A green, safe and efficient method for recovering lithium and fluorine resources from electrolyte and its application

Efficient recovery of lithium and fluorine resources in lithium-ion battery electrolytes through wet processes solves the problems of high equipment requirements and waste of fluorine resources in the existing technology, and achieves high-purity recovery and green and environmentally friendly lithium-ion battery electrolyte treatment.

CN116081654BActive Publication Date: 2024-10-29SHAOXING DONGYUAN NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310067662.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-13
Publication Date
2024-10-29
Estimated Expiration
2043-01-13

AI Technical Summary

Technical Problem

The existing technology has high equipment requirements, complex processes, waste of fluorine resources and potential safety hazards for personnel when recycling lithium resources in lithium-ion battery electrolytes, making it difficult to achieve efficient and green recovery of lithium and fluorine resources.

Method used

Using a wet process, the electrolyte containing fluorine lithium compounds is mixed with a strong alkali solution, and through evaporation and solid-liquid separation steps, lithium and fluorine resources are recovered respectively, using low equipment requirements and simple processes to avoid the use of toxic and hazardous substances and Equipment corrosion.

Benefits of technology

It achieves 85% recovery rate of lithium resources and 90% recovery rate of fluorine resources. The product has high purity and avoids the generation of HF and equipment corrosion. The process is low energy consumption, environmentally friendly, and suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116081654B_ABST
    Figure CN116081654B_ABST
Patent Text Reader

Abstract

The present invention discloses a green, safe and efficient method for recovering lithium and fluorine resources in electrolyte and its application, comprising the following steps: mixing an electrolyte containing fluorine-lithium compounds with a strong alkaline solution; evaporating the obtained mixed solution to remove the liquid, and then fully mixing the obtained solid with water to separate the solid and liquid to obtain a solid recovery LiF; evaporating the liquid separation to remove the liquid, adding the obtained solid to an organic solvent, and then fully mixing to separate the solid and liquid, and repeatedly mixing and separating the obtained solid separation with the organic solvent to obtain a solid recovery NaF; the present invention proposes for the first time a method for recovering lithium and fluorine resources in an electrolyte using a strong alkali as an auxiliary, with a simple process flow, low recovery cost, and suitable for large-scale industrial production. In addition, the recovered sample has high purity and can be used again in the preparation of lithium battery electrodes and electrolyte materials, which improves the resource recycling rate to a certain extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of recycling and reusing lithium and fluorine resources in lithium-ion battery electrolytes, and specifically relates to a method for green, safe and efficient recovery of lithium and fluorine resources in electrolytes by a wet process and its application. Background Art

[0002] Lithium-ion batteries (LIBs) have been widely used as important energy storage and conversion devices in recent years due to their high voltage, high energy density, and good cycle stability. It is expected that in the next few years, with the expansion of the market and the growth of productivity, the application of LIBs will increase accordingly, which will lead to a continuous increase in waste LIBs. Waste LIBs contain a large number of reusable resources, and reasonable recycling can improve the reuse rate of resources. Therefore, efficient recycling of waste batteries is imperative.

[0003] At present, the recycling of lithium-ion batteries is mainly focused on the recycling of high-value cathode heavy metal resources, but there are few reports on the recycling of lithium resources in batteries, especially lithium resources in electrolytes. At present, due to the high ionic conductivity and good electrochemical stability of lithium hexafluorophosphate (LiPF6), most commercial LIBs use organic electrolytes based on LiPF6. However, when recycling lithium resources in such electrolytes, acidic substances such as POF3, PF5 and HF are easily formed, which poses great risks to human health, the environment and the stability of the recycling process equipment, thus making it more difficult and costly to recover lithium resources from the electrolyte.

[0004] At present, there are few studies on the recycling and reuse of lithium resources in waste lithium-ion battery electrolytes at home and abroad. Patent document CN111934041A discloses a method for recycling and reusing waste lithium-ion battery electrolytes, including recycling and reusing through a recycling device, separating lithium ions in the form of lithium fluoride crystals, and treating the generated toxic mixed gas. Patent document CN107910610A discloses a method for mixing and recycling the positive electrode and electrolyte of a lithium battery, mixing the positive electrode material of the battery with the electrolyte in hot water, and dissolving the positive electrode material by hydrolyzing the lithium hexafluorophosphate in the electrolyte to produce hydrofluoric acid, so as to achieve simultaneous recycling of the positive electrode material and the battery electrolyte. Patent document CN104852102A discloses another method and device for resource utilization and harmless treatment of waste lithium-ion battery electrolyte. After discharging the waste lithium-ion battery, the battery core is retained and immersed in a heated reaction tank. A small amount of water is added to the reaction solution, and lithium phosphate is added at the same time. Hydrogen fluoride is absorbed by an absorption device, and the process product lithium fluoride is recovered by filtration.

[0005] These methods generally have the disadvantages of high equipment requirements and complex processes. In addition, the above-mentioned inventive methods all simply treat toxic and harmful fluorine-containing substances such as hydrogen fluoride, which not only leads to a waste of fluorine resources in the electrolyte, but also these fluorine-containing solutions are extremely corrosive and can strongly corrode metals, glass and silicon-containing objects. Direct operation poses a hidden danger to personnel safety and health, and is not easy to promote and apply in large-scale production.

[0006] Therefore, it is necessary to develop a method that has low requirements on equipment materials, easy to implement process equipment and processes, and can effectively recycle and reuse lithium and fluorine resources in electrolytes. Summary of the invention

[0007] At present, there are few studies on the recycling and reuse of lithium resources in waste lithium-ion battery electrolytes at home and abroad. Although the process methods in the prior art can successfully recycle and reuse lithium resources from waste lithium battery electrolytes, these methods also generally have the disadvantages of high equipment requirements and complex processes. In addition, the focus of the prior art is on recycling and reusing lithium resources in the electrolyte, but there are very few recycling and reuse of fluorine resources in the electrolyte. Compared with the prior art, the present invention uses a wet process to recover lithium resources and fluorine resources in the electrolyte in a green, safe and efficient manner. The process has the advantages of low equipment requirements, low energy consumption and simple process. In addition, the entire process does not use toxic and harmful organic solvents, ensuring that the entire recycling process is green and environmentally friendly. The lithium element in the electrolyte of the present invention is recovered in the form of LiF, and the recovered LiF is characterized by X-ray diffraction (XRD) test, indicating that the recovered LiF has extremely high purity and can be used as a battery additive or other industrial raw materials. The fluorine element in the electrolyte is recovered in the form of NaF and LiF solid salts. The recovered NaF is characterized by X-ray diffraction (XRD) test, indicating that the recovered NaF has high purity and good reusability. The observed instruments and equipment after recovery are intact and not corroded, indicating that the method of the present invention successfully avoids the damage of HF produced by LiPF6 hydrolysis during the recovery process to the corrosion of instruments and equipment and environmental pollution, and is a green, safe and efficient recovery route for recovering lithium and fluorine resources from electrolytes.

[0008] In order to achieve the above-mentioned invention object, the first aspect of the present invention is to provide a method for recovering lithium resources and fluorine resources in an electrolyte in a green, safe and efficient manner using a wet process, the method comprising the following steps:

[0009] (1) mixing an electrolyte containing a fluorinated lithium compound with a strong base solution to obtain a mixed solution, wherein the molar ratio of LiPF6 to the strong base is 1:4-6;

[0010] (2) evaporating the mixed liquid obtained in step (1) to remove the liquid, and then fully mixing the obtained solid with water to separate the solid from the liquid to obtain a liquid separator and a solid separator, respectively; repeatedly mixing the obtained solid separator with water and separating the solid separator, and performing this process once or multiple times, and finally drying the obtained solid separator to obtain a solid recovered product LiF;

[0011] (3) evaporating the liquid separated from the liquid in step (2) to remove the liquid, adding the obtained solid to an organic solvent, mixing them thoroughly, and performing solid-liquid separation to obtain a liquid separated product and a solid separated product, respectively; repeatedly mixing and separating the obtained solid separated product with the organic solvent, and performing this process once or multiple times, and finally drying the obtained solid separated product to obtain a solid recovered product NaF;

[0012] The organic solvent is at least one of ethanol, dichloromethane, tetrahydrofuran, acetone, acetonitrile and dimethylformamide, more preferably ethanol.

[0013] Preferably, the strong alkaline solution is at least one of NaOH and KOH aqueous solutions, more preferably NaOH solution.

[0014] In a preferred embodiment of the present invention, the electrolyte is the electrolyte in a lithium battery after circulation, and the electrolyte contains a fluorine-lithium compound and an organic solvent.

[0015] The fluorine-lithium compound is a lithium compound and / or a fluorine compound, including but not limited to lithium hexafluorophosphate (LiPF6).

[0016] The present invention can be applied to the electrolyte in the lithium battery after circulation, wherein the electrolyte contains fluorine-lithium compounds and organic solvents, wherein the organic solvents include but are not limited to at least one of ethylene carbonate (EC), dimethyl carbonate (DMC) and diethyl carbonate (DEC).

[0017] Generally speaking, waste electrolyte is the electrolyte in lithium batteries after recycling, which is composed of organic solvent (at least one of EC, DMC or DEC) and lithium salt (LiPF6), etc., among which the theoretical content of lithium hexafluorophosphate (LiPF6) is 1 mol / L. In addition, waste electrolyte also contains a small amount of substances produced by the decomposition of LiPF6, including POF3, PF5 and trace HF.

[0018] The inventor of the present invention has found through research that the phosphorus-containing substances, fluorine-containing substances and organic solvents produced after the decomposition of LiPF6 in the electrolyte have a competitive relationship with the strong base (taking NaOH as an example) reaction, and it is difficult to remove the phosphorus-containing substances while recycling elements such as F and Li, that is, it is difficult to obtain a product with a high recovery rate, and it is more difficult to obtain a recovered product with a higher purity on the basis of obtaining a product with a high recovery rate. After research, the inventor of the present invention was surprised to find that when the ratio of NaOH and LiPF6 is (4-6): 1, more preferably (4.8-5.2): 1, and most preferably 5: 1, using the specific recovery method in the present invention, the competitive relationship between NaOH and phosphorus-containing substances, fluorine-containing substances and organic solvents is unexpectedly maintained in a more ideal state, and NaOH, while ensuring efficient absorption of fluorine-containing substances, has as few side reactions as possible, making the recovery process the most economical and environmentally friendly. At this time, the phosphorus-containing substances in the electrolyte are mostly washed away by organic solvents such as ethanol, and a very small part is doped in NaF, but it can be seen from XRD characterization that NaF still has a higher purity and can be directly applied in other processes.

[0019] The inventors of the present invention have found out through XRD test characterization results of the product that when the ratio is higher than the above ratio (the ratio of NaOH and LiPF6 (4-6): 1), although the fluorine-containing substances can be efficiently absorbed, the amount of side reaction products of NaOH with phosphorus-containing substances and organic solvents increases, which reduces the purity of NaF and makes purification difficult; when it is lower than the above ratio, it can be theoretically known that the absorption efficiency of fluorine-containing substances is reduced, resulting in a lower recovery rate of fluorine resources and an increased risk of the experimental process.

[0020] In a preferred embodiment of the present invention, in step (1): the molar ratio of LiPF6 to the strong base is 1:(4.8-5.2). The inventors of the present invention found that when the molar ratio of NaOH to LiPF6 is increased, the excess NaOH will react with the organic solvent, resulting in a decrease in the purity of the recovered product; when the molar ratio of NaOH to LiPF6 is reduced, NaOH cannot completely fix the fluorine-containing toxic and harmful substances produced by LiPF6, resulting in a certain amount of corrosion to the equipment during the experiment.

[0021] In a preferred embodiment of the present invention, the strong alkaline solution is at least one of NaOH and KOH aqueous solutions.

[0022] In a preferred embodiment of the present invention, the concentration of the strong alkali solution is 1.5-2.5mol / L, and most preferably 1.8-2.2mol / L. The inventors of the present invention have found that within the optimal range of the amount of the substance to which the alkali is added, more effective absorption of fluorine-containing toxic and harmful substances can be performed. The concentration of the strong alkali solution is related to the amount of the substance to which the alkali is added and the volume of water. When the concentration of the strong alkali solution is low, the volume of the strong alkali solution added becomes larger, which reduces the efficiency of treating the waste liquid (the amount of waste liquid treated by the equipment of the same volume is reduced) and is not conducive to efficient reaction with harmful substances, resulting in overflow of some toxic substances; when the concentration of the strong alkali solution is high, the strong alkali is accompanied by precipitation in the process of mixing with the waste liquid, which also affects the absorption effect of harmful substances (there is a process of alkali redissolution), so the concentration of the strong alkali should be controlled within the preferred range to ensure efficient and economical absorption of harmful substances.

[0023] According to the present invention, the mixing conditions in step (1) can be selected within a wide range. In a preferred embodiment of the present invention, in step (1): the mixing conditions include: a temperature of 0-40°C, and / or a time of 6-18h.

[0024] According to the present invention, the conditions for evaporating and removing the liquid in step (2) can be selected within a wide range. In a preferred embodiment of the present invention, in step (2): the conditions for evaporating and removing the liquid include: a temperature of 80-120°C, and / or a time of 6-18h.

[0025] According to the present invention, the amount of water added in step (2) can be selected within a wide range. In a preferred embodiment of the present invention, the amount of water added is 3-5 times the volume of the waste electrolyte in step (1), and the mixing is repeated 2-3 times. Too much or too little water can also achieve similar effects, but too much water will increase the energy consumption of subsequent treatment and reduce the LiF yield; too little water will reduce the purity of LiF.

[0026] According to the present invention, the mixing conditions in step (2) can be selected within a wide range. In a preferred embodiment of the present invention, in step (2): the mixing conditions include: a temperature of 0-60°C, and / or a time of 2-6h.

[0027] According to the present invention, the solid-liquid separation method in step (2) includes but is not limited to centrifugal separation or filtration separation; and / or,

[0028] According to the present invention, the drying conditions in step (2) can be selected within a wide range. In a preferred embodiment of the present invention, the drying temperature is 60-100° C., and / or the drying time is 6-12 h.

[0029] According to the present invention, the conditions for evaporating and removing the liquid in step (3) can be selected within a wide range. In a preferred embodiment of the present invention, in step (3): the conditions for evaporating and removing the liquid include: a temperature of 80-120°C, and / or a time of 6-18h.

[0030] According to the present invention, the amount of organic solvent added in a single step (3) can be selected within a wide range. In a preferred embodiment of the present invention, the amount of organic solvent added is 3-5 times the volume of the waste electrolyte in step (1), and the mixing is repeated 2-5 times. Too much or too little organic solvent can also achieve similar effects. Too much organic solvent will reduce the NaF yield; too little organic solvent will reduce the NaF purity.

[0031] According to the present invention, the mixing conditions in step (3) can be selected within a wide range. In a preferred embodiment of the present invention, the mixing conditions include: a temperature of 0-40° C., and / or a time of 2-6 h.

[0032] According to the present invention, the separation method in step (3) includes but is not limited to centrifugal separation or filtration separation.

[0033] According to the present invention, the drying conditions in step (3) can be selected within a wide range. In a preferred embodiment of the present invention, the drying conditions include: a temperature of 30-80° C., and / or a drying time of 6-12 h.

[0034] In a preferred embodiment of the present invention, the method further comprises: after drying, optionally crushing the solid recovered LiF and NaF obtained in steps (2) and (3), respectively.

[0035] In the present invention, "and / or" means that the two conditions connected by "and / or" can exist at the same time, or only one of them can exist.

[0036] The second aspect of the present invention is to provide an application of the method described above in lithium ion battery recycling.

[0037] Specifically, the method comprises crushing the lithium-ion battery by the method in the prior art, recovering the electrolyte, and then recovering the electrolyte according to the method of the present invention.

[0038] Compared with the prior art, the present invention provides a method for recovering lithium and fluorine resources in electrolyte in a green, safe and efficient wet process and its application has the following advantages:

[0039] (1) Yield and purity of recovered products. Compared with the prior art, the method provided by the present invention recovers the lithium element in the lithium-ion battery electrolyte in the form of lithium fluoride (LiF) solid salt, and the recovery rate of LiF can reach 85%. The X-ray diffraction (XRD) test and characterization analysis of the recovered LiF product shows that the recovered LiF has extremely high purity and can be used as a battery additive or other industrial raw material. The fluorine element in the electrolyte is recovered in the form of sodium fluoride (NaF) and lithium fluoride (LiF) solid salts, and the recovery rate can reach 90%. The X-ray diffraction (XRD) test and characterization analysis of the recovered NaF product shows that the recovered NaF has a high purity and good reusability, and can continue to be used in lithium batteries and other preparation processes.

[0040] (2) Treatment of toxic and harmful substances containing fluorine. In the prior art, most of the special absorption devices are used to absorb and treat toxic and harmful substances containing fluorine, but in the process of HF separation and discharge, corrosion to the equipment is inevitable; or as the method provided in patent document CN 104852102 A, lithium phosphate and phosphorus oxyfluoride are used to form a solid-liquid reaction to generate an organic solvent containing lithium difluorophosphate, which can be used as an electrolyte salt or an additive for an electrolyte composition containing an electrolyte salt. In contrast, the method of the present invention can completely avoid the hydrolysis of LiPF6 in the electrolyte to produce HF, does not use special absorption devices and other expensive additives, and directly converts the fluorine resources in the electrolyte into high-purity NaF and LiF solid salts by optimizing the addition amount of strong alkali such as NaOH, thereby realizing green, environmentally friendly and efficient recovery of fluorine resources in the electrolyte, avoiding the corrosion of equipment and instruments during the experiment and the hidden dangers of personnel safety and health, and has a wider application and greater economic benefits.

[0041] (3) Equipment requirements, energy consumption and cost. In the prior art, most of them provide a special processing device to recover valuable resources in the electrolyte, such as patent document CN111934041A. The application of these devices must be carried out under special conditions, such as a closed environment, inert gas filling, etc., which leads to higher equipment requirements for the recovery process, increased costs, and does not take advantage of large-scale production applications. In contrast, the method of the present invention does not require special instruments and equipment and operating environment, and the process flow only uses two green, environmentally friendly, and low-cost solvents, water and simple and easily available organic solvents such as ethanol. The process flow is simple, without high temperature and high pressure operation steps, which reduces the energy consumption and cost of the process flow and is easy to promote and apply in large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is a flow chart of the recovery process in Example 1 of the present invention.

[0043] Figure 2This is an XRD test curve diagram of LiF recovered in Example 1 of the present invention.

[0044] Figure 3 It is a comparison chart of XRD test curves of NaF recovered in Example 1, Comparative Example 1 and Comparative Example 2 of the present invention.

[0045] Figure 4 The figure is a comparison of the corrosion of HF acid on instruments and equipment in Example 1 of the present invention and Comparative Example 3 (direct evaporation solvent recovery method). DETAILED DESCRIPTION

[0046] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0047] The theoretical content of LiPF6 in the electrolyte is 1M, and the molar ratio of LiPF6 to NaOH is 1:5. The theoretical mass of LiF is m1, and the recovered mass is m2. The theoretical mass of NaF is n1, and the recovered mass is n2. The product recovery rate of the invention is calculated as follows:

[0048] Calculation method of LiF recovery rate: Y = m2 / m1×100%

[0049] Calculation method of NaF recovery rate: X = n2 / n1×100%

[0050] Calculation method of F recovery rate: Z = (m2 + n2) / (m1 + n1) × 100%

[0051] Preparation Example

[0052] Waste electrolyte is obtained from recycled lithium-ion batteries, in which the theoretical content of lithium hexafluorophosphate (LiPF6) is 1 mol / L, and the organic solvents are ethylene carbonate (EC) and dimethyl carbonate (DMC). In addition, the waste electrolyte also contains a small amount of substances decomposed by LiPF6, including POF3, PF5 and trace HF.

[0053] Example 1

[0054] (1) Add 50 ml of 2 mol / L NaOH aqueous solution (the molar ratio of LiPF6 to NaOH is 1:5) dropwise into 20 ml of the waste electrolyte while stirring, and stir thoroughly at room temperature for 24 h;

[0055] (2) Use an oil bath to evaporate the liquid at 120°C to obtain a white solid mixture; add the white solid mixture to 80 ml of deionized water, stir it thoroughly at room temperature for 4 hours, and then use a vacuum pump to filter it through a Buchner funnel at a vacuum degree of 0.1 MPa to obtain a solid separator and a liquid separator. Disperse the solid separator again in deionized water, repeat the above operation twice, and bake the final solid separator in a vacuum oven at 80°C for 6 hours to obtain a white solid, i.e., the recovered LiF. Grind it in a mortar for 5 minutes to obtain a white powder of LiF with a recovery rate of 85%;

[0056] (3) The liquid separated product in (2) was heated in an oil bath at 100°C to evaporate the liquid and obtain a white solid mixture; the white solid mixture was added with 80 ml of anhydrous ethanol, stirred for 4 hours at room temperature, and then filtered through a Buchner funnel at a vacuum degree of 0.1 MPa using a vacuum pump to obtain a solid separated product. The solid separated product was dispersed in anhydrous ethanol again, and the above operation was repeated 4 times. The final solid separated product was dried in a vacuum oven at a temperature of 80°C for 6 hours to obtain a white solid, i.e., the recovered NaF. The white powder of NaF was obtained by grinding in a mortar for 5 minutes, and the recovery rate was 90%. The recovery rate of F was calculated to be 89%.

[0057] Comparative Example 1

[0058] Compared with Example 1, the molar amount of NaOH in step (1) is increased in Comparative Example 1, that is, the molar ratio of NaOH to LiPF6 is adjusted to 8:1. The remaining operating steps are the same as those in Example 1.

[0059] The molar amount of NaOH increases, which is not conducive to the recovery and reuse of lithium and fluorine resources in the electrolyte. Specifically, as the molar amount of NaOH increases, the excess NaOH will react with the solvent in the electrolyte and the P-containing substances produced by the decomposition of LiPF6, resulting in low purity of the final recovered NaF product, and a reduced recovery rate of LiF and NaF, with a recovery rate of LiF of only 75%. The impurities produced by the side reactions are relatively large and difficult to separate from NaF, and the recovery rates of NaF and F cannot be determined. However, in this comparative example, due to the addition of NaOH, the hydrolysis of LiPF6 in the electrolyte to produce HF can be avoided, so that the inner wall of the glass bottle is not corroded.

[0060] Comparative Example 2

[0061] Compared with Example 1, in Comparative Example 2, a trace amount of water (0.2 ml of water) was first added to 20 ml of electrolyte, and the mixed solution was obtained after being fully stirred at room temperature for 12 hours; 50 ml of a 2 mol / L NaOH aqueous solution was dropwise added to the waste electrolyte while stirring, and the mixture was fully stirred at room temperature for 6 hours; the remaining operating steps were the same as in Example 1.

[0062] Adding a small amount of deionized water to the electrolyte can accelerate the decomposition of LiPF6 and improve the efficiency of the subsequent reaction with NaOH solution. However, the addition of a small amount of ionized water accelerates the decomposition of LiPF6 to produce hydrofluoric acid, which causes corrosion to the bottle body and the release of HF, which is not conducive to the green and safe process.

[0063] In order to verify the feasibility of the above method, the LiF and NaF recovered by the method of Example 1 were characterized and tested. Please refer to Figure 2 , Figure 3 .

[0064] Depend on Figure 2 It can be seen that the diffraction signal of LiF recovered in Example 1 of the present invention is consistent with that of the LiF standard XRD card and has no impurity peaks, which proves that the recovered material is LiF with high purity.

[0065] Depend on Figure 3 It can be seen that the diffraction signal of NaF recovered by the method of Example 1 of the present invention is consistent with the diffraction signal of the XRD card of the NaF standard and has no impurity peaks, which proves that the product recovered in Example 1 is NaF and has a high purity. Although the products recovered by the methods of Comparative Examples 1 and 2 also have the diffraction signal peaks of the NaF standard XRD card, there are other impurity peaks, indicating that the purity of NaF recovered by the comparative method is not high and contains other impurities.

[0066] Comparative Example 3

[0067] Compared with Example 1, Comparative Example 3 is a direct evaporation solvent recovery method, and the specific operating steps are:

[0068] (1) taking 20 ml of the waste electrolyte, gradually heating it in an oil bath, evaporating and removing the solvent in the solution to obtain a white solid mixture;

[0069] (2) Add the white solid mixture to 80 ml of deionized water, stir it thoroughly at room temperature for 4 hours, and then filter it through a Buchner funnel with a vacuum pump at a vacuum degree of 0.1 MPa. Dissolve the solid separated material in deionized water again, repeat the above operation 4 times, and bake the final solid separated material in a vacuum oven at a temperature of 80°C for 6 hours to obtain a white solid, i.e., the recovered LiF. Grind it in a mortar for 5 minutes to obtain LiF white powder.

[0070] Compared with Example 1, the recovery rate of LiF solid salt recovered by the direct evaporation solvent recovery method is low, only 70%, the purity is poor, and the fluorine resources in the electrolyte cannot be efficiently recovered. In addition, compared with the corrosion of the bottle body after recovery, since the direct evaporation solvent recovery method cannot effectively avoid the hydrolysis of LiPF6 in the electrolyte to produce HF, the direct evaporation solvent recovery method of lithium resources in the electrolyte causes serious corrosion to the inner wall of the glass bottle.

[0071] To verify that the present invention can completely avoid the generation of HF, Figure 4 This is a comparison chart of the corrosion conditions of the equipment after the experiments of Example 1 and Comparative Example 3.

[0072] Compared with Example 1, the corrosion of the bottle body after recovery is shown in that in the method of directly evaporating the solvent to recover lithium resources in the electrolyte in Comparative Example 3, the inner wall of the bottle body is severely etched, and the numbers on the cardboard behind the bottle body cannot be observed. On the contrary, in the method of recovering lithium resources in the electrolyte in Example 1 of the present invention, the inner wall of the bottle body is smooth and transparent, and the numbers behind the bottle body can be clearly observed, indicating that the method of the invention completely avoids HF generation and reduces the corrosion of the bottle body. In addition, the direct evaporation solvent recovery method cannot efficiently and simultaneously recover the fluorine resources in the electrolyte, resulting in a waste of resources and harm to the environment and personnel health.

[0073] Example 2

[0074] The experiment was carried out according to the method of Example 1, except that the concentration of NaOH was changed to 3 mol / L and the amount added was 33 mL.

[0075] After NaOH and waste electrolyte were mixed and stirred for a period of time, white solids were found to precipitate in the solution, which was not conducive to the efficient absorption of fluorine-containing substances, resulting in an 80% reduction in the recovery rate of fluorine resources. NaOH easily reacts with phosphorus-containing substances and organic solvents, resulting in a reduction in the purity of the NaF product.

[0076] Example 3

[0077] The experiment was carried out according to the method of Example 1, except that the concentration of NaOH was changed to 1 mol / L and the amount added was 100 mL.

[0078] When the concentration of NaOH is reduced, it is not conducive to the rapid absorption of fluorine-containing substances, resulting in the overflow of some fluorine-containing toxic substances, which intensifies the corrosion of the bottle after recovery and reduces the recovery rate of fluorine resources by 75%. In addition, NaOH is prone to side reactions with phosphorus-containing substances and organic solvents, resulting in a decrease in the purity of NaF products. Obviously, the volume of NaOH used increases and the economic efficiency decreases.

[0079] Moreover, when the concentration of NaOH is too high or too low, NaOH cannot react and absorb fluorine-containing substances efficiently, which will lead to intensified side reactions with phosphorus-containing substances and organic solvents, thereby reducing the purity of the NaF product.

[0080] The above contents are merely examples and explanations of the concept of the present invention. Those skilled in the art may make modifications, supplements or replace the specific embodiments described in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they shall fall within the protection scope of the present invention.

[0081] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.

[0082] All publications, patent applications, patents and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings conventionally understood by those skilled in the art. In the event of a conflict, the definition in this specification shall prevail.

[0083] When this specification uses the prefix "well-known to those skilled in the art", "prior art" or similar terms to introduce materials, substances, methods, steps, devices or components, etc., the objects introduced by the prefix cover those commonly used in the art when this application is filed, but also include those that are not commonly used at present but will become recognized in the art as being suitable for similar purposes.

[0084] The endpoints and any values ​​of the scope disclosed in the present application document are not limited to the precise scope or value, and these scopes or values ​​should be understood to include values ​​close to these scopes or values. For numerical ranges, between the endpoint values ​​of each scope, between the endpoint values ​​of each scope and a separate point value, and between separate point values, one or more new numerical ranges can be combined with each other, and these numerical ranges should be considered as specifically disclosed in this article. Hereinafter, in principle, each technical solution can be combined with each other to obtain a new technical solution, which should also be considered as specifically disclosed in this article.

[0085] In the context of the present specification, any matters or items not mentioned are directly applicable to those known in the art without any changes except those explicitly stated.

[0086] Moreover, any embodiment described in this document may be freely combined with one or more other embodiments described in this document, and the technical solutions or technical ideas formed thereby are deemed to be part of the original disclosure or original record of the present invention, and should not be regarded as new content that has not been disclosed or anticipated in this document, unless a person skilled in the art considers that the combination is obviously unreasonable.

Claims

1. A method for recovering lithium resources and fluorine resources in an electrolyte, the method comprising the following steps: (1) mixing an electrolyte containing a fluorine-lithium compound with a strong base solution to obtain a mixed solution, wherein the molar ratio of LiPF6 to the strong base is 1:(4-6); the strong base solution is a NaOH aqueous solution, or a NaOH and KOH aqueous solution; (2) evaporating the mixed liquid obtained in step (1) to remove the liquid, and then fully mixing the obtained solid with water to separate the solid and the liquid, respectively obtaining a liquid separation and a solid separation; repeatedly mixing the obtained solid separation with water and separating, and this is performed once or multiple times, and finally drying the obtained solid separation to obtain a solid recovered product LiF; (3) The liquid separated product in step (2) is evaporated to remove the liquid, and the obtained solid is added to an organic solvent, and after being fully mixed, solid-liquid separation is performed to obtain a liquid separated product and a solid separated product respectively; the obtained solid separated product is repeatedly mixed with the organic solvent and separated, and this is performed once or multiple times, and the finally obtained solid separated product is dried to obtain a solid recovered product NaF; The organic solvent is at least one of ethanol, dichloromethane, tetrahydrofuran, acetone, acetonitrile and dimethylformamide.

2. The method according to claim 1, characterized in that The electrolyte is the electrolyte in the lithium battery after circulation, and the electrolyte contains fluorine-lithium compounds and organic solvents. The organic solvent is at least one of ethylene carbonate, dimethyl carbonate and diethyl carbonate.

3. The method according to claim 2, characterized in that The fluorine-lithium compound is lithium hexafluorophosphate.

4. The method according to claim 1, characterized in that In step (1): The molar ratio of LiPF6 to strong base is 1:(4.8-5.2); and / or, The concentration of the strong alkaline solution is 1.5-2.5 mol / L.

5. The method according to claim 4, characterized in that In step (1): The concentration of the strong alkaline solution is 1.8-2.2 mol / L.

6. The method according to claim 1, characterized in that In step (1): The mixing conditions include: a temperature of 0-40° C., and / or a mixing time of 6-18 h.

7. The method according to claim 1, characterized in that In step (2): The conditions for evaporating and removing the liquid include: a temperature of 80-120°C, and / or a time of 6-18 hours; and / or, The amount of water added is 3-5 times the volume of the waste electrolyte in step (1), and the mixing is repeated 2-3 times.

8. The method according to claim 1, characterized in that In step (2): The mixing conditions include: a temperature of 0-60°C, and / or a time of 2-6 h; and / or, The solid-liquid separation method is centrifugal separation or filtration separation; and / or, The drying temperature is 60-100 ℃, and / or the drying time is 6-12 h.

9. The method according to claim 1, characterized in that: In step (3): The conditions for evaporating and removing the liquid include: a temperature of 80-120° C., and / or a time of 6-18 h; and / or, The amount of organic solvent added is 3-5 times the volume of the waste electrolyte in step (1), and the mixing is repeated 2-5 times; and / or, The mixing conditions include: temperature of 0-40°C, and / or time of 2-6 h; and / or, The separation method is centrifugal separation or filtration separation; and / or, The drying conditions include: a temperature of 30-80°C, and / or a drying time of 6-12 h.

10. The method according to any one of claims 1 to 9, characterized in that: The method further comprises: after drying, optionally crushing the solid recovered LiF and NaF obtained in steps (2) and (3), respectively.

11. Use of the method according to any one of claims 1 to 10 in lithium ion battery recycling.

Citation Information

Patent Citations

  • Method and device for recycling and harmlessly treating waste lithium ion battery electrolyte

    CN104852102A

  • Positive electrode and electrolyte hybrid recycling method of lithium battery

    CN107910610A

  • Method for recycling and reusing electrolyte of waste lithium ion battery

    CN111934041A

  • Waste electrolyte treatment method for lithium-ion battery

    CN108923092A

  • Method and system for recovering lithium from waste lithium iron phosphate battery

    CN109207730A