Steaming method

Through pre-steam treatment and grinding compression steps, the yield of high molecular weight xylan and lignin is improved, the problems of long cooking time and low yield are solved, and high-efficiency and low energy consumption are achieved, and the product is improved. Quality and recovery rate.

CN116113737BActive Publication Date: 2024-11-29AMPPC FINLAND OY
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202180047853.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-23
Publication Date
2024-11-29
Estimated Expiration
2041-06-23

AI Technical Summary

Technical Problem

In the existing pulping process, the long cooking time and the high degradation rate of hemicellulose lead to low yield of dissolved pulp, and residual hemicellulose affects textile mechanical properties, and conventional processes consume high energy and low yield.

Method used

Using pre-steam treatment, pre-hydrolysis and grinding compression steps, lignocellulose raw materials are treated by steam or water, high molecular weight xylan and lignin are released, and steamed in a cooking liquid containing sodium hydroxide or organic acids to reduce steaming time, increase yield and molecular weight.

Benefits of technology

It improves the yield of high molecular weight xylan, lignin and dissolved slurry, reduces energy consumption and cooking time, reduces hemicellulose content, improves the brightness and viscosity of the product, and the recovery rate of value-added products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116113737B_ABST
    Figure CN116113737B_ABST
Patent Text Reader

Abstract

The present invention discloses a cooking process in which partially digested lignocellulosic feedstock is compressed during cooking to provide high molecular weight xylan, lignin and pulp.
Need to check novelty before this filing date? Find Prior Art

Description

Field of the Invention

[0001] The present disclosure relates to a cooking method for producing a combination of high yield and high molecular weight (HMW) xylan, HMW lignin, sulfite and dissolving pulp from a cellulose fiber source, and to a digester system in which the cooking method can be used. The pulp produced according to the method can be used to make paper grade pulp, dissolving cellulose products and cellulose derivatives. Background of the Invention

[0003] Pulp, also known as paper pulp or dissolved cellulose, is a bleached wood pulp with a high cellulose content and is chemically produced from wood using the soda process or the kraft process. The Kraft process and the soda process are commonly used pulping processes, and in the traditional Kraft process, the wood is treated with an aqueous mixture of sodium hydroxide and sodium sulfide. In the soda process, the wood is treated with sodium hydroxide. This treatment degrades and dissolves lignin, resulting in fiber separation of wood fibers.

[0004] Generally, wood pulp containing high levels of alpha cellulose is known in the art as dissolving pulp, and it is used to make cellulose derivatives and products for a variety of uses. Other terms synonymous with dissolving pulp are chemical cellulose and special high alpha pulp. Dissolving pulp is usually made using two processes, namely:

[0005] 1) the acid sulfite process, the development of which began around the beginning of this century (Rydholm, SA, Pulping Processes, p. 280, Interscience Publishers, New York-London-Sydney 1965); and

[0006] 2) Prehydrolysis - the Kraft process, development of which began in 1929 (Rydholm, supra - p. 281).

[0007] The latter process utilizes an acid pretreatment ("prehydrolysis") step to remove hemicellulose prior to the alkaline pulping (delignification) step. South African Patent 88 / 4037 discloses a prehydrolysis-neutral sulfite-anthraquinone process (PH-NS-AO) for making "hemicellulose hydrolysates and special pulps" (high alpha grade). The prehydrolysis step performs essentially the same function as the prehydrolysis step prior to the Kraft (sulfate) pulping process for making dissolving grade pulp; although the neutral sulfite-anthraquinone delignification step is essentially the same as the process also known as the semi-alkaline sulfite-anthraquinone (SAS-AQ) process, which was first reported by Raubenheimer, S and Eggers, SH at a 1979 technical conference (both of whom were researchers employed by SAPPI LIMITED, the applicants herein), namely the 11th European ESPRA Conference held during May 1979, Maastricht, the Netherlands.

[0008] In addition, the conventional production of paper and dissolving pulp by the kraft process or soda process including a prehydrolysis step has a low yield because the hemicellulose and cellulose in the wood are degraded in the process, mainly in the prehydrolysis step, and are transferred to the acid condensate as low molecular weight hemicellulose, monosaccharides and hemicellulose degradation products. Since the cooking time is very long, the hemicellulose and cellulose in the wood are degraded during the cooking process, so the yield of the soda process is low. Due to the difficulty in extracting these degradation products from the digester, the degraded material is preferably used for energy production by evaporating and burning the components, or simply discarded as waste.

[0009] WO 99 / 47733 discloses a process for producing cellulose fibers, wherein the degree of polymerization of the fibers obtained can be adjusted via acid hydrolysis and oxidative degradation. However, the kraft pulp obtained by this process has a large amount of residual hemicellulose, which makes the obtained pulp less useful for the production of regenerated cellulose for, for example, textile applications, since these residual compounds have a negative impact on the process behavior and therefore also on the textile mechanical properties of the fibers produced therefrom.

[0010] US 2009 / 0312536 discloses a process for producing dissolving pulp suitable for textile applications from a cellulosic raw material using the kraft process combined with a purification step of the cold caustic extraction (CCE) type.

[0011] WO2011 / 138633 and WO2011 / 138634 both disclose pulp processing methods including a cold caustic extraction step. However, the disclosed methods describe expensive processes with low overall yields of dissolving pulp.

[0012] It is therefore an object of the present disclosure to provide an improved industrial scale cooking process for producing high yield dissolving pulp which has a low hemicellulose content and which can be easily delignified and bleached to desired brightness and viscosity levels.

[0013] Another object is to provide a cooking system for lignocellulosic feedstocks that provides a pulp free of sulfur compounds, high molecular weight xylans and high molecular weight lignin. SUMMARY OF THE INVENTION

[0015] At least some of the above objects and other objects can be obtained by the present invention as defined in the independent claims. The present invention has the advantage that it can produce value-added products such as HMW hemicellulose, HMW xylan and HMW lignin from lignocellulosic raw materials for pulping. In addition, the present invention uses less energy in the production of dissolving pulp or paper grade pulp compared to conventional pulping processes.

[0016] The invention also allows to reduce processing time and / or cooking time. Another advantage is that in the present process the total yield of paper and dissolving pulp is higher than that achievable using conventional prehydrolysis-soda, prehydrolysis-kraft or sulfite processes in the production of paper or dissolving grade pulp. The embodiments described below provide further advantages.

[0017] According to a first aspect, there is provided a cooking method, comprising:

[0018] a) providing a lignocellulosic raw material, which comprises wood chips, pin chips, wood shavings, sawdust or a combination thereof;

[0019] b) pretreating the lignocellulosic feedstock by subjecting it to a steam treatment to provide a pretreated material;

[0020] c) optionally prehydrolyzing the pretreated material with steam or water to provide a prehydrolyzed material;

[0021] d) optionally grinding and compressing the pretreated material and / or prehydrolyzed material to release the HMW xylan from the pretreated and / or prehydrolyzed material into a hydrolysate, and recovering the hydrolysate containing the HMW xyloglucan;

[0022] e) neutralization with sodium hydroxide containing sulfur or with sodium hydroxide, or replacement with an organic acid selected from lactic acid, acetic acid, formic acid, citric acid, oxalic acid, uric acid and malic acid;

[0023] f) cooking in a cooking liquor comprising sodium hydroxide or sodium hydroxide with sulfur, or an organic acid selected from the group consisting of lactic acid, acetic acid, formic acid, citric acid, oxalic acid, uric acid and malic acid to provide a cooked cellulosic material in a spent liquor;

[0024] g) grinding and compressing the cooked cellulosic material to release HMW lignin from the cooked material into the spent liquor, thereby providing a HMW lignin fraction in black liquor and a compressed cellulose fraction.

[0025] H) replacing the spent cooking liquor with a replacement liquor containing 1% to 40% of effective alkali as NaOH or acidic sulfite cooking liquor, or with an organic acid selected from the group consisting of lactic acid, acetic acid, formic acid, citric acid, oxalic acid, uric acid and malic acid;

[0026] i) recovering said HMW lignin from the HMW lignin fraction in said black liquor and from said displacement liquor; and

[0027] j) recovering dissolving pulp from said compressed cellulose fraction.

[0028] The cooking method of the present invention is advantageous in that it can provide the combined production of HMW hemicellulose, HMW xylan, HMW lignin and dissolving pulp. In particular, HMW xylan can be produced in the present method by opening the fiber cell wall structure by prehydrolysis and then pushing HMW xylan out of the fiber cell wall by compression.

[0029] The method improves at least one of the xylan yield, the lignin yield and the cellulose yield, and reduces wood consumption, cooking time and the amount of water in the lignin-containing fraction. These effects have the advantage of lower evaporation energy consumption. In addition, the method makes it possible to recover the high-value products HMW xylan and HMW lignin in the pulping process.

[0030] According to a second aspect, there is provided a HMW xylan fraction obtainable using the present method.

[0031] As shown in the Examples, the present method provides xylans with higher molecular weight, higher xylan yield and higher xyloglucan concentration in the HMW xylan fraction compared to prior art cooking processes.

[0032] According to a third aspect, there is provided a HMW lignin fraction obtainable using the present method.

[0033] With the process of the invention, a HMW lignin fraction with better lignin yield and higher consistency can be obtained. The HMW lignin also has an increased molecular weight compared to lignin produced according to prior art processes, such as the lignin disclosed in PCT / FI2011 / 050651.

[0034] According to a fourth aspect, there is provided a pulp obtainable by using the present method. The pulp obtained according to the present method may have a higher brightness and require less wet pressing and lower steam consumption during drying than pulp produced according to prior art methods. The dissolving pulp may additionally have a lower hemicellulose content than conventionally produced pulp.

[0035] Embodiments of the present disclosure provide certain benefits. Depending on the embodiment, one or more of the following benefits may be achieved: reduced consumption of chemicals, water, cellulose fiber sources, and energy; increased yield of cellulose, increased molecular weight of xylan and lignin.

[0036] BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 Schematically illustrated is an embodiment of the present cooking process involving pre-steaming and pre-hydrolysis of lignocellulosic feedstock and a digester system for grinding and / or compressing condensate from the wood chips after pre-hydrolysis. Figure 1 The process parameters mentioned in are exemplary only, and other process parameters may be used as described in the present disclosure.

[0038] Figure 2 An embodiment of a digester system for compressing cooking liquor from wood chips in pre-hydrolyzed kraft or soda cooking is schematically shown. Figure 2 The process parameters mentioned in are exemplary only, and other process parameters may be used as described in the present disclosure.

[0039] Figure 3 An embodiment of an illustrative process for compressing wood chips to press out cooking liquor is shown. Figure 3 The process parameters mentioned in are exemplary only, and other process parameters may be used as described in the present disclosure.

[0040] Figure 4 An embodiment of a process for displacing spent liquor from compressed wood chips is schematically shown. Figure 4 The process parameters mentioned in are exemplary only, and other process parameters may be used as described in the present disclosure. DETAILED DESCRIPTION OF THE INVENTION

[0042] As used herein, the term "comprising" includes the broader meanings of "including," "containing," and "comprehending," as well as the narrower expressions "consisting of" and "consisting only of."

[0043] In one embodiment, the process steps are performed in the order identified in any aspect, embodiment or claim. In another embodiment, any process step specified to be performed on a product or intermediate obtained in a previous process step is performed directly on said product, i.e., without an additional, optional or auxiliary processing step between said two steps that chemically or physically changes the product.

[0044] In one embodiment, the lignocellulosic raw material used in the cooking method is in the form of wood chips, wood strands, wood shavings, sawdust or a combination thereof. Preferably, wood chips are used, more preferably softwood or hardwood chips, such as eucalyptus, pine or spruce chips. However, when wood chips are used as the main raw material, the raw material may contain a smaller amount of, for example, wood strands and / or sawdust.

[0045] Unless otherwise stated, all percentage values ​​refer to % by dry weight.

[0046] This process is suitable for a plant or mill, i.e. an industrial (large) scale process.

[0047] refer to Figure 1 In one embodiment, pretreatment includes steaming of the chips, which can be performed in a silo by supplying 3.5 bar steam for 30 min. In one embodiment, prehydrolysis can be performed at 175°C for 20 min. In one embodiment, cooking can be performed at 155°C in cooking liquor for 50-70 min.

[0048] refer to Figure 2 In one embodiment, cooking is performed in a cooking vessel operated at 155°C for 50-70 min, compression is performed at 155°C for 50-70 min, and displacement is performed at 90°C.

[0049] refer to Figure 3 In one embodiment, the wood chips from the cooking step are fed to the grinding and compression step at 155°C and a Kappa number of 100-2, where they are passed through a gap of 7 mm.

[0050] refer to Figure 4 In one embodiment, a column of wood chips is compressed at 1 bar at 90°C in the presence of a liquor containing 1-15 g / l effective alkali, which allows the collection of high molecular weight waste liquor (containing HMW lignin) and cellulose.

[0051] In one embodiment, the lignocellulosic feedstock has a xylan content of 4 wt% or more.

[0052] The term high molecular weight xylan (HMW xylan) means xylan having an average weight molecular weight (MW) of 45 000 g / mol or more for hardwoods and softwoods.

[0053] The term high molecular weight lignin (HMW lignin) means lignin having an average weight molecular weight (MW) of 4580 g / mol or more for hardwoods and 4980 g / mol or more for softwoods.

[0054] In one embodiment, the molecular weight is measured by size exclusion chromatography and expressed as an average molecular weight (MW).

[0055] Hemicellulose may be recovered from the hydrolysate in step d.

[0056] According to one embodiment, the pretreatment is preferably performed by steam treatment to achieve exhaust of air inside the wood chips, thereby increasing the liquid permeability of the porous wood raw material. Pre-steaming can be performed in a separate steam tank or a wood chip silo. The steam treatment is performed by using low-pressure steam at a pressure of about 3.5 bar for at least 10 minutes, preferably more than 20 minutes. In one embodiment, the pre-steaming includes pre-steaming with low-pressure steam at 1-4 bar for 1-100 minutes to provide a pre-treated material.

[0057] The temperature used in the pretreatment is preferably selected from the range of 80-120°C, more preferably the range of 100-120°C, and even more preferably the range of 110-120°C.

[0058] In one embodiment, the prehydrolysis is performed by steam or water at a temperature selected from the range of 150-220° C. In one embodiment, the prehydrolysis step comprises prehydrolysis with 8-15 bar steam at a temperature selected from the range of 150-220° C. for 1-150 min.

[0059] Wood chips generally have a generally rectangular shape, with a height, a length and a width. However, the geometry of the wood chips may vary, for example, depending on their manufacturing process. The length (longest dimension) and the width (second longest dimension) of the wood chip may be considered to determine the general "flat side" of the wood chip, and the thickness is the smallest dimension of the wood chip. For thin wood strips, the width and thickness may be close to each other, thereby forming a match-like elongated object. The exact dimensions of the wood chips may vary.

[0060] In one embodiment, the cellulosic raw material used as the fiber source of the lignocellulosic raw material comprises or consists of wood chips, and grinding and compression are applied to the largest area of ​​the surface of the wood chips. Preferably, grinding and compression are performed to obtain 250-2000 kg / m 3 Between, preferably 350-1525kg / m 3density between to release HMW xylan and / or HMW lignin. Grinding and compression of the maximum surface area can be achieved by using gaps that allow the wood chips to enter their smallest size, or "one side" first. Equipment used for this purpose can be equipment between segmented plates, feeding screws with blades that reduce the distance, plug-type feeding screws that feed by rotating segmented plates, rotors and stators with segmented plates, improved pumps in which the stator and rotor of the pump have segmented plates to achieve a pressing and feeding action, roller presses with gaps and segmented surfaces, improved stator and rotor systems. Solutions are not limited to those mentioned above and can be applied by a person skilled in the art.

[0061] In a preferred embodiment, the wood chip is forced into the gap so that its flat side with the largest surface area does not enter the gap first. This can be achieved by guiding the wood chip to a gap where the wood chip does not fit into the flat side in front of it.

[0062] In one embodiment, grinding and compression are performed by passing the material through a gap under cooking conditions to release the HMW lignin into the spent liquor to provide a HMW lignin fraction in the black liquor.

[0063] In one embodiment, the conditions of a previous step, such as an optional pre-hydrolysis step or a cooking step, are maintained while the material is passed through a gap in the next step, for example to release xylan or lignin.

[0064] In one embodiment, grinding and compression is performed to a consistency of more than 10%, preferably more than 20% or more preferably more than 30%, preferably more than 65%.The consistency may be measured using the standard TAPPI T 240 consistency (concentration) of pulp suspensions or the corresponding ISO 4119 standard.

[0065] In one embodiment, the process comprises steps c) and d), and the grinding and compression in step d) are carried out at the prehydrolysis temperature used in step c) and to a consistency of at least 10% by weight.

[0066] In one embodiment, the wood chips are ground and compressed by passing them through a gap in the range of 50 mm to 8 mm, so that the wood porosity in the gap is reduced by at least 20%, 30%, 40%, 50%, 60%, 70% or more, and HMW lignin is released. Accordingly, when the method includes an optional prehydrolysis step and an optional grinding and compression step directly after the prehydrolysis step, HMW xylan can be released.

[0067] In one embodiment, grinding and compression are performed by passing the thin wood strips through a gap in the range of 35 mm to 6 mm, so that the wood porosity in the gap is reduced by at least 20%, 30%, 40%, 50%, 60%, 70% or more, and HMW lignin is released. Accordingly, when the method includes an optional prehydrolysis step and an optional grinding and compression step directly after the prehydrolysis step, HMW xylan can be released.

[0068] In one embodiment, the sawdust is ground and compressed by passing the sawdust through a gap in the range of 20 mm to 4 mm, so that the wood porosity in the gap is reduced by at least 20%, 30%, 40%, 50%, 60%, 70% or more, and HMW lignin is released. Accordingly, when the method includes an optional prehydrolysis step and an optional grinding and compression step directly after the prehydrolysis step, HMW xylan can be released.

[0069] In one embodiment, the grinding and compression is performed by pressing the pre-hydrolyzed material and / or the cooked cellulosic material through a gap, and the size of the gap is selected such that:

[0070] For wood chips, the gap is selected from the range of 50mm-8mm,

[0071] For thin wood strips, the gap is selected from the range of 35mm-6mm, and

[0072] For sawdust, the gap is selected from the range of 20 mm to 4 mm.

[0073] The porosity of wood materials is the amount of wood (kg / m 3 ) / 1500kg / m 3 calculate.

[0074] The term black liquor in the present invention means: used cooking liquor, ie spent liquor or waste cooking liquor.

[0075] In one embodiment, the black liquor or spent liquor is replaced with a displacement liquor containing 1% to 40% effective alkali as NaOH or NaOH cooking liquor, or an organic acid selected from lactic acid, acetic acid, formic acid, citric acid, oxalic acid, uric acid and malic acid. Thus, the displacement liquor replaces or changes the black liquor (spent cooking liquor) and after the displacement step, the material containing the cooked and compressed cellulose (cellulose fraction from which HMW xylan and HMW lignin have been removed in the previous step) remains in the displacement liquor.

[0076] In one embodiment, HMW lignin is recovered from the HMW lignin fraction in the spent liquor and the displacement liquor. Recovery can be accomplished, for example, by evaporating water from the black liquor and recovering the lignin.

[0077] When the HMW xylan is pressed out of the cell walls, a liquid having a HMW xylan fraction and a solid fraction comprising compressed material is formed.

[0078] In one embodiment, grinding and compression in step d) are started before the wood chips reach a porosity level of 0.66-0.9, preferably 0.67-0.9, more preferably 0.7-0.85. The porosity level can be calculated as 1-(dry material mass / cellulose density (1500 kg / m 3 ).

[0079] In one embodiment, the method comprises steps c) and d), and the compression in step d) is carried out to a pressure selected from 350 kg / m 3 and 2000kg / m 3 Between, preferably 350kg / m 3 and 1525kg / m 3 The density of the range between.

[0080] In one embodiment, the cooking process comprises a pre-hydrolysis step c) and a grinding and compression step d).

[0081] In one embodiment, the neutralization in step e) is performed using white liquor having a sulphurization degree between 1% and 45% or sodium hydroxide or an organic acid selected from lactic acid, acetic acid, formic acid, citric acid, oxalic acid, uric acid and malic acid.

[0082] In one embodiment, steps d) and g) are performed to increase the porosity of the fiber cell wall.

[0083] Total alkali, active alkali and effective alkali refer to the measurement of soda, white liquor and green liquor by standard method SCAN-N 30:85 or corresponding TAPPI or ISO standards.

[0084] In one embodiment, the neutralization is performed using an alkaline liquid containing 1%-45% effective alkali as NaOH with 1%-45% sulfide, NaOH liquid (determined by method SCAN-N 30:85 or corresponding TAPPI or ISO standards) or with an organic acid selected from lactic acid, acetic acid, formic acid, citric acid, oxalic acid, uric acid and malic acid. When an organic acid is used, the chemical charge can be selected from an organic acid in the range of 1-100 g / kg. The chemical charge is calculated as the mass of the selected chemical from the initial dry wood mass (kg). The relationship between the cooking liquor and the biomass and can be selected from 2-10 as mass (kg).

[0085] In one embodiment, the neutralization is performed using sodium hydroxide having a degree of sulfidation.

[0086] In one embodiment, NaOH liquid is used for neutralization.

[0087] In one embodiment, the neutralization liquor contains 1% to 45% effective alkali as NaOH, NaOH cooking liquor, or an organic acid selected from lactic acid, acetic acid, formic acid, citric acid, oxalic acid, uric acid, and malic acid having a sulfidation degree of 1% to 45% to provide a cooked cellulosic material in the spent liquor. The chemical charge is calculated as the mass of the selected chemical from the initial dry wood mass (kg).

[0088] The mass ratio of the neutralizing liquid to the lignocellulosic material is selected from the range of 2-10 based on the dry mass of the lignocellulosic material.

[0089] In one embodiment, the hydrolysate with HMW xylan is recovered and then neutralized. Under these conditions, the present invention is able to press xylan out of the cell wall and keep the xylan undegraded because most of the xylan is removed before entering the high alkaline concentration in the neutralization step.

[0090] In one embodiment, the neutralization is carried out at a temperature of at least 120°C, preferably above 150°C, or more preferably above 170°C.

[0091] Weight % refers to dry weight, such as wood dry weight for lignocellulosic feedstock.

[0092] The HMW xylan of the present invention can be collected directly after pre-hydrolysis because the xylan will not contact the alkali used in the cooking stage. Therefore, the xylan yield and molecular weight are maximized. The hydrolyzate can also be replaced with a neutralizing solution. However, part of the xylan is degraded by the alkali of the neutralizing solution, and the xylan yield is low. In the prior art PCT / FI2011 / 050651, pressing and shearing are only started after the cooking stage after lignin, hemicellulose and cellulose reach their softness points, thereby producing chemically and physically different products.

[0093] According to one embodiment, in the neutralization step, a base charge of 10%, 15%, 20%, 25%, 30%, 35% or 70% w / w of the effective base as NaOH or pure NaOH is used for neutralization. Preferably, a base charge of about 20% w / w is used. In one embodiment, the neutralization step is carried out by contacting the cellulosic material with the neutralizing liquid by pressing the liquid into the compressed material with a pump.

[0094] The term cooking liquor means white liquor, black liquor, white and black liquor, soda or mixtures thereof commonly used in chemical pulping during the cooking stage. White liquor comprises sodium hydroxide and sodium sulfide in water and is a strongly alkaline solution with a white opaque color. White liquor may contain small amounts of sodium carbonate, sodium sulfate, sodium thiosulfate, sodium chloride, calcium carbonate and other accumulated salts. Soda comprises sodium hydroxide and trace compounds contained in wood.

[0095] In one embodiment, cooking is carried out in an alkaline cooking liquor containing 1%-45% effective alkali as NaOH having a sulfidation of 1%-45%, with NaOH or with an organic acid selected from lactic acid, acetic acid, formic acid, citric acid, oxalic acid, uric acid and malic acid to provide a cooked cellulosic material in the spent liquor.

[0096] The mass ratio of cooking liquor to lignocellulosic material is selected from the range of 2-10 based on the dry mass of the raw materials.

[0097] According to one embodiment, cooking is performed in a cooking liquor at a temperature of at least 120°C, preferably above 150°C, more preferably above 170°C.

[0098] In the cooking process, at least 5 wt% of dry wood raw material is used, such as 5-10 wt%, and preferably more than 10 wt%.

[0099] During the cooking process, more than 10 wt% of cooking liquor based on the total weight is used.

[0100] The cooking cellulosic material in the cooking liquor may have an alpha-cellulose content of more than 60 w%, preferably more than 70 w%, and even more preferably more than 80 w%.

[0101] According to one embodiment, cooking is continued until the final kappa number is reached, followed by compression and / or grinding through the gap, wood chips between 50 mm and 8 mm or wood strands between 35 mm and 6 mm or sawdust 20 mm 4 mm.

[0102] In the cooking step, the kappa number may be selected between 120 and 1. More specifically, for dissolving pulp, the desired kappa number may be selected between 1-15, and for paper grade pulp, the kappa number may be between 15-50. The cooking temperature is selected from the range between 120° C. and 180° C. Those skilled in the art may select the temperature according to the kappa number target.

[0103] In one embodiment, when making a pulp for dissolving pulp, cooking is continued until a Kappa number selected between 100 and 1 is reached.

[0104] In one embodiment, when making paper grade pulp, cooking is continued until a Kappa number selected between 50 and 15 is reached.

[0105] In one embodiment, the method comprises steps c) and d), and the grinding and compressing in step d) is performed to a consistency of at least 60% by weight.

[0106] In one embodiment, the cooking in step f) is continued at a cooking temperature selected in the range between 120 and 180° C. to a kappa number selected in the range between 100 and 3.

[0107] According to one embodiment, in step g), the grinding and compression of the wood chips in step g) is carried out as described above, by forcing the wood chips through the gap under the conditions of the cooking step and releasing the HMW lignin into the cooking liquor, thereby forming a liquid HMW lignin fraction and a solid fraction comprising compressed material.

[0108] In one embodiment, the grinding and compression in step g) may be started before the wood chips reach a porosity level of 0.65-0.9, preferably 0.66-0.9, more preferably 0.7-0.85.

[0109] The compressed cellulose fraction has an alpha cellulose content exceeding 85%, more preferably exceeding 90%, and more preferably exceeding 95%.

[0110] In one embodiment, the cooked cellulosic material is compressed in black liquor with a pressure selected from the range between 1 and 250 kPa to form a column having a consistency of at least 5% solids by weight. Non-limiting examples of suitable pressures to achieve the selected target consistency value are 1 kPa, 2 kPa, 3 kPa, 4 kPa, 5 kPa, 6 kPa, 7 kPa, 8 kPa, 9 kPa, 10 kPa, 20 kPa, 30 kPa, 40 kPa, 50 kPa, 60 kPa, 70 kPa, 80 kPa, 90 kPa, 100 kPa, 110 kPa, 120 kPa, 130 kPa, 140 kPa, 150 kPa, 160 kPa, 170 kPa, 180 kPa, 190 kPa, 200 kPa, 210 kPa, 220 kPa, 230 kPa, 240 kPa and 250 kPa. Non-limiting examples of suitable consistency values ​​are 5%, 6%, 7%, 8%, 9%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 5%-50%, 5%-40%, 5%-30%, and 5%-20% by weight.

[0111] In step h), the black liquor is preferably replaced with a replacement liquor having a lower lignin content than the black liquor. At the end of step g), the compressed column of material may be replaced by diluting to a consistency selected from the range between 2% and 35% by weight, such as 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 15%, 20%, 25%, 30%, 35%, 2%-30%, 2%-25%, 2%-20%, 2%-10% or 2%-5% by weight.

[0112] In one embodiment, in step i), a HMW lignin fraction is recovered from the black liquor and from the displacement liquor.

[0113] In one embodiment, in step j), a cellulose fraction or a dissolving pulp is recovered.

[0114] In one embodiment, step g) is carried out at the cooking temperature used in step f) and to a consistency of at least 10% by weight.

[0115] In one embodiment, the method comprises steps c) and d), and in step d), the compression pressure is selected from the range between 35 kPa and 1000 kPa.

[0116] In one embodiment, step g) comprises pressing with a pressure selected from the range between 1 kPa and 250 kPa to form a column having a consistency of at least 5% by weight, and wherein said displacement step h) is performed by displacing said black liquor with a second displacement liquid having a lignin content lower than the lignin content in said black liquor.

[0117] In one embodiment, the replacement fluid has as effective base an alkali charge selected in the range between 1% and 40% by dry weight of the cellulosic material, or sodium hydroxide or an organic acid selected from lactic acid, acetic acid, formic acid, citric acid, oxalic acid, uric acid and malic acid.

[0118] In one embodiment, the displacement step h) is performed at a temperature selected from the range between 70°C and 200°C.

[0119] In one embodiment, after step j), the dissolving pulp is dewatered to remove 90% or more of the alkali, lignin and dissolved xylan and other organic and inorganic materials from the pulp as a liquid stream and to provide a dewatered pulp.

[0120] In one embodiment, the method comprises delignifying a dewatered pulp by oxygen to provide a delignified pulp, optionally followed by washing and pressing.

[0121] In this embodiment, at least a HMW lignin fraction and at least a HMW xylan fraction are recovered from the spent liquor and from the second displacement liquor. Optionally, a lignin fraction and / or a xylan fraction containing smaller molecular weight species is also recovered.

[0122] The method improves the xylan yield, the lignin yield and the cellulose yield, reduces the wood consumption and the cooking time, and increases the amount of liquid in the recovered lignin and xylan. Example

[0123] The effects obtainable by embodiments of the method of the present invention are demonstrated by the following experiments, which should not be considered as limiting the scope of the present invention. The abbreviation REF refers to the method of the prior art, i.e. the cooking method according to the present invention without a compression step. A person skilled in the art can select the cooking conditions to obtain the target kappa number at the end of the cooking stage.

[0124] Example 1

[0125] In this example, when performing the method according to the present invention involving a pre-hydrolysis step and a grinding and compression step, an increase in the molecular weight of xylan was observed. Eucalyptus wood chips and pine wood chips were treated according to the present method and according to the reference method (REF), i.e., the method presented in EP0442806A1. The wood chips were pre-treated to remove air from the wood chips by steam at 115°C for 5 minutes. Pre-hydrolysis was carried out with water at 175°C for 25 minutes. Afterwards, the wood chips were fed through a narrow gap, rotor grinding and compression against the pressure vessel wall, followed by compression of the hydrolyzate from the raw material source so that the material consistency exceeded 65%. HMW xylan was recovered from the hydrolyzate. The pre-hydrolyzed raw material was then neutralized with an alkali having an effective alkali charge in soda cooking as NaOH 6 mol / kg and a sulfidation degree of 28% in the pre-hydrolyzed kraft cooking. The temperature was 150°C. The neutralization time was 17 minutes, after which the neutralizing liquid was replaced with the cooking liquor by using a cooking liquor to wood ratio of 4. In the prehydrolysis kraft cooking, the effective alkali charge was NaOH 2.5 mol / kg and the degree of sulfidation was 28%. The cooking temperature was 156°C and after cooking at an H factor of 25, the wood chips were fed through a narrow gap where the rotors ground and compressed against the pressure vessel wall, resulting in grinding and compression and replacement of the HWM lignin-containing waste liquor with wash filtrate. Table 1 presents the cooking results for prehydrolysis soda and prehydrolysis kraft cooking.

[0126] Table 1.

[0127]

[0128] According to Table 1, when cooking is performed according to the present invention, the molecular weights of xylan and lignin Mw increase, and the cooking time decreases.

[0129] Example 2

[0130] In this example, the xylan yield and consistency obtained by using the present invention are demonstrated and compared with the previous cooking method. In the sample, after pre-hydrolysis at a pressure of 15 MPa, the wood chips were ground and compressed through a gap between 50 mm and 8 mm, and the hydrolyzate was collected for xylan analysis. In the prior art marked as REF, grinding and compression were not used.

[0131] Table 2.

[0132] sample Xylan yield, % from wood REF Pre-hydrolyzed Kraft Eucalyptus 12% REF Pre-hydrolyzed Kraft Pine 10% Pre-hydrolyzed soda eucalyptus 45% Pre-hydrolyzed soda pine 35% Pre-hydrolyzed Kraft Eucalyptus 51% Prehydrolyzed Kraft Pine 38%

[0133] According to Table 2, when cooking was performed according to the present invention, the xylan yield (%) increased.

[0134] As the results demonstrate, the present method increases the yield and reduces the cooking time from raw materials and different kappa numbers.

[0135] The above description provides a complete and informative description of the best mode currently contemplated by the inventor for carrying out the present invention by way of non-limiting examples of specific embodiments and embodiments of the present invention. However, it will be clear to those skilled in the art that the present invention is not limited to the details of the embodiments set forth above, but may be implemented in other embodiments using different combinations of equivalents or embodiments without departing from the features of the present invention.

[0136] In addition, some features of the above disclosed embodiments of the present invention can be advantageously used without corresponding use of other features. Therefore, the above description should be regarded as merely illustrating the principles of the present invention and is not limited thereto. Therefore, the scope of the present invention is only limited by the attached patent claims.

Claims

1. A cooking method comprising: a) providing a lignocellulosic raw material, which includes wood chips, wood strands, wood shavings, sawdust or a combination thereof; b) pretreating the lignocellulosic feedstock by subjecting it to a steam treatment to provide a pretreated material; c) prehydrolyzing the pretreated material with steam or water to provide a prehydrolyzed material; d) grinding and compressing the pre-hydrolyzed material to release HMW xylan from the pre-hydrolyzed material into a hydrolysate, and recovering the hydrolysate having HMW xyloglucan; e) neutralization with sodium hydroxide containing sulfur or with sodium hydroxide, or replacement with an organic acid selected from lactic acid, acetic acid, formic acid, citric acid, oxalic acid, uric acid and malic acid; f) cooking in a cooking liquor comprising sodium hydroxide or sodium hydroxide with sulfur, or an organic acid selected from the group consisting of lactic acid, acetic acid, formic acid, citric acid, oxalic acid, uric acid and malic acid to provide a cooked cellulosic material in a spent liquor; g) grinding and compressing the cooked cellulosic material to release HMW lignin from the cooked material into the spent liquor, thereby providing a HMW lignin fraction in black liquor and a compressed cellulose fraction. h) displacing the black liquor with a displacement liquor containing 1% to 40% of effective alkali as NaOH or acidic sulfite cooking liquor, or with an organic acid selected from the group consisting of lactic acid, acetic acid, formic acid, citric acid, oxalic acid, uric acid and malic acid; i) recovering said HMW lignin from the HMW lignin fraction in said black liquor and from said displacement liquor; and recovering a dissolving pulp from the compressed cellulose fraction; and j) wherein the grinding and compressing is carried out at the prehydrolysis temperature used in step c) and to a consistency of at least 10% by weight.

2. The process of claim 1, wherein the grinding and compressing in step d) is carried out to a consistency of at least 60% by weight.

3. The method of claim 1, wherein the compression in step d) is carried out to a pressure selected from 350 kg / m 3 and 2000kg / m 3 The density of the range between.

4. The method of claim 1, wherein the compression in step d) is carried out to a pressure selected from 350 kg / m 3 and 1525kg / m 3 The density of the range between.

5. The method according to any one of claims 1 to 4, wherein in said step d), said compression pressure is selected from the range between 35 kPa and 1000 kPa.

6. The method of claim 1, wherein the cooking in step f) is continued at a cooking temperature selected from the range between 120 and 180°C to a Kappa number selected from the range between 100 and 3.

7. The method of claim 1, wherein the grinding and compressing is performed by pressing the pre-hydrolyzed material and / or the cooked cellulosic material through a gap, and the size of the gap is selected such that: For wood chips, the gap is selected from the range of 50mm-8mm, For thin wood strips, the gap is selected from the range of 35mm-6mm, and For sawdust, the gap is selected from the range of 20 mm to 4 mm.

8. The process of claim 1 wherein step g) is conducted at the cooking temperature used in step f) to a consistency of at least 10% by weight.

9. The process as claimed in claim 1, wherein the neutralization in step e) is carried out using white liquor having a sulfidation degree between 1% and 45% or sodium hydroxide or an organic acid selected from lactic acid, acetic acid, formic acid, citric acid, oxalic acid, uric acid and malic acid.

10. The method of claim 1, wherein step d) and step g) are performed to increase the porosity of the fiber cell wall.

11. The method of claim 1 , wherein said step g) comprises pressing with a pressure selected from the range between 1 kPa and 250 kPa to form a column having a consistency of at least 5% by weight, and wherein said displacement step h) is performed by displacing said black liquor with a second displacement liquid having a lignin content lower than the lignin content in said black liquor.

12. The method of claim 1, wherein the replacement fluid has as effective alkali an alkali charge selected from the range between 1% and 40% based on the dry weight of the cellulosic material, or sodium hydroxide or an organic acid selected from lactic acid, acetic acid, formic acid, citric acid, oxalic acid, uric acid and malic acid.

13. The method of claim 1, wherein the replacing step h) is performed at a temperature selected from the range between 70°C and 200°C.

14. The method of claim 1, wherein after step j), the dissolving pulp is dewatered to remove 90% or more of the alkali, lignin and dissolved xylan and other organic and inorganic materials from the pulp as a liquid stream and provide a dewatered pulp.

15. A method as claimed in claim 14 comprising delignifying the dewatered pulp by oxygen to provide a delignified pulp followed by washing and pressing.

16. A high molecular weight xylan fraction obtainable by using the method of any one of claims 1 to 15 and having an average molecular weight (MW) of 45 000 g / mol or more.

17. A high molecular weight lignin fraction obtainable from hardwood by using the method of any one of claims 1 to 15 and having an average molecular weight (MW) of 4580 g / mol or more.

18. A high molecular weight lignin fraction obtainable from softwood by using the method of any one of claims 1 to 15 and having an average molecular weight (MW) of 4980 g / mol or more.

19. A pulp product obtainable by using the method of any one of claims 1-15.

Citation Information

Patent Citations

  • A process for producing pulp from a lignocellulosic-containing material

    EP0442806A1

  • Process For Producing A Pulp

    US20090312536A1

  • Lyocell fibers, and compositions for making the same

    WO1999047733A1

  • Method and system for pulp processing using cold caustic extraction with alkaline filtrate reuse

    WO2011138633A1

  • Method and system for high alpha dissolving pulp production

    WO2011138634A1