Polyethylene composition, preparation method and application thereof, polyolefin microporous breathable film

By using maleic anhydride copolymer microspheres as porogen in the polyethylene breathable film, the porogen is evenly dispersed in the polyethylene matrix and solves the problems of uneven pore size distribution and poor dispersion caused by inorganic porogens. problem, improving the breathability uniformity and physical properties of the breathable membrane.

CN116063769BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111272418.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-10-15
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

Inorganic porogens in existing polyethylene breathable films have uneven particle size, poor dispersion, and poor compatibility, resulting in problems such as uneven pore size distribution, insufficient strength, and color difference, which affect the performance of the breathable film.

Method used

Maleic anhydride copolymer microspheres are used as the porogen. By uniformly dispersing in the polyethylene matrix, the use of coupling agents and dispersants is avoided to achieve uniform dispersion and high air permeability of the porogen.

Benefits of technology

It improves the air permeability uniformity and physical properties of the breathable membrane, solves the problems of uneven pore size distribution and poor dispersion, has wide adaptability, simple operation, and stable product performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116063769B_ABST
    Figure CN116063769B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of polyolefin compositions, and discloses a polyethylene composition and its preparation method and application. The composition includes polyethylene, a porogen and an antioxidant; based on 100 parts by weight of polyethylene, the amount of the porogen is 35-110 parts by weight, and the amount of the antioxidant composite auxiliary agent is 0.1-2 parts by weight; the porogen is maleic anhydride copolymer microspheres, and the average particle size of the maleic anhydride copolymer microspheres is 500-1600nm. The composition contains organic porogen maleic anhydride copolymer microspheres, and the copolymer microspheres have uniform particle size distribution, can be well dispersed in the polyethylene blend matrix without the use of coupling agents and dispersants, and no agglomeration phenomenon occurs, and the shortcomings of uneven pore size distribution, poor dispersibility, poor compatibility, etc. caused by inorganic porogens can be avoided. The composition is applied to a breathable film to improve the air permeability uniformity of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polyolefin compositions, in particular to a polyethylene composition and a preparation method and application thereof, and a polyolefin microporous breathable film. Background Art

[0002] Breathable film is also called "water-blocking breathable microporous film", which has the characteristics of being breathable but not water-permeable. It is a composite material with thermoplastic as the matrix and filled with a certain proportion of solid particles (such as calcium carbonate, barium sulfate, titanium dioxide, talcum powder and other mineral fillers). It is made into a film by methods such as blow molding, calendering or casting, and then uniaxial or biaxial stretching under appropriate conditions to obtain a microporous film material with smaller pores. Microporous breathable film can allow gases such as water vapor and air to pass through, while blocking liquids. It can be widely used in medical protective clothing, wound care bandages and dressings and other medical supplies, sanitary products such as baby diapers and adult care products, as well as food packaging and daily products. It is a new material that has developed rapidly in the past two decades.

[0003] In theory, all thermoplastics can be used as the base resin of breathable membrane materials, but from the perspective of the overall market value of microporous breathable membranes, polyethylene breathable membranes account for the largest share. Polyethylene has the advantages of abundant raw material sources, easy processing and molding, good film-forming effect, and comfortable and soft feel, and is widely used as the base resin of breathable membrane materials.

[0004] The sanitary products industry is the largest terminal market for polyethylene breathable membranes, so the safety and comfort of the breathable membranes must be taken into consideration. Therefore, very high quality requirements are placed on the porogens used in the preparation of polyethylene breathable membranes. Inorganic fillers, especially calcium carbonate, have become the preferred material for porogens due to their abundant resources, low prices, and good comprehensive performance. However, inorganic porogens have hydrophilic and oleophobic surfaces, are extremely polar, and have poor compatibility with polymer matrices, making them difficult to disperse evenly in the matrix. At the same time, the uniformity of the dispersion of the porogen in the matrix will affect the mechanical properties, surface flatness, uniformity of the pore size of the micropores, and porosity of the breathable membrane. In the traditional production process, surfactants are often used to pretreat inorganic fillers to increase their compatibility with the matrix, and coupling agents and dispersants are added to solve the dispersion problem of inorganic fillers.

[0005] CN102336940A discloses a composition of a low-permeability breathable film and a preparation method thereof, wherein the components include a polyolefin resin mixture, a permeability regulator, surface-modified micron-sized inorganic particles, an antioxidant, a lubricant and a coupling agent. The composition has the advantages that the micron-sized inorganic filler can improve the mechanical properties of the breathable film, and coupling modification of the surface of the inorganic particles can increase their compatibility with the polyolefin resin. However, the composition has the disadvantage that the micron-sized inorganic particles cannot be evenly dispersed in the matrix resin, thereby affecting the air permeability uniformity of the film.

[0006] CN1176986C discloses a preparation method of a special resin for polyolefin high permeability air-cast film, which is made of polyolefin resin (LDPE, LLDPE, copolymerized PP) and ultrafine mineral filler (calcium carbonate, talcum powder, etc., with a particle size of 3-10μm) as the main raw materials, and Ti-Al composite coupling agent, POE modifier, OPE dispersant are added, and the film is processed by coupling treatment, volume expansion dispersion, internal mixing and extrusion pelletizing. The special resin is processed by the casting and stretching process to produce uniform and fine pores between the mineral filler particles and the polyolefin in the film, and the polyolefin high permeability air-cast film is formed after cooling and crystallization. This method cannot effectively form holes and control the pore size, and uses an internal mixer, and the process is cumbersome and complicated.

[0007] CN101747548A discloses a composite material for preparing a high-strength polyolefin breathable membrane and a method thereof, the components of which include: polyolefin resin, micron- and nano-scale inorganic fillers, antioxidants, processing aids, and coupling agents. The nano-inorganic fillers can improve the mechanical properties of the polyolefin breathable membrane, reduce the thickness of the breathable membrane, and can prepare a high-strength and high-permeability breathable membrane by adjusting the process conditions; however, due to the poor compatibility of the nano-inorganic fillers with the polyolefin resin, the breathability of the material will be uneven, thereby affecting the use of the breathable membrane.

[0008] At present, inorganic porogens used in the production of breathable membranes on the market have the following problems: (1) they are easy to agglomerate; (2) due to the large particle size and uneven particle size distribution, the pore size uniformity of the breathable membrane is poor, and even a large number of pinhole defects appear; (3) the surface modification effect of the filler particles is poor, and the compatibility with the matrix is ​​poor, thus affecting the strength of the film; (4) the filler particles have poor dispersibility and will migrate to the surface of the breathable membrane, causing color difference or color spots on the breathable membrane. Summary of the invention

[0009] In order to overcome the problems existing in the prior art, the present invention provides a polyethylene composition, a preparation method and application thereof, and a polyolefin microporous breathable film. The composition contains organic porogen maleic anhydride copolymer microspheres, the particle size distribution of the copolymer microspheres is uniform, and can be well dispersed in the polyethylene matrix without using a coupling agent or a dispersant, without agglomeration, and can avoid the shortcomings of uneven pore size distribution, poor dispersibility, poor compatibility, etc. caused by inorganic porogens. The composition is applied to a breathable film to improve the air permeability uniformity of the product.

[0010] In order to achieve the above object, the first aspect of the present invention provides a polyethylene composition, characterized in that the composition comprises polyethylene, a porogen and an antioxidant;

[0011] Based on 100 parts by weight of polyethylene, the amount of the porogen is 35-110 parts by weight, and the amount of the antioxidant composite auxiliary is 0.1-2 parts by weight;

[0012] The porogen is maleic anhydride copolymer microspheres, and the average particle size of the maleic anhydride copolymer microspheres is 500-1600nm.

[0013] The second aspect of the present invention provides use of the polyethylene composition in a polyolefin microporous breathable membrane.

[0014] The third aspect of the present invention provides a method for preparing the above-mentioned polyethylene composition, characterized in that the method comprises:

[0015] (1) mixing polyethylene, a porogen and an antioxidant composite additive to obtain a mixture;

[0016] (2) The mixture is melt-blended, extruded, pelletized and dried in a twin-screw extruder to obtain the polyethylene composition.

[0017] A fourth aspect of the present invention provides a polyolefin microporous breathable membrane, characterized in that the microporous breathable membrane is made from the above polyethylene composition.

[0018] Through the above technical scheme, the polyethylene composition, preparation method and application thereof, and polyolefin microporous breathable film provided by the present invention achieve the following beneficial effects:

[0019] Maleic anhydride copolymer microspheres are added to the composition provided by the invention as a porogen, and the particle size distribution of the copolymer microspheres is uniform, and the porogen can be evenly dispersed in a polyethylene blend matrix without using a coupling agent or a dispersant, and the pore sizes of the micropores are uniform; the problem that the adjustable range of the physical properties and the air permeability of the breathable membrane in the prior art is small can be solved, and the invention has wide adaptability, simple operation, and stable product performance.

[0020] The polyethylene composition provided by the present invention can be widely used in the fields of disposable medical and sanitary products, water-blocking and moisture-permeable materials, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 is a SEM photograph of a cross section of a polyethylene composition sample obtained in Example 1;

[0022] Figure 2 is a SEM photograph of a cross section of a polyethylene composition sample obtained in Example 2;

[0023] Figure 3 is a SEM photograph of a cross section of a polyethylene composition sample obtained in Example 4;

[0024] Figure 4is a SEM photograph of a cross section of a polyethylene composition sample obtained in Example 5;

[0025] Figure 5 is a SEM photograph of a cross section of a polyethylene composition sample obtained in Comparative Example 1;

[0026] Figure 6 is a SEM photograph of a cross section of a polyethylene composition sample obtained in Comparative Example 2;

[0027] Figure 7 This is a SEM photograph of the cross section of the polyethylene composition sample prepared in Comparative Example 3. DETAILED DESCRIPTION

[0028] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0029] The first aspect of the present invention provides a polyethylene composition, characterized in that the composition comprises polyethylene, a porogen and an antioxidant;

[0030] Based on 100 parts by weight of polyethylene, the amount of the porogen is 35-110 parts by weight, and the amount of the antioxidant composite auxiliary is 0.1-2 parts by weight;

[0031] The porogen is maleic anhydride copolymer microspheres, and the average particle size of the maleic anhydride copolymer microspheres is 500-1600nm.

[0032] Maleic anhydride copolymer microspheres are added to the composition provided by the invention as a porogen, and the particle size distribution of the copolymer microspheres is uniform, and the porogen can be evenly dispersed in a polyethylene blend matrix without using a coupling agent or a dispersant, and the pore sizes of the micropores are uniform; the problem that the adjustable range of the physical properties and the air permeability of the breathable membrane in the prior art is small can be solved, and the invention has wide adaptability, simple operation, and stable product performance.

[0033] Furthermore, based on 100 parts by weight of polyethylene, the amount of the porogen is 50-100 parts by weight, and the amount of the antioxidant composite auxiliary is 0.1-1.5 parts by weight.

[0034] According to the present invention, the average particle size of the maleic anhydride copolymer microspheres is 600-1300 nm, preferably 600-1200 nm.

[0035] According to the present invention, the melting enthalpy of the polyethylene is ΔHmPE , the melting enthalpy of the polyethylene composition is ΔH m组合物 ;

[0036] Among them, △H mPE With △H m组合物 The difference is 10-45 J / g.

[0037] In the present invention, when the difference between the melting enthalpy of the polyethylene and the melting enthalpy of the polyethylene composition satisfies the above range, it can be shown that the maleic anhydride copolymer microspheres are evenly distributed in the polyethylene composition, and there is no significant decrease in the melting enthalpy of the composition due to agglomeration of the maleic anhydride copolymer microspheres, thereby making the breathable film made from the composition have both excellent physical properties and breathability.

[0038] In the present invention, the melting enthalpy of the polyethylene and the polyethylene composition is measured by differential scanning calorimetry.

[0039] Furthermore, △H mPE With △H m组合物 The difference is 20-45J / g.

[0040] According to the present invention, the copolymer in the maleic anhydride copolymer microspheres comprises a structural unit A derived from maleic anhydride and a structural unit B derived from a comonomer, and based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A is 48-55%, and the molar content of the structural unit B is 45-52%.

[0041] According to the present invention, the comonomer is selected from at least one of styrene, α-methylstyrene, vinyl acetate, mixed C4 and mixed C5.

[0042] In the present invention, the mixed C4 refers to a general term for hydrocarbon compounds with four carbon atoms (mainly including butene). Generally, in addition to butenes of various structures (such as trans-2-butene, cis-2-butene, normal butene, isobutene), the C4 also includes a certain amount of alkanes (such as normal butane) and other impurities that may exist. In the present invention, the content of olefins in the mixed C4 is within the range of 60-75% by weight.

[0043] In the present invention, the mixed C5 refers to a general term for hydrocarbon compounds with five carbon atoms (mainly including pentenes). Generally, in addition to various pentenes of different structures (such as dienes (isoprene, cyclopentadiene, 1,4-pentadiene, piperylene) and monoolefins (1-pentene, 2-pentene, cyclopentene, 2-methyl-1-butene, 2-methyl-2-butene)), the C5 also includes a certain amount of alkanes (such as n-pentane, isopentane, cyclopentane, 2-methylbutane), alkynes (such as butyne-2, 3-pentene-1yne) and other impurities that may exist. In the present invention, the content of olefins in the mixed C5 is 55-65% by weight.

[0044] According to the present invention, based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A is 48-53%, preferably 49-51%, and the molar content of the structural unit B is 47-52%, preferably 49-51%.

[0045] In one specific embodiment of the present invention, the porogen maleic anhydride copolymer microspheres are prepared according to the following steps:

[0046] (1) dissolving maleic anhydride, comonomer and initiator in a reaction medium in an inert atmosphere to form a homogeneous solution;

[0047] (2) the homogeneous solution is subjected to polymerization reaction to obtain a copolymer emulsion suspension, and then solid-liquid separation is performed to obtain the maleic anhydride copolymer microspheres;

[0048] Wherein, based on the total weight of maleic anhydride and the comonomer, the amount of maleic anhydride is 50-90wt%, and the amount of the comonomer is 10-50wt%;

[0049] The reaction medium is a mixture of the compound represented by formula (1) and an alkane;

[0050]

[0051] Among them, R 1 and R 2 Each is independently an alkyl group having 1 to 6 carbon atoms;

[0052] The comonomer is selected from at least one of styrene, α-methylstyrene and vinyl acetate.

[0053] In the present invention, maleic anhydride monomer and comonomer are copolymerized in a specific ratio, so that the prepared maleic anhydride copolymer is in the form of microspheres with excellent uniformity, and the copolymer has the characteristics of clean surface, good dispersibility in the medium and no aggregation.

[0054] Furthermore, in order to obtain maleic anhydride copolymer microspheres with uniform particles and excellent morphology, the inventors studied the dosage of maleic anhydride and comonomers during the polymerization process. The study showed that when the dosage of maleic anhydride is 50-60wt% and the dosage of the comonomer is 40-50wt% based on the total weight of the polymerized monomers, the obtained maleic anhydride copolymer microspheres have uniform particles, excellent particle morphology, and a clean particle surface, and the comprehensive performance of the copolymer microspheres is even better.

[0055] According to the present invention, based on the total weight of the homogeneous solution, the total mass concentration of the maleic anhydride and the comonomer is 5-25 wt %, preferably 5-20 wt %.

[0056] According to the present invention, based on the total weight of the homogeneous solution, the mass concentration of the initiator is 0.01-5wt%, preferably 1-4wt%.

[0057] According to the present invention, in formula (1), R 1 and R 2 Each is independently an alkyl group having 1 to 4 carbon atoms, more preferably a methyl group or an ethyl group.

[0058] According to the present invention, the alkane is an alkane having 6 to 12 carbon atoms.

[0059] In the present invention, a mixture of the compound represented by formula (1) and an alkane is selected as the reaction medium, which can cooperate with the specific amount of maleic anhydride and the comonomer described in the present invention to achieve a self-stabilizing precipitation polymerization reaction of maleic anhydride and the comonomer I. The polymerization reaction system does not need to add any stabilizer or co-stabilizer, has a self-stabilizing dispersion effect, and the surface of the obtained polymer microspheres is clean and pollution-free.

[0060] Furthermore, the alkane is at least one selected from hexane, heptane and octane, more preferably hexane.

[0061] According to the present invention, the amount of the alkane used is 50-90 vol%, preferably 60-80 vol%, based on the total volume of the reaction medium.

[0062] In the present invention, the polymerization reaction is carried out in an inert atmosphere, and the inert atmosphere can be provided by conventional inert gases in the prior art, such as nitrogen.

[0063] According to the present invention, the conditions of the polymerization reaction include: the polymerization temperature is 61-100° C., preferably 70-90° C.; the polymerization time is 1-24 h, preferably 2-12 h.

[0064] In one embodiment of the present invention, the porogen maleic anhydride copolymer microspheres are prepared according to the following steps:

[0065] In the presence of an inert atmosphere, an initiator and an organic solvent, maleic anhydride and a comonomer are copolymerized to obtain the maleic anhydride copolymer microspheres;

[0066] The comonomer is selected from mixed C4 and / or mixed C5.

[0067] In the present invention, the copolymerization reaction may be a one-step reaction using a precipitation polymerization method.

[0068] According to the present invention, the weight ratio of the maleic anhydride to the comonomer is 1:(0.2-3); preferably 1:(0.8-3).

[0069] According to the present invention, based on the total amount of maleic anhydride, the amount of the initiator is 0.05-20 mol%.

[0070] According to the present invention, the organic solvent is selected from at least one of isoamyl acetate, butyl acetate, isopropyl acetate and ethyl acetate. Preferably, based on the total weight of the organic solvent, the concentration of maleic anhydride is 5-25wt%; preferably 10-20wt%.

[0071] According to the present invention, the copolymerization reaction conditions are: copolymerization reaction temperature is 50-100°C, preferably 70-90°C; copolymerization reaction pressure is 0.2-2MPa, preferably 0.5-1MPa; copolymerization reaction time is 5-10h, preferably 6-9h.

[0072] According to the present invention, the initiator is an organic peroxide and / or an azo compound.

[0073] According to the present invention, the organic peroxide is at least one selected from dibenzoyl peroxide, diisopropyl peroxide, di-tert-butyl peroxide, dodecyl peroxide, tert-butyl perbenzoate, diisopropyl peroxydicarbonate and dicyclohexyl peroxydicarbonate.

[0074] According to the present invention, the azo compound is selected from azobisisobutyronitrile and / or azobisisoheptanenitrile.

[0075] In the present invention, a water bath and / or an oil bath is used to provide the heat required for the polymerization of the present invention.

[0076] In the present invention, the solid-liquid separation may be a conventional solid-liquid separation method in the art, such as centrifugal separation or flash separation.

[0077] In the present invention, when centrifugal separation is adopted, the centrifugal speed is 1500-5000 rad / min, and the centrifugal time is 5-60 min.

[0078] In the present invention, when flash separation is adopted, it can be carried out in a flash separator, the flash temperature is 10-40° C., and the flash pressure is 0 MPa.

[0079] According to the present invention, the polyethylene is linear low-density polyethylene and low-density polyethylene.

[0080] According to the present invention, based on 100 parts by weight of polyethylene, the amount of the linear low-density polyethylene is 60-99 parts by weight, preferably 70-95 parts by weight; the amount of the low-density polyethylene is 1-40 parts by weight, preferably 5-30 parts by weight.

[0081] According to the present invention, the linear low-density polyethylene is a copolymer of ethylene and α-olefin; preferably, the α-olefin is selected from at least one of butene, hexene and octene.

[0082] In the present invention, the linear low-density polyethylene is a linear low-density polyethylene prepared by catalysis with a Ziegler-Natta catalyst and / or a metallocene catalyst.

[0083] According to the present invention, the density of the linear low-density polyethylene is 0.905 g / cm 3 -0.935g / cm 3 .

[0084] According to the present invention, the melt flow rate of the linear low-density polyethylene at 190° C. and a load of 2.16 kg is 0.5 g / 10 min-10 g / 10 min, preferably 2 g / 10 min-6 g / 10 min.

[0085] According to the present invention, the molecular weight distribution of the linear low density polyethylene is 2-12, preferably 2-10.

[0086] According to the present invention, the density of the low-density polyethylene is 0.913 g / cm 3 -0.934g / cm 3 .

[0087] According to the present invention, the melt flow rate of the low-density polyethylene at 190° C. and a load of 2.16 kg is 0.1 g / 10 min-12 g / 10 min, preferably 2 g / 10 min-9 g / 10 min.

[0088] According to the present invention, the molecular weight distribution of the low-density polyethylene is 5-11, preferably 6-10.

[0089] According to the present invention, the polyethylene composition further comprises at least one selected from the following components: medium density polyethylene (MDPE), high density polyethylene (HDPE), ultra low density polyethylene (VLDPE), ultra high molecular weight polyethylene (HMWHDPE), polypropylene, propylene-based copolymers, ethylene-vinyl acetate copolymers, ethylene methyl acrylate copolymers, polyolefin plastomers, polyolefin elastomers and polybutene.

[0090] According to the present invention, the antioxidant composite auxiliary agent comprises an antioxidant and an acid absorbent.

[0091] According to the present invention, the weight ratio of the antioxidant to the acid scavenger is 1-6:1, preferably 2-5:1.

[0092] According to the present invention, the antioxidant is selected from at least one of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris(2,4-di-tert-butyl)phenyl phosphite, octadecyl propionate and alkylated polyphenols.

[0093] According to the present invention, the acid absorber is a stearate, preferably at least one selected from calcium stearate, zinc stearate and sodium stearate.

[0094] According to the present invention, the antioxidant composite auxiliary agent is a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), (2,4-di-tert-butylphenyl)trisphosphite and calcium stearate, wherein the weight ratio of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), (2,4-di-tert-butylphenyl)trisphosphite to calcium stearate is (1-3):(1-3):1, preferably (1-2):(1-2):1.

[0095] According to the present invention, the polyethylene composition does not contain coupling agent and dispersant.

[0096] The second aspect of the present invention provides use of the polyethylene composition in a polyolefin microporous breathable membrane.

[0097] In the present invention, the polyethylene composition is used to prepare a polyolefin microporous breathable film, which can significantly improve the physical properties and air permeability of the breathable film, and can be used in the fields of disposable medical and sanitary products, water-blocking and moisture-permeable materials, etc.

[0098] The third aspect of the present invention provides a method for preparing the above-mentioned polyethylene composition, characterized in that the method comprises:

[0099] (1) mixing polyethylene, a porogen and an antioxidant composite additive to obtain a mixture;

[0100] (2) The mixture is melt-blended, extruded, pelletized and dried in a twin-screw extruder to obtain the polyethylene composition.

[0101] According to the present invention, the rotation speed of the twin-screw extruder is 150-400 r / min, preferably 180-350 r / min.

[0102] According to the present invention, the temperatures of the feeding section, melting section, homogenizing section and die head of the twin-screw extruder are 150-180°C, 165-200°C, 180-215°C and 175-210°C respectively.

[0103] Preferably, the temperatures of the feeding section, melting section, homogenizing section and die head of the twin-screw extruder are 160-175°C, 175-190°C, 190-210°C and 180-205°C, respectively.

[0104] A fourth aspect of the present invention provides a polyolefin microporous breathable membrane, characterized in that the microporous breathable membrane is made from the above polyethylene composition.

[0105] In the present invention, the polyolefin microporous breathable film prepared from the above polyethylene composition not only retains the excellent physical properties of the polyethylene composition, but more importantly, the polyolefin microporous breathable film has high air permeability and can be used in the fields of disposable medical and sanitary products, water-blocking and moisture-permeable materials, etc.

[0106] In the present invention, there is no particular limitation on the preparation method of the polyolefin microporous breathable film, and a suitable method can be selected as needed, for example, the polyethylene composition is added to an extrusion casting machine for melting and casting, the extrusion temperature is 210-240°C, the cooling roller temperature is 20-60°C, and the polyethylene cast film is prepared. The cast film is uniaxially stretched 2-5 times to obtain a polyethylene microporous breathable film with an average thickness of 25-35 μm, and the heat setting temperature is 70-120°C.

[0107] The present invention will be described in detail below by way of examples. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention and are not intended to limit the present invention.

[0108] The relevant data in the present invention and its embodiments are obtained by the following test methods:

[0109] 1. The content of each structural unit in maleic anhydride copolymer microspheres is 1 H NMR was tested by 1 The content of each structural unit was calculated from the ratio of the peak area corresponding to the characteristic hydrogen in the corresponding structural unit in H NMR;

[0110] 2. Polymerization yield of maleic anhydride copolymer (Cp): Cp = Mp × 100% / Mm

[0111] Wherein, Mp is the mass of the obtained polymer; Mm is the total mass of the added monomers;

[0112] 3. Copolymer microsphere particle size test method: After the copolymer microsphere powder is vacuum sprayed with gold, the morphology is observed on a Hitachi S4800 field emission scanning electron microscope of Hitachi. 500 microspheres are selected from the electron microscope photos, and their diameters are measured. The average particle size of the microspheres is calculated by the mathematical average method.

[0113] 4. Conversion efficiency of mixed C4: weigh the polymer after the reaction, conversion efficiency (%) = [(4×actual mass of the obtained polymer) / (11×actual mass of C4 used)]×100%;

[0114] 5. Morphology of the cross section of the polyethylene composition sample and the dispersion of the porogen: The sample was soaked in liquid nitrogen for 15 minutes and then fractured. The cross section was treated with gold spraying. The cross section of the material was characterized by a Hitachi S4800 field emission scanning electron microscope to obtain microscopic morphology photos;

[0115] 6. Melt flow rate (MFR): measured at 190°C and 2.16 kg load according to the method specified in GB / T 3682-2000;

[0116] 7. Density: Determined by the density gradient column method specified in GB / T 1033.2-2010;

[0117] 8. Tensile properties: measured by the method specified in GB / T1040.3-2006 using a universal tensile testing machine.

[0118] 9. T C , Tm and △Hm: Differential scanning calorimeter was used to analyze the melting process and crystallization process of the material. The specific operation is: under nitrogen protection, 5-10 mg of sample was measured from 20℃ to 200℃ using a three-stage temperature rise and fall measurement method, and the change in heat flow reflects the melting and crystallization process of the material. The crystallization temperature T was calculated according to GB / T 19466.3-2004. C , melting temperature Tm and melting enthalpy △Hm.

[0119] 10. Water vapor transmission rate (WVTR): measured according to the method specified in GB / T 12704-1991.

[0120] The raw materials used in the examples and comparative examples are all commercially available.

[0121] Preparation Example 1

[0122] Preparation of porogen

[0123] 302.5g maleic anhydride, 51.3g azobisisobutyronitrile, 299.9g styrene, 1.462L acetone and 4.614L hexane (the amount of hexane is 75.9vol%) are added to a 20L reactor. After the materials are evenly mixed, nitrogen is passed through for 20 minutes, the reactor temperature is raised to 70°C, and the reaction is carried out for 6 hours. After the reaction is completed, the obtained polymer emulsion suspension is centrifuged at a speed of 2000rad / min for 20min by a centrifuge to obtain 542g of porogen maleic anhydride styrene copolymer microspheres A1, corresponding to a polymerization yield of 90%. In the polymerization monomer, the amount of maleic anhydride is 50.2wt%, the amount of styrene is 49.8wt%, and in the homogeneous solution, the mass concentration of maleic anhydride and comonomer is 12.4wt%, and the mass concentration of initiator is 1.06wt%.

[0124] The polymer microspheres 1 According to H NMR measurement, based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 49.5%, and the molar content of the structural unit B derived from styrene was 50.5%.

[0125] The average particle size of the porogen maleic anhydride copolymer microspheres A1 is about 1000 nm.

[0126] Preparation Example 2

[0127] The mass percentage of each component in the mixed C4 is as follows: 1,3-butadiene, 0.06%; trans-2-butene, 12.67%; isobutane, 37.09%; isobutylene, 19.48%; cis-2-butene, 27.79%; 1-butene, 1.02%; others, 1.89%. 13.5 kg of the mixed C4 composed above is introduced into a 200 L reactor containing 10 kg of maleic anhydride, 4 kg of dibenzoyl peroxide and 100 L of isoamyl acetate organic reaction liquid for free radical copolymerization, the copolymerization pressure is 1 MPa, the copolymerization temperature is 80 ° C, and the copolymerization time is 6 hours; the weight ratio of maleic anhydride to mixed C4 is 1:1.35. The concentration of maleic anhydride in the organic solvent is 10.2 wt%.

[0128] The copolymerization product was passed into a flash separator for gas-liquid separation at 30°C and 0 MPa, and the obtained liquid-solid mixture was further centrifuged in a centrifugal separator at 4000 rad / min for 20 min to obtain a solid product, and the liquid was returned to the reactor. The solid product was then washed with hexane, and the filter cake obtained by suction filtration through a sand core funnel was vacuum dried at 90°C for 8 hours to obtain 20.5 kg of maleic anhydride-mixed C4 copolymer A2.

[0129] The porogen maleic anhydride-mixed C4 copolymer A2 was subjected to 1H NMR measurement, and the results showed that based on the total molar amount of each structural unit in the polymer, the molar content of structural unit A derived from maleic anhydride was 49 mol%; the molar content of structural unit B derived from mixed C4 was 51 mol%, and the conversion efficiency of mixed C4 calculated by weight method was 55wt%.

[0130] The average particle size of the maleic anhydride-mixed C4 copolymer microspheres is about 1200 nm.

[0131] Preparation Example 3

[0132] Preparation of porogen

[0133] 376.4g maleic anhydride, 48.8g azobisisobutyronitrile, 256.6g styrene, 1.165L acetone and 4.614L hexane (the amount of hexane is 79.8vol%) are added to a 20L reactor. After the materials are evenly mixed, nitrogen is passed through for 20 minutes, the reactor temperature is raised to 70°C, and the reaction is performed for 8h. After the reaction is completed, the obtained polymer emulsion suspension is centrifuged at a speed of 2000rad / min for 20min by a centrifuge to obtain porogen maleic anhydride styrene copolymer microspheres A3493g, corresponding to a polymerization yield of 78%. In the polymerization monomer, the amount of maleic anhydride is 59.5wt%, the amount of styrene is 40.5wt%, the mass concentration of maleic anhydride and comonomer in the homogeneous solution is 13.6wt%, and the mass concentration of initiator is 1.1wt%.

[0134] The polymer microspheres 1 According to H NMR measurement, based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 48%, and the molar content of the structural unit B derived from styrene was 52%.

[0135] The average particle size of the porogen maleic anhydride copolymer microspheres A3 is about 1200 nm.

[0136] Preparation Example 4

[0137] Preparation of porogen

[0138] 262.6g maleic anhydride, 51.3g azobisisobutyronitrile, 235.1g styrene, 1.253L acetone and 4.614L hexane (the amount of hexane is 78.6vol%) are added to a 20L reactor. After the materials are evenly mixed, nitrogen is passed through for 20min, the reactor temperature is raised to 70°C, and the reaction is carried out for 5h. After the reaction is completed, the obtained polymer emulsion suspension is centrifuged at a speed of 2000rad / min for 20min by a centrifuge to obtain 4438g of porogen maleic anhydride copolymer microspheres A, corresponding to a polymerization yield of 88%. In the polymerization monomer, the amount of maleic anhydride is 52.8wt%, the amount of styrene is 47.2wt%, and in the homogeneous solution, the mass concentration of maleic anhydride and comonomer is 10.9wt%, and the mass concentration of initiator is 1.1wt%.

[0139] The polymer microspheres were subjected to 1H NMR measurement, and it was found that based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 49%, and the molar content of the structural unit B derived from styrene was 51%.

[0140] The average particle size of the porogen maleic anhydride copolymer microspheres A4 is about 700 nm.

[0141] Preparation Example 5

[0142] 124.6g maleic anhydride, 51.3g azobisisobutyronitrile, 129.9g styrene, 2.307L acetone and 2.645L hexane (the amount of hexane is 53.4vol%) are added to a 20L reactor. After the materials are evenly mixed, nitrogen is passed through for 20min, the reactor temperature is raised to 70°C, and the reaction is carried out for 4h. After the reaction is completed, the obtained polymer emulsion suspension is centrifuged at a speed of 2000rad / min for 20min by a centrifuge to obtain porogen maleic anhydride copolymer microspheres A5 191g, corresponding to a polymer yield of 75%. In the polymerization monomer, the amount of maleic anhydride is 49.0wt%, the amount of styrene is 51.0wt%, the mass concentration of maleic anhydride and comonomer in the homogeneous solution is 6.6wt%, and the mass concentration of initiator is 1.3wt%.

[0143] The polymer microspheres 1 According to H NMR measurement, based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A derived from maleic anhydride was 47%, and the molar content of the structural unit B derived from styrene was 53%.

[0144] The average particle size of the porogen maleic anhydride copolymer microspheres A5 is about 460 nm.

[0145] Example 1

[0146] Preparation of polyethylene compositions

[0147] 90 parts of linear low-density polyethylene (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution is 4) and 10 parts of low-density polyethylene (MFR is 7.5g / 10min, density is 0.919g / cm 3 , molecular weight distribution is 7.2), 70 parts of porogen A1, and 1 part of antioxidant composite auxiliary agent are blended in a high-speed mixer, wherein the antioxidant composite auxiliary agent is selected from pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, (2,4-di-tert-butylphenyl) triester phosphite and calcium stearate in a weight ratio of 2:2:1.

[0148] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The screw speed was 200 r / min, and the temperatures of the feed section, melting section, homogenization section and die head were 170°C, 180°C, 200°C and 190°C, respectively, to obtain a polyethylene composition. The obtained polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. The polyethylene composition was melted and pressed at 200°C, and the thickness of the sample was 120-160 μm. Figure 1 is a SEM photo of the cross section of the polyethylene composition sample. Figure 1 It can be seen that the porogen particle size is uniform and evenly distributed in the polyethylene matrix.

[0149] Example 2

[0150] Preparation of polyethylene compositions

[0151] 90 parts of linear low-density polyethylene (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution is 4) and 10 parts of low-density polyethylene (MFR is 7.5g / 10min, density is 0.919g / cm 3 , molecular weight distribution is 7.2), 100 parts of porogen A1 and 1 part of antioxidant composite auxiliary agent are blended in a high-speed mixer, wherein the weight ratio of the antioxidant selected is 2:2:1 of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, (2,4-di-tert-butylphenyl)triphosphite and calcium stearate.

[0152] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The screw speed was 200 r / min, and the temperatures of the feed section, melting section, homogenization section and die head were 170°C, 180°C, 200°C and 190°C, respectively, to obtain a polyethylene composition. The obtained polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. The polyethylene composition was melted and pressed into sheets at 200°C, and the thickness of the sample sheet was 120-160 μm. Figure 2 is a SEM photo of the cross section of the polyethylene composite sample. Figure 2 It can be seen that the porogen particle size is uniform and evenly distributed in the polyethylene matrix.

[0153] Example 3

[0154] Preparation of polyethylene compositions

[0155] 75 parts of linear low-density polyethylene (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution is 4) and 25 parts of low-density polyethylene (MFR is 7.5g / 10min, density is 0.919g / cm 3 , molecular weight distribution is 7.2), 85 parts of porogen A2, and 1 part of antioxidant composite auxiliary agent are blended in a high-speed mixer, wherein the weight ratio of the antioxidant selected from pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, (2,4-di-tert-butylphenyl)triphosphite and calcium stearate is 2:2:1.

[0156] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The speed of the screw was 200 r / min, and the temperatures of the feed section, melting section, homogenization section and die head were 170° C., 180° C., 200° C. and 190° C., respectively, to obtain a polyethylene composition. The obtained polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1.

[0157] Example 4

[0158] Preparation of polyethylene compositions

[0159] 75 parts of linear low-density polyethylene (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution is 4) and 25 parts of low-density polyethylene (MFR is 7.5g / 10min, density is 0.919g / cm 3, molecular weight distribution is 7.2), 100 parts of porogen A3 and 1 part of antioxidant composite auxiliary agent are blended in a high-speed mixer, wherein the weight ratio of the antioxidant selected is 2:2:1 of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, (2,4-di-tert-butylphenyl)triphosphite and calcium stearate.

[0160] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The screw speed was 200 r / min, and the temperatures of the feed section, melting section, homogenization section and die head were 170°C, 180°C, 200°C and 190°C, respectively, to obtain a polyethylene composition. The obtained polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. The polyethylene composition was melted and pressed into sheets at 200°C, and the thickness of the sample sheet was 120-160 μm. Figure 3 is a SEM photo of the cross section of the polyethylene composite sample. Figure 3 It can be seen that the porogen particle size is uniform and evenly distributed in the polyethylene matrix.

[0161] Example 5

[0162] Preparation of polyethylene compositions

[0163] 90 parts of linear low-density polyethylene (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution is 4) and 10 parts of low-density polyethylene (MFR is 7.5g / 10min, density is 0.919g / cm 3 , molecular weight distribution is 7.2), 45 parts of porogen A4, and 1 part of antioxidant composite auxiliary agent are blended in a high-speed mixer, wherein the weight ratio of the antioxidant selected from pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, (2,4-di-tert-butylphenyl)triphosphite and calcium stearate is 2:2:1.

[0164] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The screw speed was 200 r / min, and the temperatures of the feed section, melting section, homogenization section and die head were 170°C, 180°C, 200°C and 190°C, respectively, to obtain a polyethylene composition. The obtained polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. The polyethylene composition was melted and pressed at 200°C, and the thickness of the sample was 120-160 μm. Figure 4 is a SEM photo of the cross section of the polyethylene composite sample. Figure 4 It can be seen that the porogen particle size is uniform and evenly distributed in the polyethylene matrix.

[0165] Comparative Example 1

[0166] Preparation of polyethylene compositions

[0167] 90 parts of linear low-density polyethylene (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution is 4) and 10 parts of low-density polyethylene (MFR is 7.5g / 10min, density is 0.919g / cm 3 , molecular weight distribution is 7.2), 25 parts of porogen A1, and 1 part of antioxidant composite auxiliary agent are blended in a high-speed mixer, wherein the weight ratio of the antioxidant selected is 2:2:1 of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, (2,4-di-tert-butylphenyl)triphosphite and calcium stearate.

[0168] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The screw speed was 200 r / min, and the temperatures of the feed section, melting section, homogenization section and die head were 170°C, 180°C, 200°C and 190°C, respectively, to obtain a polyethylene composition. The obtained polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. The polyethylene composition was melted and pressed at 200°C, and the thickness of the sample was 120-160 μm. Figure 5 is a SEM photo of the cross section of the polyethylene composite sample. Figure 5 It can be seen that the porogen particle size is uniform, but the number is small and the distribution is uneven.

[0169] Comparative Example 2

[0170] 90 parts of linear low-density polyethylene (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution is 4) and 10 parts of low-density polyethylene (MFR is 7.5g / 10min, density is 0.919g / cm 3 , molecular weight distribution is 7.2), 100 parts of nano-CaCO 3 Powder (Shanghai Yuanjiang Chemical Co., Ltd., 10000 mesh) and 1 part of antioxidant composite auxiliary agent are blended in a high-speed mixer, wherein the antioxidant selected is pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), (2,4-di-tert-butylphenyl)triphosphite and calcium stearate in a weight ratio of 2:2:1.

[0171] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The screw speed was 200 r / min, and the temperatures of the feed section, melting section, homogenization section and die head were 170°C, 180°C, 200°C and 190°C, respectively, to obtain a polyethylene composition. The obtained polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. The polyethylene composition was melted and pressed at 200°C, and the thickness of the sample was 120-160 μm. Figure 6This is a SEM photograph of the cross section of the polyethylene composition sample, where it can be seen that the porogen is obviously aggregated.

[0172] Comparative Example 3

[0173] 90 parts of linear low-density polyethylene (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution is 4) and 10 parts of low-density polyethylene (MFR is 7.5g / 10min, density is 0.919g / cm 3 , molecular weight distribution is 7.2), 100 parts of nano BaSO 4 Powder (Sahliben Blanc FixeMicro, organic coating, d50 = 0.7 μm) and 1 part of antioxidant composite auxiliary agent are blended in a high-speed mixer, wherein the antioxidant selected is pentaerythritol tetrakis (β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate), (2,4-di-tert-butylphenyl) triester phosphite and calcium stearate in a weight ratio of 2:2:1.

[0174] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The speed of the screw was 200 r / min, and the temperatures of the feed section, melting section, homogenization section and die head were 170° C., 180° C., 200° C. and 190° C., respectively, to obtain the polyethylene composition of the present invention. The obtained polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1. The polyethylene composition was melted and pressed into sheets at 200° C., and the thickness of the sample sheet was 120-160 μm. Figure 7 This is a SEM photograph of the cross section of the polyethylene composition sample, where it can be seen that the porogen is obviously aggregated.

[0175] Comparative Example 4

[0176] Preparation of polyethylene compositions

[0177] 90 parts of linear low-density polyethylene (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution is 4) and 10 parts of low-density polyethylene (MFR is 7.5g / 10min, density is 0.919g / cm 3 , molecular weight distribution is 7.2), 140 parts of porogen A1, and 1 part of antioxidant composite auxiliary agent are blended in a high-speed mixer, wherein the antioxidant composite auxiliary agent is selected from pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, (2,4-di-tert-butylphenyl)triphosphite and calcium stearate in a weight ratio of 2:2:1.

[0178] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The speed of the screw was 200 r / min, and the temperatures of the feed section, melting section, homogenization section and die head were 170° C., 180° C., 200° C. and 190° C., respectively, to obtain a polyethylene composition. The obtained polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1.

[0179] Comparative Example 5

[0180] Preparation of polyethylene compositions

[0181] 90 parts of linear low-density polyethylene (MFR 3.5 g / 10 min, density 0.917 g / cm 3 , molecular weight distribution is 4) and 10 parts of low-density polyethylene (MFR is 7.5g / 10min, density is 0.919g / cm 3 , molecular weight distribution is 7.2), 70 parts of porogen A5 and 1 part of antioxidant composite auxiliary agent are blended in a high-speed mixer, wherein the antioxidant composite auxiliary agent is selected from pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, (2,4-di-tert-butylphenyl) triester phosphite and calcium stearate in a weight ratio of 2:2:1.

[0182] After being mixed evenly, the mixture was added to a twin-screw extruder for melt blending and extrusion granulation. The speed of the screw was 200 r / min, and the temperatures of the feed section, melting section, homogenization section and die head were 170° C., 180° C., 200° C. and 190° C., respectively, to obtain a polyethylene composition. The obtained polyethylene composition was dried. The properties of the polyethylene composition are shown in Table 1.

[0183] Table 1

[0184]

[0185] It can be seen from Table 1 that the melt flow rate (MFR) of the polyethylene composition provided by the present invention meets the requirements of the casting process, and ΔH mPE With △H m组合物 When the difference meets the range of the present invention, it indicates that the maleic anhydride copolymer microspheres in the composition are evenly distributed in the composition, so that the composition also has good mechanical properties and can meet the requirements of the stretching ratio of the breathable film.

[0186] Test Case

[0187] The polyethylene compositions of the examples and comparative examples were added to an extrusion casting machine for melting and casting, the extrusion temperature was 210-240°C, the cooling roller temperature was 20-60°C, and a polyethylene cast film was prepared. The cast film was subjected to 3 times uniaxial stretching to obtain a polyethylene microporous breathable film with an average thickness of 30 μm, and the heat setting temperature was 85°C. The properties of the polyethylene microporous breathable film are shown in Table 2.

[0188] Table 2

[0189]

[0190]

[0191] As can be seen from Table 2, the present invention significantly improves the uniformity of the dispersion of the porogen in the matrix resin by reasonably selecting an organic porogen with uniform particles and a polyolefin matrix resin without using a coupling agent and a dispersant, so that the prepared breathable film has high air permeability. The polyethylene breathable film prepared in the embodiment of the present invention has high air permeability and can be widely used in the fields of disposable medical and sanitary products, water-blocking and moisture-permeable materials, etc.

[0192] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A polyethylene composition, characterized in that The composition comprises polyethylene, a porogen and an antioxidant composite auxiliary agent; Based on 100 parts by weight of polyethylene, the amount of the porogen is 35-110 parts by weight, and the amount of the antioxidant composite auxiliary is 0.1-2 parts by weight; The porogen is maleic anhydride copolymer microspheres, and the average particle size of the maleic anhydride copolymer microspheres is 500-1600nm; The copolymer in the maleic anhydride copolymer microspheres comprises a structural unit A derived from maleic anhydride and a structural unit B derived from a comonomer; based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A is 48-55%, and the molar content of the structural unit B is 45-52%; The comonomer is selected from at least one of styrene, α-methylstyrene, vinyl acetate, mixed C4 and mixed C5.

2. The polyethylene composition according to claim 1, wherein Based on 100 parts by weight of polyethylene, the amount of the porogen is 50-100 parts by weight, and the amount of the antioxidant composite auxiliary is 0.1-1.5 parts by weight.

3. The polyethylene composition according to claim 1, wherein The average particle size of the maleic anhydride copolymer microspheres is 600-1300 nm.

4. The polyethylene composition according to claim 1, wherein The melting enthalpy of the polyethylene is △ H mPE , the melting enthalpy of the polyethylene composition is △ H m组合物 ; in, △ H mPE and △ H m组合物 The difference is 10-45 J / g.

5. The polyethylene composition according to claim 4, wherein △ H mPE and △ H m组合物 The difference is 20-45J / g.

6. The polyethylene composition according to claim 1, wherein Based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A is 49-51%, and the molar content of the structural unit B is 49-51%.

7. The polyethylene composition according to any one of claims 1 to 6, wherein The porogen maleic anhydride copolymer microspheres are prepared according to the following steps: (1) In an inert atmosphere, maleic anhydride, comonomer and initiator are dissolved in a reaction medium to form a homogeneous solution; (2) the homogeneous solution is polymerized to obtain a copolymer emulsion suspension, and then the maleic anhydride copolymer microspheres are obtained after solid-liquid separation; Wherein, based on the total weight of maleic anhydride and the comonomer, the amount of maleic anhydride is 50-90wt%, and the amount of the comonomer is 10-50wt%; The reaction medium is a mixture of the compound represented by formula (1) and an alkane; Formula (1), Wherein, R1 and R2 are each independently an alkyl group having 1 to 6 carbon atoms.

8. The polyethylene composition according to claim 7, wherein The comonomer is selected from at least one of styrene, α-methylstyrene and vinyl acetate.

9. The polyethylene composition according to claim 7, wherein Based on the total weight of the homogeneous solution, the mass concentration of the comonomer is 5-25wt%.

10. The polyethylene composition according to claim 9, wherein Based on the total weight of the homogeneous solution, the mass concentration of the comonomer is 5-20wt%.

11. The polyethylene composition according to claim 7, wherein Based on the total weight of the homogeneous solution, the mass concentration of the initiator is 0.01-5wt%.

12. The polyethylene composition according to claim 11, wherein Based on the total weight of the homogeneous solution, the mass concentration of the initiator is 1-4wt%.

13. The polyethylene composition according to claim 7, wherein Based on the total weight of maleic anhydride and the comonomer, the amount of maleic anhydride used is 50-60wt%, and the amount of the comonomer used is 40-50wt%.

14. The polyethylene composition according to claim 7, wherein In formula (1), R1 and R2 are each independently a methyl group or an ethyl group.

15. The polyethylene composition according to claim 7, wherein The alkane is an alkane having 6 to 12 carbon atoms.

16. The polyethylene composition according to claim 7, wherein The alkane is used in an amount of 50-90 vol% based on the total volume of the reaction medium.

17. The polyethylene composition according to claim 16, wherein The alkane is used in an amount of 60-80 vol% based on the total volume of the reaction medium.

18. The polyethylene composition according to claim 7, wherein The polymerization reaction conditions include: polymerization temperature of 61-100° C.; polymerization time of 1-24 h.

19. The polyethylene composition according to claim 18, wherein The polymerization reaction conditions include: polymerization temperature of 70-90° C.; polymerization time of 2-12 h.

20. The polyethylene composition according to any one of claims 1 to 6, wherein: The preparation method of the porogen maleic anhydride copolymer microspheres comprises the following steps: In the presence of an inert atmosphere, an initiator and an organic solvent, maleic anhydride and a comonomer are copolymerized to obtain the maleic anhydride copolymer microspheres.

21. The polyethylene composition according to claim 20, wherein The comonomer is selected from mixed C4 and / or mixed C5.

22. The polyethylene composition according to claim 20, wherein The weight ratio of the maleic anhydride to the comonomer is 1:(0.2-3).

23. The polyethylene composition according to claim 22, wherein The weight ratio of the maleic anhydride to the comonomer is 1:(0.8-3).

24. The polyethylene composition according to claim 20, wherein Based on the total amount of maleic anhydride used, the amount of the initiator used is 0.05-20 mol%.

25. The polyethylene composition according to claim 20, wherein The organic solvent is selected from at least one of isoamyl acetate, butyl acetate, isopropyl acetate and ethyl acetate.

26. The polyethylene composition according to claim 20, wherein Based on the total weight of the organic solvent, the concentration of the maleic anhydride is 5-25wt%.

27. The polyethylene composition according to claim 26, wherein Based on the total weight of the organic solvent, the concentration of the maleic anhydride is 10-20wt%.

28. The polyethylene composition according to claim 20, wherein The copolymerization reaction conditions include: copolymerization reaction temperature of 50-100° C.; copolymerization reaction pressure of 0.2-2 MPa; and copolymerization reaction time of 5-10 h.

29. The polyethylene composition according to claim 28, wherein The copolymerization reaction conditions include: copolymerization reaction temperature of 70-90° C.; copolymerization reaction pressure of 0.5-1 MPa; and copolymerization reaction time of 6-9 h.

30. The polyethylene composition of claim 1, wherein: The polyethylene is linear low density polyethylene and low density polyethylene.

31. The polyethylene composition according to claim 30, wherein Based on 100 parts by weight of polyethylene, the amount of the linear low-density polyethylene is 60-99 parts by weight; the amount of the low-density polyethylene is 1-40 parts by weight.

32. The polyethylene composition according to claim 30, wherein Based on 100 parts by weight of polyethylene, the amount of the linear low-density polyethylene is 70-95 parts by weight; the amount of the low-density polyethylene is 5-30 parts by weight.

33. The polyethylene composition according to claim 30, wherein: The linear low-density polyethylene is a copolymer of ethylene and α-olefin.

34. The polyethylene composition according to claim 33, wherein The α-olefin is at least one selected from butene, hexene and octene.

35. The polyethylene composition of claim 30, wherein: The density of the linear low-density polyethylene is 0.905 g / cm 3 -0.935g / cm 3 .

36. The polyethylene composition of claim 30, wherein: The linear low-density polyethylene has a melt flow rate of 0.5 g / 10 min to 10 g / 10 min at 190° C. and a load of 2.16 kg.

37. The polyethylene composition according to claim 36, wherein The linear low-density polyethylene has a melt flow rate of 2 g / 10 min to 6 g / 10 min at 190° C. and a load of 2.16 kg.

38. The polyethylene composition of claim 30, wherein: The molecular weight distribution of the linear low density polyethylene is 2-12.

39. The polyethylene composition according to claim 38, wherein The molecular weight distribution of the linear low density polyethylene is 2-10.

40. The polyethylene composition of claim 30, wherein: The density of the low-density polyethylene is 0.913 g / cm 3 -0.934g / cm 3 .

41. The polyethylene composition of claim 30, wherein: The low-density polyethylene has a melt flow rate of 0.1 g / 10 min to 12 g / 10 min at 190° C. and a load of 2.16 kg.

42. The polyethylene composition of claim 41, wherein The low-density polyethylene has a melt flow rate of 2 g / 10 min to 9 g / 10 min at 190° C. and a load of 2.16 kg.

43. The polyethylene composition of claim 30, wherein: The molecular weight distribution of the low-density polyethylene is 5-11.

44. The polyethylene composition of claim 43, wherein The molecular weight distribution of the low-density polyethylene is 6-10.

45. The polyethylene composition of claim 30, wherein: The polyethylene composition further comprises at least one selected from the following components: medium density polyethylene, high density polyethylene, ultra low density polyethylene, ultra high molecular weight polyethylene, polypropylene, propylene-based copolymers, ethylene-vinyl acetate copolymers, ethylene methyl acrylate copolymers, polyolefin plastomers, polyolefin elastomers and polybutylene.

46. ​​The polyethylene composition of claim 1, wherein: The antioxidant composite auxiliary agent comprises an antioxidant and an acid absorbent.

47. The polyethylene composition of claim 46, wherein The weight ratio of the antioxidant to the acid scavenger is 1-6:

1.

48. The polyethylene composition of claim 46, wherein The antioxidant is at least one selected from pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris(2,4-di-tert-butyl)phenyl phosphite, octadecyl propionate and alkylated polyphenols.

49. The polyethylene composition of claim 46, wherein: The acid absorbent is stearate.

50. The polyethylene composition of claim 49, wherein The acid absorber is selected from at least one of calcium stearate, zinc stearate and sodium stearate.

51. The polyethylene composition of claim 46, wherein: The antioxidant composite auxiliary agent is a mixture of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), (2,4-di-tert-butylphenyl)trisphosphite and calcium stearate, wherein the weight ratio of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), (2,4-di-tert-butylphenyl)trisphosphite to calcium stearate is (1-3):(1-3):

1.

52. The polyethylene composition of claim 1, wherein: The polyethylene composition does not contain coupling agent and dispersant.

53. Use of the polyethylene composition according to any one of claims 1 to 52 in a polyolefin microporous breathable film.

54. A method for preparing the polyethylene composition according to any one of claims 1 to 52, characterized in that: The method comprises: (1) mixing polyethylene, a porogen and an antioxidant composite additive to obtain a mixture; (2) The mixture is melt-blended, extruded, pelletized and dried in a twin-screw extruder to obtain the polyethylene composition.

55. The preparation method according to claim 54, wherein The rotation speed of the twin-screw extruder is 150-400 r / min.

56. The preparation method according to claim 54, wherein The temperatures of the feeding section, melting section, homogenizing section and die head of the twin-screw extruder are 150-180° C., 165-200° C., 180-215° C. and 175-210° C. respectively.

57. A polyolefin microporous breathable membrane, characterized in that: The microporous breathable membrane is made from the polyethylene composition described in any one of claims 1-52.