriallyl isocyanurate;
[0163] The dispersant is a turbid liquid formed by dispersing polyethylene glycol 400 distearate in a solvent; the solvent is mineral oil; the weight ratio of the polyethylene glycol fatty acid ester to the solvent is 1:1;
[0164] The polymerization agent is polyvinyl n-butyl ether;
[0165] The catalyst is a Ni-Fe oxide catalyst (same as in Example 1);
[0166] Wherein, the weight ratio of each component is:
[0167] Coal gasification residue: water = 1:10
[0168] Coal gasification residue: additive = 3:1
[0169] Coal gasification residue: cross-linking agent = 4:1
[0170] Coal gasification residue: dispersant = 100:1
[0171] Coal gasification residue: polymerizer = 15:1
[0172] Coal gasification residue: catalyst = 3:1;
[0173] Among them, the thickness of the coal gasification residue sheet is 1.05mm;
[0174] Among them, the length and width of the coal gasification residue sheet are 100 mm respectively;
[0175] (2) placing the coal gasification residue sheet in a fixed bed reactor (a closed rotary kiln is used in this comparative example), heating the sheet to about 100°C at a heating rate of 15°C / h under air-tight conditions (i.e., under inert gas protection) and keeping the temperature for 2 hours to distill out water vapor, gaseous reactants (the gaseous reactants mainly include compound impurities containing O and / or S, etc.) and light hydrocarbons (in the form of hydrocarbon vapor); continuing to heat the sheet to below 400°C at a heating rate of 15°C / h to distill out the residual fuel fraction (in the form of hydrocarbon vapor); continuing to heat the sheet to 400°C-600°C at a heating rate of 15°C / h and keeping the temperature for 2 hours, so that the high-boiling-point macromolecular hydrocarbons in the coal gasification residue sheet undergo thermal conversion reaction and cracking to generate light hydrocarbons and distill them out (in the form of hydrocarbon vapor), and part of the residue is coked to generate coke, thereby obtaining a porous carbon sheet;
[0176] (3) in an air-tight condition (i.e., under the protection of an inert gas), the temperature is continuously raised to 1800° C. at a heating rate of 15° C. / h and kept at this temperature for 2 hours to sinter and graphitize the porous carbon sheet, and after cooling, a porous graphite electrode is obtained;
[0177] wherein the gaseous reactants and hydrocarbon vapors distilled out of the fixed bed reactor during the temperature increase process are transported to the oil and gas fractionation system for oil and gas fractionation;
[0178] The water vapor distilled from the fixed bed reactor during the heating process is condensed and sent to the sewage treatment system for treatment; after being treated by the sewage treatment system, clean water and sludge are obtained;
[0179] wherein, the clean water treated by the sewage treatment system is used to wash the screened coal gasification residue in step (1); the waste liquid obtained by washing the screened coal gasification residue is subjected to oil-water separation to obtain sewage and waste oil, the sewage is sent to the sewage treatment system for treatment, and the waste oil is sent to the oil-gas fractionation system for oil-gas fractionation;
[0180] wherein the purified water treated by the sewage treatment system is mixed with the coal gasification residue in step (1);
[0181] wherein the sludge obtained after treatment in the sewage treatment system is used as a raw material (counted in the coal gasification residue), mixed with the coal gasification residue, water, additives, crosslinking agent, dispersant, polymerization agent and catalyst in step (1) and then molded to obtain the molded coal gasification residue;
[0182] (4) sending the liquefied gas obtained after the oil and gas fractionation system performs oil and gas fractionation to a liquefied gas storage tank for storage, and sending the hydrocarbon oil obtained after the oil and gas fractionation system performs oil and gas fractionation to a hydrocarbon oil storage tank for storage;
[0183] The raw materials stored in the hydrocarbon oil storage tank and the liquefied gas storage tank are used as auxiliary fuel for heating in step (2) and step (3); coal gasification residue scraps or a mixture of coal gasification residue scraps and coal are used as main fuel for heating in step (2) and step (3); and the waste gas generated by the combustion of the fuel during heating in the fixed bed reactor is discharged into the atmosphere after tail gas treatment (the main component is CO2).
[0184] The density of the porous graphite electrode prepared in this comparative example is 0.4 g / cm 3 , with a specific surface area of 120m 2 / g, and the average pore size is 6nm.
[0185] Comparative Example 2
[0186] This comparative example provides a method for producing porous graphite electrode sheets from coal gasification residue.
[0187] The method includes:
[0188] (1) screening the coal gasification residue by flotation to obtain fine residue with a particle size of less than 200 μm, washing the screened coal gasification residue with water and mixing it with water in a reactor, then adding a dispersant under stirring conditions at a speed of 500-700 rpm, mixing evenly, and obtaining a suspension; adding a foaming agent to the suspension under stirring conditions at a speed of 200-300 rpm to generate foam, then adding a polymerization agent and a catalyst, continuing to stir for a period of time under stirring conditions at a speed of 500-700 rpm, injecting into a mold before forming a gel, and forming into a sheet in the mold to obtain a coal gasification residue sheet;
[0189] Wherein, the dispersant is a turbid liquid formed by dispersing polyethylene glycol 400 distearate in a solvent; the solvent is mineral oil; the weight ratio of the polyethylene glycol fatty acid ester to the solvent is 1:1;
[0190] The foaming agent is a water-based polyurethane surfactant;
[0191] The polymerization agent is polyvinyl n-butyl ether;
[0192] The catalyst is a Ni-Fe oxide catalyst (same as in Example 1);
[0193] Wherein, the weight ratio of each component is:
[0194] Coal gasification residue: water = 1:10
[0195] Coal gasification residue: dispersant = 100:1
[0196] Coal gasification residue: foaming agent = 150:1
[0197] Coal gasification residue: polymerizer = 15:1
[0198] Coal gasification residue: catalyst = 4:1;
[0199] Among them, the thickness of the coal gasification residue sheet is 0.8mm;
[0200] Among them, the length and width of the coal gasification residue sheet are 70 mm respectively;
[0201] (2) placing the coal gasification residue sheet in a fixed bed reactor (a closed rotary kiln is used in this comparative example), heating the sheet to about 100°C at a heating rate of 15°C / h under air-tight conditions (i.e., under inert gas protection) and keeping the temperature for 2 hours to distill out water vapor, gaseous reactants (the gaseous reactants mainly include compound impurities containing O and / or S, etc.) and light hydrocarbons (in the form of hydrocarbon vapor); continuing to heat the sheet to below 400°C at a heating rate of 15°C / h to distill out the residual fuel fraction (in the form of hydrocarbon vapor); continuing to heat the sheet to 400°C-600°C at a heating rate of 15°C / h and keeping the temperature for 2 hours, so that the high-boiling-point macromolecular hydrocarbons in the coal gasification residue sheet undergo thermal conversion reaction and cracking to generate light hydrocarbons and distill them out (in the form of hydrocarbon vapor), and part of the residue is coked to generate coke, thereby obtaining a porous carbon sheet;
[0202] (3) in an air-tight condition (i.e., under the protection of an inert gas), the temperature is continuously raised to 1000° C. at a heating rate of 15° C. / h and kept at this temperature for 2 hours to sinter and graphitize the porous carbon sheet, and after cooling, a porous graphite electrode is obtained;
[0203] wherein the gaseous reactants and hydrocarbon vapors distilled out of the fixed bed reactor during the temperature increase process are transported to the oil and gas fractionation system for oil and gas fractionation;
[0204] The water vapor distilled from the fixed bed reactor during the heating process is condensed and sent to the sewage treatment system for treatment; after being treated by the sewage treatment system, clean water and sludge are obtained;
[0205] wherein, the clean water treated by the sewage treatment system is used to wash the screened coal gasification residue in step (1); the waste liquid obtained by washing the screened coal gasification residue is subjected to oil-water separation to obtain sewage and waste oil, the sewage is sent to the sewage treatment system for treatment, and the waste oil is sent to the oil-gas fractionation system for oil-gas fractionation;
[0206] wherein the purified water treated by the sewage treatment system is mixed with the coal gasification residue in step (1);
[0207] wherein the sludge obtained after treatment in the sewage treatment system is used as a raw material (counted in the coal gasification residue), mixed with the coal gasification residue, water, a dispersant, a foaming agent, a polymerization agent and a catalyst in step (1) and then molded to obtain a molded coal gasification residue;
[0208] (4) sending the liquefied gas obtained after the oil and gas fractionation system performs oil and gas fractionation to a liquefied gas storage tank for storage, and sending the hydrocarbon oil obtained after the oil and gas fractionation system performs oil and gas fractionation to a hydrocarbon oil storage tank for storage;
[0209] The raw materials stored in the hydrocarbon oil storage tank and the liquefied gas storage tank are used as auxiliary fuel for heating in step (2) and step (3); coal gasification residue scraps or a mixture of coal gasification residue scraps and coal are used as main fuel for heating in step (2) and step (3); and the waste gas generated by the combustion of the fuel during heating in the fixed bed reactor is discharged into the atmosphere after tail gas treatment (the main component is CO2).
[0210] The density of the porous graphite electrode prepared in this comparative example is 0.4 g / cm 3 , with a specific surface area of 100m 2 / g, and the average pore size is 4nm.
Claims
1. A method for preparing a porous graphite material produced from coal gasification residue, comprising the following steps: (1) mixing coal gasification residue with water, additives, a cross-linking agent, a dispersant, a foaming agent, a polymerization agent and a catalyst and molding the mixture to obtain a molded coal gasification residue; (2) heating the formed coal gasification residue to generate porous carbon; (3) sintering and cooling the porous carbon to obtain the porous graphite material; Wherein, the additive includes one or a combination of paraffin, light mineral oil and aromatic hydrocarbons; The crosslinking agent includes one or a combination of hydroxyethyl acrylate crosslinking agent, methacrylate crosslinking agent and blocked isocyanate crosslinking agent; The dispersant includes a turbid liquid formed by dispersing polyethylene glycol fatty acid ester in a solvent; The foaming agent includes one or a combination of waterborne polyurethane surfactants, carboxylic acid and salt surfactants, alkyl sulfonic acid and salt surfactants, phenolic surfactants and pyridine surfactants; The polymerization agent includes one or a combination of polyvinyl n-butyl ether, vinyl sulfite and vinyl ethylene carbonate; The catalyst comprises one or a combination of iron, nickel, titanium, silicon, carbides and oxides thereof.
2. The preparation method according to claim 1, wherein In step (1), the coal gasification residue is screened coal gasification residue, and the particle size of the screened coal gasification residue is less than 200 μm.
3. The preparation method according to claim 2, wherein In step (1), the coal gasification residue is screened by flotation.
4. The preparation method according to claim 1, wherein In step (1), the light mineral oil is a light mineral oil containing polycyclic aromatic hydrocarbons as main components.
5. The preparation method according to claim 1, wherein In step (1), the cross-linking agent includes polytriallyl isocyanurate.
6. The preparation method according to claim 1, wherein In step (1), the solvent in the dispersant includes water, mineral oil or vegetable oil.
7. The preparation method according to claim 1, wherein In step (1), the weight ratio of the coal gasification residue to water is (1-5):
10.
8. The preparation method according to claim 1, wherein In step (1), the weight ratio of the coal gasification residue to the additive is (2-5):
1.
9. The preparation method according to claim 1, wherein In step (1), the weight ratio of the coal gasification residue to the cross-linking agent is (3-6):
1.
10. The preparation method according to claim 1, wherein: In step (1), the weight ratio of the coal gasification residue to the dispersant is (80-110):
1.
11. The preparation method according to claim 1, wherein: In step (1), the weight ratio of the coal gasification residue to the foaming agent is (100-300):
1.
12. The preparation method according to claim 1, wherein: In step (1), the weight ratio of the coal gasification residue to the polymerization agent is (10-20):
1.
13. The preparation method according to claim 1, wherein In step (1), the weight ratio of the coal gasification residue to the catalyst is (4-10):
1.
14. The preparation method according to claim 1, wherein: In step (1), the formed coal gasification residue is a coal gasification residue sheet.
15. The preparation method according to claim 14, wherein: In step (1), the thickness of the coal gasification residue sheet is 1-2 mm.
16. The preparation method according to claim 1, wherein: Step (1) specifically comprises: screening the coal gasification residue and mixing it with water; then adding additives, crosslinking agents and dispersants to obtain a mixture; adding a foaming agent to the mixture to generate foam, then adding a polymerizing agent and a catalyst, injecting the mixture into a mold before forming a gel, and forming it into a sheet in the mold to obtain a coal gasification residue sheet.
17. The preparation method according to claim 16, wherein: In step (1), the coal gasification residue is screened, washed with water and then mixed with water.
18. The preparation method according to claim 1, wherein: In step (2), the formed coal gasification residue is heated to 100-150° C. and kept warm for 2-3 hours in an airtight condition, and then continued to be heated to 400-600° C. and kept warm for 1.5-2.5 hours.
19. The preparation method according to claim 1, wherein: In step (2), the porous carbon is a porous carbon sheet.
20. The preparation method according to claim 18, wherein: Step (2) specifically includes: The coal gasification residue pieces are heated to 100-150°C in an airtight condition and kept at this temperature for 2-3 hours to distill out water vapor, gaseous reactants and hydrocarbon vapor; Continue heating to 400-600°C and keep warm for 1.5-2.5 hours to make the high-boiling-point macromolecular hydrocarbons in the coal gasification residue pieces undergo thermal conversion reaction and cracking to generate light hydrocarbons which are distilled out in the form of hydrocarbon vapor. Part of the residue is coked to generate coke to obtain a porous carbon sheet.
21. The preparation method according to claim 20, wherein: Step (2) further comprises: subjecting the gaseous reactants and hydrocarbon vapor distilled out during the heating process of the coal gasification residue flakes to oil and gas fractionation and collecting them to obtain hydrocarbon oil and liquefied gas.
22. The preparation method according to claim 20, wherein: Step (2) further includes: condensing the water vapor distilled during the heating of the coal gasification residue pieces and sending it to a sewage treatment system for treatment.
23. The preparation method according to claim 1, wherein In step (3), the sintering temperature is 800-1500° C. and the sintering time is 2-5 hours.
24. The preparation method according to claim 1, wherein In step (3), the porous graphite material is a porous graphite sheet.
25. A porous graphite material produced from coal gasification residue, which is prepared by the method for preparing a porous graphite material produced from coal gasification residue according to any one of claims 1 to 24.
26. The porous graphite material according to claim 25, wherein: The density of the porous graphite material is 0.5-0.9 g / cm 3 .
27. The porous graphite material according to claim 25, wherein: The specific surface area of the porous graphite material is 150-400m 2 / g.
28. The porous graphite material according to claim 25, wherein: The pore size of the porous graphite material is 2-15 nm.
29. The porous graphite material according to claim 25, wherein: The porous graphite material is a porous graphite sheet.
30. Use of the porous graphite material produced from coal gasification residue according to any one of claims 25 to 29 as a graphite electrode.
31. The use according to claim 30, wherein: The application is: the porous graphite material is used as a graphite electrode in an electrolytic cell or a fuel cell.