Diamond grinding paste and preparation method thereof

By using components such as coupled diamond micropowder and spherical alumina powder in the diamond abrasive paste, the performance of the abrasive paste is optimized, which solves the problems of poor fluidity, high temperature and large surface roughness during the grinding and polishing process, and achieves high efficiency. , easy-to-clean grinding effect, meeting the precision processing needs of high-hardness materials.

CN116083052BActive Publication Date: 2024-10-22BEIJING GRISH HITECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211727720.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-31
Publication Date
2024-10-22
Estimated Expiration
2042-12-31

AI Technical Summary

Technical Problem

During the precision and ultra-precision grinding and polishing process, existing diamond abrasive pastes have problems such as poor fluidity, excessive temperature on the grinding disc surface, large surface roughness of the workpiece, poor smoothness, and difficulty in cleaning. They cannot meet the needs of high-precision processing of high-hardness materials.

Method used

Coupled diamond micropowder and spherical alumina powder are used, combined with an appropriate amount of liquid oil, metallic copper powder, lubricant, anti-wear agent and amphiphilic organic matter to optimize the dispersion, thermal conductivity and consistency of the grinding paste and improve its fluidity and cleaning performance, reducing grinding disc temperature and surface roughness.

Benefits of technology

It achieves the controllable surface temperature of the grinding disc, improves the surface finish of the workpiece, improves the grinding efficiency, and makes the workpiece easy to clean, overcomes the poor fluidity and bonding problems of traditional grinding paste, and significantly improves processing efficiency and product quality.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a diamond grinding paste and a manufacturing method thereof. The diamond grinding paste is mainly composed of the following components: grinding micropowder, liquid oil and grinding aid; wherein the grinding micropowder includes coupling-treated diamond micropowder and spherical alumina powder; the liquid oil includes a mixture of one or more of solvent oil, synthetic oil and saturated alcohol polymer; the grinding aid includes metal copper powder, sorbitol fatty acid ester, wetting dispersant, lubricant, anti-wear agent, amphiphilic organic matter and thickener. The diamond grinding paste of the present invention improves the dispersibility and grinding performance of the diamond micropowder by adding spherical alumina powder. At the same time, the spherical alumina powder also plays a role in reducing the temperature of the grinding disc during the grinding process; the grinding disc temperature during the grinding process and the surface roughness of the workpiece being processed are reduced by adding metal copper powder, lubricant, anti-wear agent and using specific liquid oil; the cleaning performance of the diamond grinding paste is improved by adding specific amphiphilic organic matter; the consistency of the grinding paste is adjusted by adding a thickener, thereby improving its use performance and grinding performance. The diamond grinding paste of the invention has the outstanding characteristics of good dispersibility, good fluidity, high grinding rate, controllable grinding disc temperature, high workpiece surface finish, no sticking to the workpiece, and easy cleaning, and can improve grinding processing efficiency and reduce processing costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material precision processing, and in particular to a diamond grinding paste and a preparation method and application thereof. Background Art

[0002] At present, as a key technology in the equipment manufacturing industry, precision and ultra-precision machining technology has long been the focus of research and development and application in countries around the world. With the rapid development of this machining technology, its application in my country is no longer limited to a few fields such as cutting-edge national defense and aerospace, and has expanded to various fields of the national economy, such as precision and ultra-precision machining technology for small and ultra-small electronic and optical parts in sound, light, imaging, and office equipment. Its application scale has increased year by year, from single-piece small-batch production to large-scale production. With the continuous emergence of new products, the application scope of precision and ultra-precision machining will be further expanded.

[0003] Precision and ultra-precision machining technology has become the foundation of the current high-tech field. In view of the rapid development of advanced manufacturing technology, the requirements for precision are getting higher and higher. Conventional processes can no longer meet the requirements of high-precision manufacturing, and precision and ultra-precision machining technology is urgently needed to support it.

[0004] When performing precision and ultra-precision machining, the final process is often precision and ultra-precision grinding and polishing. During precision and ultra-precision grinding and polishing, grinding consumables such as diamond grinding paste are generally required. There are two main types of existing diamond grinding pastes, namely water-soluble diamond grinding paste and oil-soluble diamond grinding paste. Compared with the defects of low polishing rate and large workpiece surface roughness of water-based diamond grinding paste, oil-based diamond grinding paste has higher grinding rate, better workpiece surface processing quality and better performance. However, traditional oil-based diamond grinding paste has the defects of poor fluidity, poor wetting and lubrication properties, large surface roughness, poor finish, easy adhesion to the workpiece, and difficult cleaning. In addition, during the grinding and polishing process, there is often a problem that the heat generated by continuous mechanical grinding and polishing under high pressure cannot be dissipated in time, resulting in excessively high local temperature of the polished workpiece, which affects the polishing effect and cannot meet the high demands of precision and ultra-precision machining. A Chinese patent (publication number CN 107400499 A) discloses a diamond grinding paste and a preparation method thereof. The invention is an oily diamond grinding paste, which has the defects of poor wetting and lubrication performance, excessively high local temperature of the polished workpiece surface, large surface roughness, poor surface finish, easy adhesion to the workpiece, and difficult cleaning. A Chinese patent (publication number CN 104017499 A) discloses a diamond grinding paste, which also has the above-mentioned defects.

[0005] In view of this, the present invention is proposed. The present invention can be widely used in the grinding and polishing of various molds, metallography, optical crystals, ball valves, hard alloys, zirconium oxide dentures and other high-hardness materials. Summary of the invention

[0006] The first purpose of the present invention is to provide a diamond grinding paste which can be widely used in the grinding and polishing of high-hardness materials such as various molds, metallography, optical crystals, ball valves, cemented carbide and zirconia dentures. The diamond grinding paste has the outstanding characteristics of good dispersibility, good fluidity, high polishing yield, controllable grinding disc surface temperature, high workpiece surface finish, no sticking to the workpiece, and easy cleaning. In the process of precision and ultra-precision grinding and polishing, the grinding disc surface temperature is relatively moderate, and the problems of excessively high grinding disc surface temperature and excessively large roughness of the workpiece grinding disc surface will not occur. The problems of excessively high grinding disc surface temperature, excessively large workpiece surface roughness, and poor finish existing in traditional diamond grinding pastes in the prior art are overcome. At the same time, the problems of poor fluidity, severe scratches, sticking to the workpiece, and difficulty in cleaning existing in the grinding pastes in the prior art are also overcome.

[0007] The second purpose of the present invention is to provide a method for preparing diamond polishing paste, which has closely connected steps, is simple and fast, easy to operate, and has mild operating conditions, can realize industrial production, and has good economic benefits.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] A diamond grinding paste, wherein the diamond grinding paste is mainly made of the following components in parts by weight:

[0010] 5-15 parts of grinding powder, 20-40 parts of liquid oil and 15-70 parts of grinding aid.

[0011] Wherein, the grinding micro-powder comprises coupled treated diamond micro-powder and spherical alumina powder, and the addition amount of the spherical alumina powder accounts for 1-5% of the mass of the diamond micro-powder;

[0012] The liquid oil includes solvent oil, synthetic oil, saturated alcohol polymer or a mixture of the above;

[0013] The grinding aid comprises, by weight: 2-10 parts of metal copper powder, 2-10 parts of sorbitol fatty acid ester, 2-10 parts of wetting and dispersing agent, 2-10 parts of lubricant, 2-10 parts of anti-wear agent, 3-15 parts of amphiphilic organic matter and 2-5 parts of thickener.

[0014] Preferably, the diamond grinding paste is mainly made of the following components in parts by weight:

[0015] 8-12 parts of grinding powder, 25-35 parts of liquid oil and 23-56 parts of grinding aid.

[0016] The amount of the spherical alumina powder added is 3% of the mass of the diamond powder; the mass ratio of the solvent oil, the synthetic oil and the saturated alcohol polymer in the liquid oil is (1-3):(1-3):(1-3), and more preferably, the mass ratio of the solvent oil, the synthetic oil and the saturated alcohol polymer is 1:1:2;

[0017] The grinding aid comprises, by weight: 4-8 parts of metal copper powder, 3-8 parts of sorbitol fatty acid ester, 3-8 parts of wetting dispersant, 3-8 parts of lubricant, 3-8 parts of anti-wear agent, 4-13 parts of amphiphilic organic matter and 3 parts of thickener.

[0018] In the prior art, traditional diamond grinding paste has the problems of poor fluidity, severe scratches, easy adhesion to the workpiece and difficulty in cleaning during the precision and ultra-precision grinding and polishing process, and also has the problems of high grinding disc surface temperature and large surface roughness. This can be analyzed from the following two aspects: on the one hand, it is related to the grinding process, such as pressure, rotation speed, external environment and other factors. Under the same other conditions, the greater the pressure and / or rotation speed, the more severe the friction between the workpiece and the grinding disc, the higher the local heat generated, and thus the higher the grinding disc surface temperature. On the other hand, it is mainly related to the grinding paste. The selection and ratio of the micropowder, additives, and liquid oil used in the grinding paste will affect the performance of the grinding paste to a certain extent.

[0019] In order to solve the above technical problems, the present invention provides a diamond grinding paste, and the components and proportions thereof are studied and explored to obtain a diamond grinding paste with relatively excellent performance in all aspects.

[0020] The present invention can effectively improve the dispersibility and compatibility of the diamond micropowder in the liquid oil by using the diamond micropowder subjected to coupling treatment, and can effectively improve the grinding performance of the diamond grinding paste.

[0021] The present invention adds a proper amount of spherical alumina powder to liquid oil. Firstly, since diamond micropowder is easy to agglomerate, adding a proper amount of spherical alumina powder during the preparation process can improve the dispersion performance of diamond micropowder in the grinding paste. Secondly, the spherical alumina powder can play a role of chemical polishing during the grinding and polishing process, which can significantly improve the grinding performance of the grinding paste. Thirdly, the spherical alumina powder has good thermal conductivity and can reduce the temperature of the grinding disc during the grinding process.

[0022] The invention adds a special wetting dispersant into the liquid oil to improve the dispersibility and wetting properties of the grinding paste.

[0023] The present invention improves the thermal conductivity of the grinding paste by adding metal copper powder to the liquid oil. The excellent thermal conductivity can effectively reduce the grinding disc temperature generated by the grinding paste during the grinding process, and will not cause the problem of excessive grinding disc temperature and excessive roughness of the surface of the polished workpiece.

[0024] The present invention adds lubricant to liquid oil so that polar molecules in the lubricant are adsorbed on the grinding disc surface and the workpiece surface during precision grinding, thereby reducing mechanical friction and wear between the workpiece and the grinding disc surface, thereby achieving the effect of lowering the disc surface temperature and reducing surface roughness.

[0025] The present invention improves the load-bearing capacity of the grinding paste by adding an anti-wear agent to the liquid oil, which can effectively reduce the friction and scratches on the grinding disc surface caused by high-load grinding and polishing conditions, thereby slowing down the temperature increase rate of the grinding disc surface.

[0026] The present invention adds a proper amount of thickener to the liquid oil and controls the consistency of the grinding paste (measured in cone penetration units) within the range of 265 to 320, thereby ensuring that the grinding paste is not only in a paste state but also has a certain fluidity, so as to facilitate the effective use of the grinding paste and control the temperature of the grinding disc during the grinding process. There are three reasons for controlling the consistency of the grinding paste: ① The grinding paste will not be thrown out of the grinding tool or the micro-powder will not be separated from the matrix during the grinding process due to too low consistency, which will not play a grinding role, nor will the micro-powder be unevenly dispersed or the grinding paste cannot be evenly applied to the grinding disc due to too high a consistency, which will affect the use; ② If the grinding paste is too thick, its fluidity is relatively poor, which will not only affect the use, but also stick to the grinding disc or the workpiece during the grinding process, blocking the grinding disc, resulting in too high a temperature on the grinding disc surface, and then causing the surface roughness of the workpiece to be ground to be too large or even unable to grind; ③ Adding a proper amount of thickener can effectively improve the stability of the grinding paste, and the paste will be stable and non-stratified for a long time during storage, ensuring that the abrasive is in a dispersed and uniform state for a long time, thereby enhancing the use performance of the grinding paste.

[0027] The present invention adds amphiphilic organic matter into liquid oil, which can improve the hydrophilicity of diamond grinding paste on the one hand, so as to improve its cleaning performance. The obtained grinding paste does not stick to the workpiece after grinding and polishing and is easy to clean; on the other hand, it can play a moisturizing role, effectively prevent the grinding paste from solidifying and hardening in the packaging tube, and make the paste have the functions of gloss and the like.

[0028] In addition, it is also particularly important to select and find a suitable type of liquid oil. After effectively combining it with other additives, the diamond grinding paste of the present invention is finally obtained, which has the characteristics of high grinding rate, controllable disk temperature, small surface roughness, non-stick workpiece and easy cleaning, which greatly improves the processing efficiency of the workpiece being ground.

[0029] The diamond powder is one or both of polycrystalline diamond powder and polycrystalline-like diamond powder. The D50 of the coupling-treated diamond powder is 0.5-40 μm, preferably 0.5-20 μm;

[0030] Preferably, the coupling agent is used to couple the diamond powder to obtain the coupled diamond powder; more preferably, the coupling method comprises: dispersing the diamond powder in a coupling agent solution, stirring at 20-60°C for 1-6h, centrifuging at 3000-4000rpm for 2-5min, collecting the precipitate, and drying to obtain the coupled diamond powder. The solvent of the coupling agent solution is a mixture of ethanol and water, preferably the mass ratio of ethanol to water is (3-5):1, and more preferably 4:1.

[0031] Preferably, the amount of coupling agent used is 0.3-3.0% of the mass of diamond powder. The type of coupling agent can be selected according to actual needs. Preferably, silane coupling agent is used, which has the best modification effect on diamond powder. A further preferred coupling agent is γ-methacryloxypropyltrimethoxysilane.

[0032] The liquid oil includes one or a mixture of solvent oil, synthetic oil, and saturated alcohol polymer; preferably, the mass ratio of the solvent oil, synthetic oil, and saturated alcohol polymer in the liquid oil is (1-3):(1-3):(1-3), and more preferably, the mass ratio of the solvent oil, synthetic oil, and saturated alcohol polymer is 1:1:2. Preferably, the solvent oil is one of D100 and D120; the synthetic oil is one of Castrol 980 and Hydrosal G250H; the saturated alcohol polymer is one of polyethylene glycol and polypropylene glycol, preferably one of PEG-1000, PEG-2000, PEG-3000, PEG-6000, and PPG-2000.

[0033] The wetting and dispersing agent includes one or more of polyether-modified silicone, modified polysiloxane, polyacrylate ammonium salt, nonylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, and alkylhydroxyaminoamide, preferably modified polysiloxane.

[0034] The lubricant is one or more of tall oil fatty acid, glycerol tristearate, propylene glycol monolaurate, diethylene glycol distearate, amide borate, and triethanolamine oleate, preferably amide borate. After the lubricant is added, the polar molecules in the lubricant are adsorbed on the surface of the workpiece during the use of the grinding paste to form a boundary oil film, so as to reduce the mechanical friction and wear generated by the workpiece during the grinding process, thereby achieving the effect of cooling and reducing the surface roughness of the workpiece.

[0035] The anti-wear agent comprises one or more of ceramic powder, chlorinated paraffin, fiber filler, aluminum stearate, zinc stearate, borate and sulfide alkyl naphthylamine salt.

[0036] The thickener includes one or more of thickener CS-02, lauramide propylamine oxide, alkyl polyvinyl pyrrolidone, Carbopol Ultrez 20 and non-ionic associative polyurethane thickener.

[0037] The amphiphilic organic matter is a mixture of one or more of alcohol, ether, acid and amine; preferably, the amphiphilic organic matter is a mixture of alcohol and amine, and more preferably, the mass ratio of the amphiphilic organic matter to the alcohol and the amine is 1: 1. By adding a small amount of amphiphilic organic matter to the abrasive paste, the cleaning performance of the abrasive paste can be effectively improved, making it easy to clean the workpiece after grinding.

[0038] The alcohol is preferably a saturated alcohol, more preferably a mixture of one or more of ethylene glycol, polyethylene glycol 400, polyethylene glycol 600 and propylene glycol;

[0039] The ether is preferably aliphatic ether, more preferably one or more of ethyl ether, dimethyl ether and dipropyl ether;

[0040] The acid is preferably a mixture of one or more of carboxylic acid and its salts and sulfonic acid and its salts, preferably one or more of acetic acid, dodecyl sulfonate and dodecylbenzene sulfonate;

[0041] The amine is preferably one or more of ethanolamine, diethanolamine and triethanolamine.

[0042] From the above analysis, we can also know that the addition of each component is to ultimately improve the comprehensive performance of the abrasive paste itself. They all have specific functions and effects, and no component can be missing.

[0043] The present invention also provides a method for preparing a diamond polishing paste, based on the diamond polishing paste as described in any one of the above, comprising the following steps:

[0044] (1) Add the coupling agent to a mixture of ethanol and water in a certain proportion, mix well to obtain a coupling agent solution, then add the diamond powder to the coupling agent solution, stir and disperse at 20-60°C for 1-6 hours, stir and disperse at 50°C for 6 hours, centrifuge at 3000-4000 rpm for 2-5 minutes, collect the precipitate, and dry to obtain the coupled diamond powder;

[0045] (2) fully mixing the diamond powder subjected to the coupling treatment described above with an appropriate amount of spherical alumina powder to obtain mixed ground powder;

[0046] (3) Fully mix the liquid oil, metal copper powder, sorbitol fatty acid ester, wetting and dispersing agent, lubricant and anti-wear agent at 50-60° C. with ultrasonic stirring to obtain a mixed solution for later use;

[0047] (4) adding the mixed ground powder and the amphiphilic organic compound obtained in step (2) to the mixed solution obtained in step (3) respectively under the conditions of 50-60° C., ultrasonic stirring and vacuuming, and dispersing by ultrasonication for 10-20 min. After the dispersion is uniform, adding a thickener, and continuing ultrasonic stirring for 10-20 min to mix uniformly to obtain a mixed slurry;

[0048] (5) The mixed slurry obtained in the above step (4) is naturally cooled. When the temperature drops to 30-40°C, the mixed slurry is dispensed into syringes or other grinding tools and naturally cooled to room temperature to finally obtain diamond grinding paste.

[0049] Preferably, in the above steps (3) and (4), the stirring rate is controlled between 100-300 rpm, and the ultrasonic frequency is controlled between 25-55 kHz.

[0050] In the preparation process of the diamond grinding paste, each operating parameter is controlled within an appropriate range, so that the prepared diamond grinding paste can achieve better performance. For example, the stirring speed should be appropriate so that no obvious vortex is formed. If the stirring speed is too high, the vortex is large and there are many bubbles, which seriously affects the use effect of the grinding paste.

[0051] The diamond grinding paste prepared by the above preparation method overcomes the problems of poor fluidity, poor lubrication performance, easy adhesion to the workpiece and difficulty in cleaning, high surface temperature of the grinding tool and large surface roughness of the diamond grinding paste on the existing market in the process of precision and ultra-precision grinding and polishing. This will greatly improve the grinding and polishing yield and reduce the processing cost of the workpiece to a great extent.

[0052] The diamond grinding paste of the invention has a wide application range and can be widely used in the grinding and polishing of various molds, metallography, ball valves, hard alloys, zirconium oxide dentures and other high-hardness materials.

[0053] Compared with the prior art, the present invention has the following beneficial effects:

[0054] (1) The diamond grinding paste provided by the present invention has the characteristics of controllable grinding disc temperature and small surface roughness during the grinding process of high-hardness materials, which greatly improves the processing efficiency of the workpiece being processed and greatly reduces the processing cost;

[0055] (2) The diamond grinding paste provided by the present invention has stronger grinding force and higher grinding rate, can effectively avoid scratching the workpiece surface during the grinding and polishing process, and has better dispersibility, fluidity and lubrication and anti-wear properties;

[0056] (3) The diamond grinding paste of the present invention is easier to clean than the conventional oily diamond grinding paste. The workpiece after grinding can be directly rinsed with water without the need to use other volatile solvents for cleaning, while the conventional oily diamond grinding paste must be combined with other organic solvents for cleaning;

[0057] (4) The preparation method of the diamond polishing paste provided by the present invention has closely connected steps, is simple and fast, easy to operate, has mild operating conditions, can be industrialized for production, and has very good economic benefits. DETAILED DESCRIPTION

[0058] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0059] The following embodiments are all measured in mass percentage, and the micropowders are all polycrystalline diamond micropowders (D50=9 μm) that have been subjected to coupling treatment. Of course, the particle size of the micropowders can also be 0.5 μm, 1 μm, 5 μm, 20 μm, 40 μm, etc.

[0060] Embodiment 1:

[0061] The method for preparing the diamond polishing film of this embodiment comprises the following steps:

[0062] (1) Add 0.1 g of silane coupling agent to a mixture of 10 g of ethanol and water (mass ratio of ethanol: water = 4:1), mix well to obtain a silane coupling agent solution, then add 10 g of polycrystalline diamond powder with D50 = 9 μm to the silane coupling agent solution, stir and disperse at 50°C for 6 h, centrifuge at 4000 rpm for 5 min, collect the precipitate, and dry to obtain coupled diamond powder;

[0063] (2) The diamond powder subjected to the coupling treatment described above is fully mixed with 0.3 g of spherical alumina powder having a D50 of 8 μm to obtain a mixed ground powder;

[0064] (3) At 50-60° C., 30 g of liquid oil (mass ratio of D120:Castrol980:PEG-2000=1:1:2), 5 g of metal copper powder, 5 g of sorbitan fatty acid ester, 5 g of modified polysiloxane, 5 g of amide borate, and 5 g of ceramic powder were fully mixed under ultrasonic stirring to obtain a mixed solution for later use;

[0065] (4) adding the mixed ground powder obtained in step (2) and 10 g of amphiphilic organic matter (mass ratio of polyethylene glycol 400: triethanolamine = 1:1) to the mixed solution obtained in step (3) at 50-60° C., stirring under ultrasonication and vacuuming, and dispersing under ultrasonication for 10-20 min. After uniform dispersion, adding 3 g of Carbopol Ultrez 20, and continuing ultrasonic stirring for 10-20 min to mix uniformly, to obtain a mixed slurry;

[0066] (5) The mixed slurry obtained in the above step (4) is naturally cooled. When the temperature drops to 30-40° C., the mixed slurry is dispensed into a needle tube or other abrasive tool and naturally cooled to room temperature to finally obtain a diamond grinding paste;

[0067] In the above steps (3) and (4), the stirring rate is 200 rpm and the ultrasonic frequency is 40 kHz.

[0068] Embodiment 2:

[0069] Except that the mass of the polycrystalline diamond powder is changed to 5 g and the mass of the spherical alumina powder is changed to 0.15 g, everything else is the same as Example 1.

[0070] Embodiment 3:

[0071] Except that the mass of the polycrystalline diamond powder is changed to 15 g and the mass of the spherical alumina powder is changed to 0.45 g, everything else is the same as Example 1.

[0072] Embodiment 4:

[0073] Except that the mass of the polycrystalline diamond powder is changed to 8 g and the mass of the spherical alumina powder is changed to 0.24 g, everything else is the same as Example 1.

[0074] Embodiment 5:

[0075] Except that the mass of the polycrystalline diamond powder is changed to 12 g and the mass of the spherical alumina powder is changed to 0.36 g, everything else is the same as Example 1.

[0076] Embodiment 6:

[0077] Except that the mass of the spherical alumina powder is changed to 0.5 g, everything else is the same as Example 1.

[0078] Embodiment 7:

[0079] Except that the mass of the spherical alumina powder is changed to 0.1 g, everything else is the same as Example 1.

[0080] Embodiment 8:

[0081] Except that the liquid oil was adjusted to 30 g of liquid oil (mass ratio of D120:Castrol 980:PEG-2000=1:1:1), the rest was the same as Example 1.

[0082] Embodiment 9:

[0083] Except that the liquid oil was adjusted to 30 g of liquid oil (mass ratio of D120:Castrol 980:PEG-2000=3:2:1), the rest was the same as Example 1.

[0084] Embodiment 10:

[0085] Except that the liquid oil was adjusted to 30 g of liquid oil (mass ratio of D120:Castrol 980:PEG-2000=1:2:3), the rest was the same as Example 1.

[0086] Embodiment 11:

[0087] Except that the mass of the metal copper powder is changed to 2g, the rest is the same as Example 1.

[0088] Embodiment 12:

[0089] Except that the mass of the metal copper powder is changed to 10 g, everything else is the same as Example 1.

[0090] Embodiment 13:

[0091] Except that the mass of the lubricant is changed to 2g, everything else is the same as Example 1.

[0092] Embodiment 14:

[0093] Except that the mass of the lubricant is changed to 10 g, everything else is the same as Example 1.

[0094] Embodiment 15:

[0095] Except that the mass of the anti-wear agent is changed to 2g, the rest is the same as Example 1.

[0096] Embodiment 16:

[0097] Except that the mass of the anti-wear agent is changed to 10 g, the rest is the same as Example 1.

[0098] Embodiment 17:

[0099] Except that the amount of the amphiphilic organic compound (mass ratio of polyethylene glycol 400: triethanolamine = 1:1) was adjusted to 3 g, the rest was the same as in Example 1.

[0100] Embodiment 18:

[0101] Except that the amount of the amphiphilic organic compound (mass ratio of polyethylene glycol 400: triethanolamine = 1:1) was adjusted to 15 g, the rest was the same as in Example 1.

[0102] Embodiment 19:

[0103] Except that the thickener was changed to 3 g of thickener CS-02, the rest was the same as in Example 1.

[0104] Embodiment 20:

[0105] Except that the thickener was changed to 2 g of thickener CS-02, everything else was the same as Example 1.

[0106] Embodiment 21:

[0107] Except that the thickener was changed to 5 g of thickener CS-02, the rest was the same as in Example 1.

[0108] Embodiment 22:

[0109] Except that the thickener is changed to 3 g of alkyl polyvinyl pyrrolidone, the rest is the same as Example 1.

[0110] Embodiment 23:

[0111] Except that the amphiphilic organic substance was changed to 10 g of polyethylene glycol 400, the rest was the same as in Example 1.

[0112] Embodiment 24:

[0113] Except that the anti-wear agent is changed to 5g of zinc stearate, the rest is the same as Example 1.

[0114] Embodiment 25:

[0115] Except that the lubricant was changed to 5 g of diethylene glycol distearate, everything else was the same as in Example 1.

[0116] Embodiment 26:

[0117] Except that the liquid oil was changed to 30 g PEG-3000, everything else was the same as Example 1.

[0118] Comparative Example 1:

[0119] Except that the mass of the polycrystalline diamond powder is changed to 1 g, everything else is the same as Example 1.

[0120] Comparative Example 2:

[0121] Except that the mass of the polycrystalline diamond powder is changed to 30 g, everything else is the same as Example 1.

[0122] Comparative Example 3:

[0123] Except for removing the spherical alumina powder, the rest is the same as Example 1.

[0124] Comparative Example 4:

[0125] Except that the mass of the liquid oil is changed to 5 g, everything else is the same as Example 1.

[0126] Comparative Example 5:

[0127] Except for removing the metal copper powder, the rest is the same as Example 1.

[0128] Comparative Example 6:

[0129] Except for removing the lubricant, everything else is the same as Example 1.

[0130] Comparative Example 7:

[0131] Except for removing the anti-wear agent, the rest is the same as Example 1.

[0132] Comparative Example 8:

[0133] Except for removing the amphiphilic organic matter, the rest is the same as Example 1.

[0134] Comparative Example 9:

[0135] Except for removing the thickener, the rest is the same as Example 1.

[0136] Comparative Example 10:

[0137] Except that the mass of the thickener is changed to 10 g, the rest is the same as Example 1.

[0138] Comparative Example 11

[0139] With reference to an easy-to-clean diamond grinding paste and a preparation method thereof disclosed in a Chinese patent (publication number CN 10578862A), the diamond grinding paste was prepared by the preparation method provided in Example 1 of the present invention.

[0140] Experimental example:

[0141] The performance of the diamond abrasive paste prepared in the above-mentioned Examples 1-26 and Comparative Examples 1-12 was tested, and the results are shown in Table 1 below. The storage time is the time when the diamond abrasive paste is left to stand at room temperature until precipitation occurs; the consistency is measured by the ZHR-5A cone penetration tester of Shanghai Precision Instruments Co., Ltd. The larger the cone penetration value, the thinner the abrasive paste, and vice versa. The roughness of the surface of the workpiece being processed is tested by a conventional roughness meter, and the temperature of the grinding disc surface is tested by a conventional infrared temperature measuring gun.

[0142] On a single-sided grinder, the diamond grinding pastes prepared in the above Examples 1-26 and Comparative Examples 1-11 were evenly coated on the grinding disc, and the sapphire crystal was ground and polished. The grinding pressure was set to 5 kgf, the rotation speed was 500 rpm, and the time was 20 min. The specific grinding test results are described in Tables 1, 2, 3 and 4 below.

[0143] Table 1 Comprehensive performance evaluation of diamond grinding paste

[0144] Example Dispersibility Cleaning performance Consistency (cone penetration unit) Scratches Roughness (Ra, nm) Rate (μm / min) Grinding disc temperature (℃) Example 1 good good 290 No scratches 10 3.0 25 Example 2 good good 320 No scratches 13 2.5 22 Example 3 good good 275 No scratches 14 2.7 27 Example 4 good good 300 No scratches 11 2.8 24 Example 5 good good 280 No scratches 12 2.8 26 Example 6 good good 288 No scratches 11 2.7 26 Example 7 good good 292 No scratches 12 2.6 23 Example 8 good good 305 No scratches 12 2.4 22 Example 9 good good 315 No scratches 13 2.2 20

[0145] Table 2 Comprehensive performance evaluation of diamond grinding paste

[0146] Example Dispersibility Cleaning performance Consistency (cone penetration unit) Scratches Roughness (Ra, nm) Rate (μm / min) Grinding disc temperature (℃) Example 10 good good 270 No scratches 12 2.7 28 Embodiment 11 good good 295 No scratches 14 3.1 27 Example 12 good good 285 No scratches 11 2.6 22 Embodiment 13 good good 291 No scratches 13 3.1 28 Embodiment 14 good good 287 No scratches 11 2.7 23 Embodiment 15 good good 300 No scratches 13 3.0 27 Example 16 good good 275 No scratches 11 2.6 22 Embodiment 17 good good 288 No scratches 12 2.8 27 Embodiment 18 good good 292 No scratches 14 2.1 20

[0147] Table 3 Comprehensive performance evaluation of diamond grinding paste

[0148] Example Dispersibility Cleaning performance Consistency (cone penetration unit) Scratches Roughness (Ra, nm) Rate (μm / min) Grinding disc temperature (℃) Embodiment 19 good good 280 No scratches 12 3.0 26 Embodiment 20 good good 295 No scratches 11 2.7 24 Embodiment 21 good good 265 No scratches 14 2.5 28 Embodiment 22 good good 298 No scratches 11 2.9 25 Embodiment 23 good good 286 No scratches 11 2.9 27 Embodiment 24 good good 293 No scratches 11 2.9 25 Embodiment 25 good good 291 No scratches 12 3.0 26 Embodiment 26 good good 265 No scratches 12 3.1 28

[0149] Table 4 Comprehensive performance evaluation of diamond grinding paste

[0150] Example Dispersibility Cleaning performance Consistency (cone penetration unit) Scratches Roughness (Ra, nm) Rate (μm / min) Grinding disc temperature (℃) Comparative Example 1 good good 355 Scratched 25 0.2 20 Comparative Example 2 good good 225 Scratched 22 2.0 40 Comparative Example 3 bad good 295 Scratched 18 2.6 27 Comparative Example 4 generally generally 235 Scratched 20 2.9 35 Comparative Example 5 good good 296 Scratched 21 3.2 36 Comparative Example 6 good good 298 Scratched 17 3.1 33 Comparative Example 7 good good 299 Scratched 17 3.1 33 Comparative Example 8 good Very bad 270 Scratched 16 3.2 32 Comparative Example 9 good good 330 Scratched 20 1.8 17 Comparative Example 10 Very bad Very bad 245 Scratched 28 2.5 42 Comparative Example 11 Very bad Very bad 370 Scratched 22 1.2 21

[0151] As can be seen from Table 1, Table 2, Table 3 and Table 4 above, the consistency of the diamond grinding paste of Examples 1-26 of the present invention is relatively suitable, and its consistency (measured in cone penetration units) is controlled within the range of 265~320, with excellent grinding and polishing performance and relatively low grinding disc temperature (general market demand: disc temperature ≤30°C). However, in comparison, the grinding pastes obtained in Comparative Examples 2, 4-8 and Comparative Example 10 all have the problem of relatively high disc temperature of the grinding disc during use. When the disc temperature is high, the grinding rate will increase due to the continuous increase in the disc temperature, causing the grinding rate to shift, and ultimately leading to an increase in surface roughness, and the problem of uneven surface of the workpiece being ground appears. By adding the metal copper powder, lubricant and anti-wear agent of the present invention, the effect of reducing the disc temperature and improving the surface roughness can be achieved. On the basis of ensuring the grinding rate, the problems of high disc temperature and large surface roughness commonly found in the grinding paste can be improved by adding an appropriate amount of metal copper powder, lubricant and anti-wear agent. The consistency of the grinding paste obtained in Comparative Example 1 is relatively low, with a consistency of 355. During use, although the disc temperature is relatively low, due to its too low consistency, the grinding paste is thrown out of the disc during the grinding process, and the grinding disc cannot hold the grinding paste at all. Less grinding paste remains on the grinding disc, resulting in a very low grinding rate, which directly affects the processing efficiency. Comparative Example 2 is just the opposite of Comparative Example 1. The consistency of the grinding paste obtained is too high, the fluidity of the grinding paste is relatively poor, and the grinding chips easily clog the grinding disc, which cannot be ground at all, resulting in the problem of high disc temperature and large surface roughness during the grinding process.

[0152] The present invention selects a suitable type of liquid oil, strictly controls the ratio thereof, adds a suitable amount of other additives, and adjusts the consistency of the abrasive paste so that the consistency of the abrasive paste is controlled within a suitable consistency range, thereby significantly improving the grinding performance of the obtained abrasive paste, effectively controlling the disk temperature, and effectively ensuring the surface roughness. The present invention effectively improves the cleaning performance of the oily abrasive paste by adding a suitable amount of amphiphilic organic matter.

[0153] In addition, by comparing Example 1 with Comparative Example 3, it can be seen that adding an appropriate amount of spherical alumina powder can not only effectively improve the dispersion performance of diamond micropowder in the grinding paste, but also play a role in chemical polishing during the grinding and polishing process, which can significantly improve the grinding rate of the grinding paste. In addition, since the spherical alumina powder has good thermal conductivity, it also plays a role in reducing the temperature of the grinding disc during the grinding process.

[0154] Although the present invention has been illustrated and described with specific embodiments, it will be appreciated that many other changes and modifications may be made without departing from the spirit and scope of the present invention. Therefore, it is intended to include all such changes and modifications within the scope of the present invention in the appended claims.

Claims

1. A diamond grinding paste, characterized in that: The invention is mainly composed of the following components by weight: 5-15 parts of grinding micro powder, 20-40 parts of liquid oil and 15-70 parts of grinding aid; The grinding powder includes coupled diamond powder and spherical alumina powder; the addition amount of the spherical alumina powder accounts for 1-5% of the mass of the diamond powder; The liquid oil includes solvent oil, synthetic oil, saturated alcohol polymer or a mixture of the above; The grinding aid comprises, by weight, 2-10 parts of metal copper powder, 2-10 parts of sorbitol fatty acid ester, 2-10 parts of wetting and dispersing agent, 2-10 parts of lubricant, 2-10 parts of anti-wear agent, 3-15 parts of amphiphilic organic matter, and 2-5 parts of thickener; The wetting and dispersing agent includes one or more of polyether-modified silicone, modified polysiloxane, polyacrylate ammonium salt, nonylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, and alkylhydroxyaminoamide; The lubricant is one or more of tall oil fatty acid, glycerol tristearate, propylene glycol monolaurate, diethylene glycol distearate, amide borate, and triethanolamine oleate; The anti-wear agent includes one or more of ceramic powder, chlorinated paraffin, fiber filler, aluminum stearate, zinc stearate, borate and sulfide alkylnaphthylamine salt; The amphiphilic organic substance is a mixture of one or more of alcohol, ether, acid and amine, the alcohol is one or more of ethylene glycol, polyethylene glycol 400, polyethylene glycol 600 and propylene glycol, the ether is one or more of ethyl ether, dimethyl ether and dipropyl ether, the acid is one or more of acetic acid, dodecyl sulfonate and dodecylbenzene sulfonate, and the amine is one or more of ethanolamine, diethanolamine and triethanolamine; The thickener includes one or more of thickener CS-02, lauramide propylamine oxide, alkyl polyvinyl pyrrolidone, Carbopol Ultrez 20 and non-ionic associative polyurethane thickener; The consistency of the grinding paste is controlled within the range of 265 to 320 in terms of cone penetration units.

2. The diamond grinding paste according to claim 1, characterized in that In parts by weight, 8-12 parts of ground micro powder, 25-35 parts of liquid oil and 23-56 parts of grinding aid; The grinding aid comprises, by weight, 4-8 parts of metal copper powder, 3-8 parts of sorbitol fatty acid ester, 3-8 parts of wetting and dispersing agent, 3-8 parts of lubricant, 3-8 parts of antiwear agent, 4-13 parts of amphiphilic organic matter and 3 parts of thickener.

3. The diamond grinding paste according to claim 1, characterized in that The added amount of the spherical aluminum oxide powder accounts for 3% of the mass of the diamond micropowder.

4. The diamond grinding paste according to claim 1, characterized in that The diamond micropowder is one or both of polycrystalline diamond micropowder and polycrystalline-like diamond micropowder; the particle size of the coupling-treated diamond micropowder is 0.5-40 μm.

5. The diamond grinding paste according to claim 4, characterized in that The particle size of the coupling-treated diamond micropowder is 0.5-20 μm; the diameter of the spherical alumina powder is 0.5-20 μm.

6. The diamond grinding paste according to claim 1 or 2, characterized in that: In the liquid oil, the mass ratio of the solvent oil, the synthetic oil and the saturated alcohol polymer is (1-3):(1-3):(1-3).

7. The diamond grinding paste according to claim 6, characterized in that The mass ratio of the solvent oil, the synthetic oil and the saturated alcohol polymer is 1:1:

2.

8. The diamond grinding paste according to claim 6, characterized in that The solvent oil is one of D100 and D120; the synthetic oil is one of Castrol 980 and Hydrosal G250H; and the saturated alcohol polymer is one of polyethylene glycol and polypropylene glycol.

9. The diamond grinding paste according to claim 8, characterized in that The saturated alcohol polymer is one of PEG-1000, PEG-2000, PEG-3000, PEG-6000 and PPG-2000.

10. The diamond grinding paste according to claim 1 or 2, characterized in that: The coupling-treated diamond micropowder is obtained by coupling-treating the diamond micropowder with a coupling agent; The coupling treatment method comprises: dispersing the diamond powder in a coupling agent solution, stirring at 20-60° C. for 1-6 hours, centrifuging at 3000-4000 rpm for 2-5 minutes, collecting the precipitate, and drying to obtain the coupled diamond powder; wherein, The solvent of the coupling agent solution is a mixture of ethanol and water.

11. The diamond grinding paste according to claim 10, characterized in that In the solvent of the coupling agent solution, the mass ratio of the ethanol to the water is (3-5):

1.

12. The diamond grinding paste according to claim 11, characterized in that The mass ratio of the ethanol to the water is 4:

1.

13. The diamond grinding paste according to claim 10, characterized in that The amount of the coupling agent is 0.3-3.0% of the mass of the diamond micropowder; the coupling agent is a silane coupling agent.

14. The diamond grinding paste according to claim 13, characterized in that The coupling agent is γ-methacryloxypropyltrimethoxysilane.

15. The diamond grinding paste according to claim 1 or 2, characterized in that: The wetting and dispersing agent is modified polysiloxane; The lubricant is an amide borate.

16. The diamond polishing paste according to claim 1 or 2, characterized in that: The amphiphilic organic substance is a mixture of the alcohol and the amine, and in the amphiphilic organic substance, the mass ratio of the alcohol to the amine is 1:

1.

17. The method for preparing a diamond polishing paste according to claim 1, characterized in that: The steps include: (1) adding a coupling agent to a mixture of ethanol and water in a certain proportion, mixing uniformly to obtain a coupling agent solution, then adding diamond powder to the coupling agent solution, stirring and dispersing at 20-60° C. for 1-6 hours, centrifuging at a speed of 3000-4000 rpm for 2-5 minutes, collecting the precipitate, and drying to obtain coupling-treated diamond powder; (2) fully mixing the coupling-treated diamond micropowder and an appropriate amount of spherical alumina micropowder to obtain a mixed ground micropowder; (3) at 50-60° C., under ultrasonic stirring, the liquid oil, the metal copper powder, the sorbitan fatty acid ester, the wetting and dispersing agent, the lubricant, and the anti-wear agent are fully mixed to obtain a mixed solution for standby use; (4) adding the mixed ground powder and the amphiphilic organic compound obtained in step (2) to the mixed solution obtained in step (3) respectively under the conditions of 50-60° C., ultrasonic stirring and vacuuming, and ultrasonically dispersing for 10-20 minutes. After uniform dispersion, adding a thickener, and continuing ultrasonic stirring for 10-20 minutes to mix uniformly, thereby obtaining a mixed slurry; (5) The mixed slurry obtained in the above step (4) is naturally cooled. When the temperature drops to 30-40° C., the mixed slurry is dispensed into syringes or other grinding tools and naturally cooled to room temperature to finally obtain a diamond grinding paste.

18. The method for preparing diamond polishing paste according to claim 17, characterized in that: In steps (3) and (4), the stirring rate is controlled between 100-300 rpm, and the ultrasonic frequency is controlled between 25-55 kHz.