Boron nitride modification method, product and application

By coating the vapor phase silica on the surface of boron nitride and performing silane coupling agent grafting reaction, the complexity and pollution problems of the existing boron nitride modification methods are solved, and the dispersion and composite of boron nitride is improved. The thermal conductivity of the material achieves simplification and safety of the process.

CN116082858BActive Publication Date: 2024-11-22YAAN BESTRY PERFORMANCE MATERIALS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211705485.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-29
Publication Date
2024-11-22
Estimated Expiration
2042-12-29

AI Technical Summary

Technical Problem

The existing boron nitride modification methods have problems such as complex processes, high pollution, safety hazards and high costs, and it is difficult to effectively improve the dispersion and thermal conductivity of boron nitride.

Method used

By dry mixing the boron nitride powder with the vapor phase silica powder, the vapor phase silica is coated on the surface of the boron nitride, and after heating and curing, the grafting reaction is performed using a silane coupling agent to form modified boron nitride. .

Benefits of technology

It achieves good dispersion and high filling amount of boron nitride, improves the thermal conductivity of composite materials, and has a simple process, safe, environmentally friendly and has a wide range of use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116082858B_ABST
    Figure CN116082858B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of composite materials. In view of the poor dispersibility of the modified boron nitride obtained by directly modifying boron nitride with a silane coupling agent, it is difficult to achieve the effects of reducing viscosity, increasing the filling amount and dispersibility when used as a thermal conductive filler; the present invention discloses a method for modifying boron nitride, by coating the surface of boron nitride with fumed silica, and the hydroxyl groups on the surface of the fumed silica can provide reactive groups for the silane coupling agent, so that the silane coupling agent is grafted onto the boron nitride. The modified boron nitride obtained by the method provided by the present invention has good dispersibility, and when used as a thermal conductive filler for a composite material, the filling amount of boron nitride can be effectively increased, thereby improving the thermal conductivity of the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials, and particularly relates to a boron nitride modification method, product and application. Background Art

[0002] Hexagonal boron nitride, similar to graphite in its hexagonal crystal structure, has very high thermal conductivity, electrical insulation, thermal stability, chemical stability, and corrosion resistance. As a thermal conductive filler, it is widely used in the preparation of high thermal conductivity and electrical insulation composite materials. However, hexagonal boron nitride has stable chemical properties, lacks active groups on its surface, and lacks strong interaction with the matrix of the composite material, so its dispersion in the matrix is ​​very poor.

[0003] At present, in order to improve the dispersibility of hexagonal boron nitride, thereby improving the improvement effect of hexagonal boron nitride on the thermal conductivity of composite materials, it is usually necessary to modify the hexagonal boron nitride.

[0004] There are three main existing modification methods:

[0005] (1) Direct modification with silane coupling agent;

[0006] However, since the surface of boron nitride itself is very smooth and it carries very few hydroxyl groups, when it is directly modified with silane coupling agent, the silane coupling agent has no action point and no functional group to combine with it; therefore, the silane coupling agent floats on the surface of boron nitride and is not truly combined with boron nitride, making it difficult to achieve the effect of reducing viscosity, increasing filling amount and dispersibility.

[0007] (2) First boil with sodium hydroxide, then modify with silane coupling agent;

[0008] Sodium hydroxide affects the crystal structure of boron nitride and easily breaks the NB bond. In addition, the amount of sodium hydroxide waste liquid is relatively large, which will cause pollution and is very troublesome to handle. At the same time, there are certain safety hazards.

[0009] (3) First connect dopamine and then modify it with a silane coupling agent;

[0010] Dopamine will turn boron nitride gray, which limits its use in many products that have color requirements. In addition, dopamine is relatively expensive and has high costs. Summary of the invention

[0011] In view of the fact that the above-mentioned three main existing boron nitride modification methods all have their own shortcomings, one of the objects of the present invention is to provide a boron nitride modification method, which has simple process, safe operation, no pollution to the product, and is beneficial to improving the dispersibility of boron nitride, thereby increasing the filling amount of boron nitride as a thermal conductive filler.

[0012] To achieve the above object, the present invention adopts the following technical solutions:

[0013] A boron nitride modification method comprises the following steps:

[0014] S1, adding boron nitride powder and fumed silicon dioxide powder into a mixing treatment device for mixing to obtain a primary product;

[0015] S2. The primary product obtained in step S1 is heated and solidified, and then naturally cooled to room temperature.

[0016] S3, adding a silane coupling agent into pure water, and performing hydrolysis and stirring in a stirring treatment device to obtain a mixed solution;

[0017] S4, adding the cooled primary product obtained in step S2 to the mixed solution obtained in step S3, stirring and mixing, to achieve a grafting reaction and obtain a dispersion;

[0018] S5. After the grafting reaction is completed, the dispersion obtained in step S4 is filtered and dried to obtain modified boron nitride.

[0019] Before the primary product is modified by the silane coupling agent, the primary product is firstly subjected to a heat treatment, so that the fumed silica can be more tightly coated on the boron nitride.

[0020] Preferably, the temperature of the heating and curing is ≤1300°C.

[0021] Since the temperature is too high, the fumed silica may change from amorphous to crystalline, which causes the fumed silica to fall off, resulting in less fumed silica on the boron nitride, which affects the reactivity of the grafting reaction when the silane coupling agent is modified. The present invention has found through a large number of experiments that when the temperature of heating and curing is 800°C, the fumed silica coating is the best, followed by 600°C and 1000°C. When the temperature exceeds 1300°C, the fumed silica will crystallize, resulting in a decrease in the fumed silica, which is not conducive to the subsequent grafting reaction of the silane coupling agent.

[0022] Preferably, after step S5, the modified boron nitride obtained in step S5 is added to a mixing treatment device for secondary mixing.

[0023] Preferably, the mass ratio of the boron nitride powder to the fumed silicon dioxide in step S1 is 1000:1-10.

[0024] Preferably, the mass ratio of the amount of the silane coupling agent used in step S3 to the boron nitride is 1-10:1000.

[0025] Preferably, the mass ratio of the amount of pure water used in step S3 to the boron nitride powder is 5 to 15:1.

[0026] Preferably, the stirring device of step S3 is a stirring kettle, and the hydrolysis stirring time is 10 min to 30 min; the stirring and mixing time of step S4 is 1 h to 3 h; the drying temperature of step S4 is 100° C. to 110° C., and the time is 4 h to 8 h.

[0027] Preferably, the mixing treatment device in step S1 is a double cone mixer, and the mixing time is 1 hour to 2 hours. The double cone mixer can mix the fumed silicon dioxide and boron nitride.

[0028] Application of the modified boron nitride obtained by any of the methods described above as a thermally conductive filler for composite materials.

[0029] Preferably, the matrix of the composite material is epoxy resin.

[0030] Preferably, the silane coupling agent is a silane coupling agent having an epoxy group.

[0031] Preferably, the silane coupling agent is KH-560.

[0032] It can be seen from the above description that compared with the prior art, the present invention has the following advantages:

[0033] The modification method provided by the present invention comprises the following steps: dry-mixing fumed silicon dioxide and boron nitride, during which the fumed silicon dioxide is coated on the surface of the boron nitride, so that the surface of the boron nitride is modified with hydroxyl groups; then the silane coupling agent is used for modification, and the silane coupling agent and the hydroxyl groups on the surface of the boron nitride undergo a dehydration reaction, so that the boron nitride is firmly grafted onto the boron nitride; the modified boron nitride obtained by the method has good dispersibility and has a higher filling amount when used as a thermal conductive filler for a composite material, so as to be beneficial to improving the thermal conductivity of the composite material.

[0034] The modification method provided by the invention has the characteristics of simple process steps, easy regulation, safe operation, environmental protection and wide application range. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or technical descriptions will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0036] Figure 1 This is the surface morphology of boron nitride without fumed silica coating.

[0037] Figure 2This is the surface morphology of the modified boron nitride obtained in Example 1. DETAILED DESCRIPTION

[0038] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the present invention. Therefore, the drawings and descriptions are considered to be exemplary and non-restrictive in nature.

[0039] The embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0040] Effective dispersion of boron nitride is a basic requirement for improving the thermal conductivity of composite materials. Boron nitride particles need an interconnected contact network to create an optimal heat transfer path through the matrix through particle-particle connectivity. However, the chemical properties of boron nitride are stable, the surface lacks active groups, the dispersion in the matrix is ​​very poor, and it is difficult to react with other substances for surface modification. In order to improve the activity of boron nitride, the prior art usually introduces functional groups by boiling boron nitride with sodium hydroxide or grafting dopamine, but sodium hydroxide will destroy the crystal structure of boron nitride, and the waste liquid generated is difficult to handle; while grafting dopamine will change the color of boron nitride, so the scope of use is narrow and the cost is high.

[0041] The modification method provided by the present invention firstly mixes fumed silica and boron nitride to coat the surface of the boron nitride with the fumed silica, thereby introducing hydroxyl groups on the surface of the boron nitride; then, a silane coupling agent is used for modification, and the silane coupling agent can undergo a dehydration reaction with the hydroxyl groups on the surface of the boron nitride, thereby grafting the silane coupling agent on the boron nitride, thereby preparing the modified boron nitride; compared with the existing modification method, the method has the characteristics of simple process, safe operation, environmental protection and wide application range.

[0042] Example 1

[0043] (1) Weigh boron nitride powder and fumed silica in a mass ratio of 1000:1-10, add them into a double cone mixer and mix them for 1h-2h to make the fumed silica powder and boron nitride powder evenly mixed to obtain the initial product of fumed silica-coated boron nitride. The surface morphology of the initial product under a scanning electron microscope is shown in the attached figure. Figure 2 As shown, it can be seen that the fumed silica is successfully coated on the boron nitride.

[0044] Since the surface of fumed silica has hydroxyl groups, the surface of boron nitride is modified with hydroxyl groups; and the fumed silica is coated on the surface of boron nitride by mixing in a double cone mixer, which is simple to operate and easy to control; the content of fumed silica is small and will not affect the performance of boron nitride.

[0045] (2) Preparation of silane coupling agent aqueous solution: Weigh pure water and silane coupling agent in a mass ratio of boron nitride, pure water and silane coupling agent of 1000:10000:1-10, and stir in a stirring kettle at a speed of 300 r / min for 10 min-30 min to hydrolyze the silane coupling agent into silanol, thereby obtaining a mixed solution.

[0046] (3) Add the cooled primary product to the mixed solution and continue stirring for 1 to 3 hours. During the stirring process, the silane coupling agent and the hydroxyl groups on the surface of the fumed silica-coated boron nitride undergo a dehydration reaction, thereby being grafted onto the fumed silica-coated boron nitride to obtain a dispersion.

[0047] (4) The dispersion is filtered and baked in an oven at a temperature of 100 to 110° C. for 4 to 8 hours to obtain modified boron nitride.

[0048] The modified boron nitride obtained by the above steps has better dispersibility because the surface of the boron nitride is coated with fumed silica, and the surface of the fumed silica has a large number of hydroxyl groups. The silane coupling agent can undergo a dehydration reaction with the hydroxyl groups on the surface of the boron nitride, thereby being grafted onto the fumed boron nitride.

[0049] Example 2

[0050] (1) Same as Example 1.

[0051] (2) The primary product obtained in (1) is sent to a sintering furnace and kept at a temperature of ≤1300°C for 2h to 6h. Before the primary product is modified with a silane coupling agent, the primary product is first heated and cured. During the heating and curing process, due to the removal of water, the phase interface of the powder particles shrinks, thereby making the contact between the fumed silica and the boron nitride closer; but too high a temperature may cause the fumed silica to transform from an amorphous form to a crystalline form, thereby causing the fumed silica to fall off, resulting in less fumed silica on the boron nitride, and affecting the reaction activity of the grafting reaction during the silane coupling agent modification. When the temperature exceeds 1300°C, the fumed silica will crystallize, resulting in a decrease in the fumed silica, thereby affecting the next step of the silane coupling agent grafting reaction.

[0052] (3) The high-temperature primary product obtained in (2) is naturally cooled to room temperature.

[0053] (4) Same as steps (2), (3) and (4) of Example 1.

[0054] Example 3

[0055] (1) Same as Example 1.

[0056] (2) The product obtained in (1) is placed in a sintering furnace and kept at 300°C, 600°C, 800°C and 1000°C for 2 h to 6 h, respectively.

[0057] (3) The high-temperature initial product obtained in (2) was naturally cooled to room temperature, and the surface morphology of each was observed by electron microscopy. It was found that the fumed silica coating at 800°C was more dense, followed by 600°C and 1000°C.

[0058] Example 4

[0059] (1) Same as Example 1.

[0060] (2) Same as Example 1.

[0061] (3) Same as Example 1.

[0062] (4) Same as Example 1.

[0063] (5) Add the modified boron nitride obtained in (4) into a clean double cone mixer and mix again for 20 min to 40 min to ensure that the modified boron nitride is evenly mixed.

[0064] Example 5

[0065] (1) Weigh 10 kg of boron nitride powder and 50 g of fumed silica (mass ratio of 1000:5) respectively, add them into five double cone mixers and mix them for 1 hour to make the fumed silica powder and boron nitride powder evenly mixed to obtain a primary product.

[0066] (2) Heating and curing the primary product: The primary product is placed in a sintering furnace and heated and cured at 800°C for 4 hours, so that the fumed silicon dioxide is tightly coated on the boron nitride.

[0067] (3) The high-temperature initial product is cooled to room temperature by autothermal cooling.

[0068] (4) Preparation of silane coupling agent aqueous solution: Weigh 100 kg of pure water, add 0 g, 10 g, 40 g, 70 g and 100 g of KH-560 silane coupling agent respectively, and stir in a stirring kettle at a speed of 300 r / min for 10 min. During the stirring process, the KH-560 silane coupling agent is hydrolyzed into silanol to obtain a mixed solution.

[0069] (5) The cooled primary product is added to the mixed solution and stirring is continued for 3 hours. During the stirring process, the KH-560 silane coupling agent undergoes a dehydration reaction with the hydroxyl groups on the surface of the fumed silica-coated boron nitride, thereby being grafted onto the fumed silica-coated boron nitride to obtain a dispersion.

[0070] (6) The dispersion was filtered and baked in an oven at 105°C for 6 hours to obtain modified boron nitride.

[0071] (7) Pour the modified boron nitride into five clean double cone mixers and mix again for 30 minutes.

[0072] (8) The modified boron nitride obtained in step (7) was mixed with epoxy resin in the same amount and the viscosity of the epoxy resin mixture, the maximum filling amount of the epoxy resin mixture after curing, and the thermal conductivity at the maximum filling amount were tested. The test results are shown in Table 1:

[0073] Table 1

[0074] KH-560 addition amount Viscosity (mPa·s) Maximum filling amount Thermal conductivity (W / m·K) 0g 922349 34.8% 1.3 10g 817855 37.1% 1.62 40g 507358 44.9% 2.03 70g 633194 41.7% 1.86 100g 692486 39.5% 1.79

[0075] It is understandable that in this embodiment, in order to adapt to the epoxy resin, other epoxy groups can also be selected.

[0076] Comparative Example 1

[0077] (1) Same as Example 5. The only difference is that no fumed silica is added.

[0078] (2) Same as Example 5.

[0079] (3) Same as Example 5.

[0080] (4) Same as Example 5.

[0081] (5) Same as Example 5.

[0082] (6) Same as Example 5.

[0083] (7) Same as Example 5.

[0084] (8) Same as Example 5. The test results are shown in Table 2:

[0085] Table 2

[0086] KH-560 addition amount Viscosity (mPa·s) Maximum filling amount Thermal conductivity (W / m·K) 0g 922198 32.4% 1.1 10g 869765 33.9% 1.28 40g 652349 40.8% 1.82 70g 798326 37.5% 1.63 100g 832134 36.3% 1.51

[0087] By comparing Table 1 and Table 2, the modified boron nitride obtained by the modification method of the present invention has better dispersibility than the method of directly modifying boron nitride with a silane coupling agent, and the maximum filling amount in the epoxy resin is increased by about 10%, and the thermal conductivity of the boron nitride / epoxy resin composite material is increased by about 20%. This shows that the modified boron nitride obtained by adding fumed silica and boron nitride for dry mixing, successfully coating fumed silica on boron nitride, and then modifying it with a silane coupling agent has better dispersibility and higher filling amount.

[0088] In summary, the boron nitride modification method provided by the embodiment of the present invention is to dry-mix fumed silica and boron nitride, and during the mixing process, the fumed silica is coated on the surface of the boron nitride, so that the surface of the boron nitride is modified with hydroxyl groups; then the silane coupling agent is used for modification, and the silane coupling agent and the hydroxyl groups on the surface of the boron nitride undergo a dehydration reaction, so that the silane coupling agent is grafted on the surface of the boron nitride; the modified boron nitride prepared by this method has good dispersibility, and when used as a thermal conductive filler for a composite material, it has a higher filling amount, which is beneficial to improve the thermal conductivity of the composite material; and compared with the existing boron nitride modification method, the modification method provided by the present invention has the characteristics of mild conditions, easy operation, safety and environmental protection, and a wide range of applications.

[0089] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A boron nitride modification method, It is characterized in that The following steps are involved: S1. Adding boron nitride and fumed silica into a mixing treatment device and mixing for 1 hour to obtain a primary product; the mass ratio of boron nitride to fumed silica is 1000:5; S2, heating and curing the primary product obtained in step S1 at 800° C. for 4 hours, and then cooling to room temperature; S3, adding a silane coupling agent to pure water, and performing hydrolysis stirring in a stirring treatment device for 10 minutes to obtain a mixed solution; the mass ratio of pure water to the silane coupling agent is 2.5:1 or 10:7; the mass ratio of the silane coupling agent to the boron nitride powder is 1:250 or 7:1000; S4, adding the cooled primary product obtained in step S2 to the mixed solution obtained in step S3 and stirring and mixing for 3 hours to achieve a grafting reaction and obtain a dispersion; S5. After the grafting reaction is completed, the dispersion obtained in step S4 is filtered and dried at 105° C. for 6 h to obtain modified boron nitride.

2. A modified boron nitride product obtained by the boron nitride modification method according to claim 1.

3. Use of the modified boron nitride product as claimed in claim 2 as a thermally conductive filler for composite materials.