High-stability rare earth nanofluorine clusters for LED lighting and methods and applications thereof
Synthesis of high-stability rare earth nanofluorine clusters by solvent thermal method solves the problems of single structure and poor stability of rare earth nanomaterials, achieves high fluorescence intensity and quantum yield, is suitable for white LED devices, and improves luminescence efficiency and safety.
Patent Information
- Application Number
- CN202310182803.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-28
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-02-28
AI Technical Summary
The existing rare earth nanofluorescent materials have single structure, poor stability, low fluorescence intensity and low quantum yield, which limits their application in white LED devices, and the preparation process is complex and has safety and environmental problems.
The high-stability rare earth nanofluoro clusters of RE16(μ4-F)6(μ3-F)12[(CH3)3CCOO]18([N(CH2CH2O)3])4 were synthesized by solvothermal method, and the rare earth oxides were used to Trimethylacetic acid and alcoholamine ligand react at high temperature and combine with solvothermal reaction of fluorine source to obtain rare earth nanofluorine clusters with high fluorescence intensity and quantum yield.
The high stability, long fluorescence lifetime and high quantum yield of rare earth nanofluorine clusters are achieved, which significantly improves the luminescence efficiency and safety of white LED devices, and the synthesis process is simple and environmentally friendly.
Smart Images

Figure CN116143809B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of material science and technology, and relates to a fluorescent nano functional material, in particular to a high-stability rare earth nano fluorine cluster for LED lighting, and a method and application thereof. Background Art
[0002] Light-emitting diodes (LEDs) have gradually transformed into an important role in the world's solid-state lighting equipment due to their high efficiency, energy saving, good light stability, long life and environmental protection. They are widely used in home lighting, automotive lighting, display lighting, backlight sources, display screens, biomedicine and plant growth. This type of spontaneous radiating semiconductor device with a PN junction transition layer that can convert electrical energy into light energy has a variety of ways to achieve full-spectrum ultra-white light. The most common and mature ones are the combination of RGB three-color light chips and blue light chips coated with yellow phosphors. The former has complex processes and high costs, while the latter, i.e., blue light technology, shows shortcomings such as spectral discontinuity, poor color rendering and low luminous efficiency. In recent years, researchers have shifted the path to achieving white light LEDs to near-ultraviolet light chips combined with RGB three-color phosphors, and obtained ultra-white light LEDs with high luminous efficiency, good white light quality and low cost. Therefore, exploring new RGB phosphors that can be effectively excited by a UV chip of one wavelength to produce an efficient emission spectrum in the visible light region, thereby realizing white light LEDs in different color temperature regions has become a basic core technology that needs to be overcome at present, and is also one of the keys to developing energy-saving and efficient lighting devices.
[0003] Among the rare earth fluorescent materials used in white light LED devices, inorganic rare earth salts and rare earth-doped inorganic rare earth nano-phosphors have greatly limited the application range of such materials due to their single structure, weak fluorescence intensity and inherent concentration quenching. Rare earth nano-phosphors are composed of rare earth ion activators and matrix materials. The doping amount of the rare earth activator is generally only 10%, which directly leads to weak luminescence brightness and low quantum yield (<25%). Therefore, in order to expand and enrich rare earth fluorescent nano-materials and solve the problems of low fluorescence intensity and concentration quenching, rare earth fluorine-bridged cluster nano-fluorescent materials provide a new choice. This material has the characteristics of unique organic-inorganic assembly structure, high fluorescence intensity and high quantum yield; the chelation of ligands and metal centers can achieve structural diversification and multiple modes of fluorescence emission: ligand-to-ligand transitions, metal-to-ligand transitions, and metal-to-metal transitions. For example, rare earth metal europium ions and terbium ions are important luminescence centers with commonly used red or green monochromatic light. In addition, the fluorine bridge (replacing the high-frequency vibration group "-OH") in the molecular structure of this type of material has also been proven to be the key to improving luminescence intensity, quantum yield and avoiding fluorescence concentration quenching.
[0004] At present, there are only three kinds of high-stability rare earth nanofluorine clusters. The reason is that fluoride ions and rare earth ions react easily to form insoluble rare earth fluoride precipitates REF x In addition, due to the harsh preparation conditions, the selection of large steric ligands, and the presence of highly toxic reactants such as mercury and hydrofluoric acid, the fluorine-bridged cluster materials prepared by this method have the following structural disadvantages: low rare earth nuclei, single structure, and instability in air and solution. The great lack of structure and variety has seriously hindered the exploration of the "guided synthesis" law, luminescence law, and "structure-activity relationship" of this type of material, and restricted in-depth research on the application of white light LED devices. Summary of the invention
[0005] The purpose of the present invention is to provide a high-stability rare earth nanofluorine cluster for LED lighting and a method and application thereof to overcome the shortcomings of the prior art. The material of the present invention has good optical properties, thermal stability and solution stability, and exhibits excellent color purity, high quantum yield and long fluorescence lifetime under a suitable excitation wavelength.
[0006] A high-stability rare earth nanofluorine cluster for LED lighting, with the molecular formula RE 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, where RE is a rare earth ion, μ4-F and μ3-F are bridging methods of fluoride ions, [N(CH2CH2O)3] 3- is a deprotonated triethanolamine ligand, [(CH3)3CCOO] - It is the trimethylacetate ion.
[0007] Preferably, RE is one or more of Y, La, Ce, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb or Lu.
[0008] Preferably, Eu 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4 and Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The emission peaks of ([N(CH2CH2O)3])4 are all in the visible light region, the excitation wavelength range is 350 to 450 nanometers, and the emission peak range is 550 to 750 nanometers.
[0009] A method for preparing a high-stability rare earth nano-fluorine cluster for LED lighting comprises the following steps:
[0010] S1, reflux reaction of rare earth oxide and trimethylacetic acid solution at a temperature of 140 to 160 degrees Celsius to obtain a rare earth precursor, and dissolving and dispersing the rare earth precursor and an alcohol amine ligand in an organic solvent to obtain a solution A;
[0011] S2, dispersing the fluorine source in a solvent to obtain solution B, subjecting solution A and solution B to a solvothermal reaction, and obtaining colorless block-like high-stability rare earth nanofluorine clusters through programmed cooling.
[0012] Preferably, the organic solvent is one or a mixture of methanol, ethanol, acetonitrile or N,N-dimethylformamide; the fluorine source is triethylamine trihydrofluoride, ammonium fluoride, sodium fluoride or tetramethylammonium fluoride tetrahydrate.
[0013] Preferably, the solvent thermal reaction temperature is 100 to 160 degrees Celsius, the reaction time is 24 to 72 hours, and the programmed cooling rate is 3 to 5 degrees Celsius per hour.
[0014] Preferably, the rare earth precursor is trimethylacetic acid rare earth salt, and the alcoholamine ligand is triethanolamine.
[0015] Preferably, the molar ratio of the rare earth precursor to the fluorine source is 1:(2-3).
[0016] Preferably, the solvent in step S2 is anhydrous ethanol.
[0017] An application of the above-mentioned high-stability rare earth nano-fluorine cluster for LED lighting in an LED lighting device. The LED lighting device includes a near-ultraviolet LED chip and an RGB three-color phosphor mixed with ultraviolet curing glue; the green and red phosphors in the RGB three-color phosphor use the above-mentioned high-stability rare earth nano-fluorine cluster for LED lighting; the near-ultraviolet light chip is an InGaN semiconductor chip with an electroluminescent wavelength of 370 nanometers, and the blue phosphor is a commercial BAM phosphor. The mass ratio of red: green: blue fluorescent materials in the RGB three-color phosphor is 10:10:1-3.
[0018] Compared with the prior art, the present invention has the following beneficial technical effects:
[0019] The present invention discloses a high-stability rare earth nano-fluorine cluster for LED lighting, which has 16 rare earth centers and is coordinated with two ligands (trimethylacetic acid and triethanolamine). The size of a single molecule is measured to be approximately 2 nanometers × 2 nanometers. The molecular size is in the nanometer range and the coordination mode is unattainable by existing materials. Compared with rare earth cluster materials synthesized by a solvent thermal method, the high-stability rare earth nano-fluorine cluster proposed by the present invention exhibits the characteristics of simple synthesis process, safety and environmental protection, and a large amount of crystalline products obtained by reaction in a suitable ratio ensures the high purity and high yield (81%) of the material.
[0020] Compared with the existing rare earth fluorescent materials, the high-stability rare earth nano-fluorine cluster molecular structure proposed by the present invention not only has fluorine ions that play a bridging role, but also has an outer layer of organic ligands that effectively chelate the inner layer of metal, so that the concentration quenching phenomenon of rare earth luminescent materials is eliminated. Compared with the existing hydroxyl-bridged rare earth cluster structure, the coordination of fluorine ions avoids the fluorescence quenching caused by high-frequency vibration groups (such as hydroxyl groups), so that the fluorescence quantum yield is significantly improved, all above 83%.
[0021] The high-stability rare earth nanofluorine cluster proposed in the present invention exhibits a unique negative temperature quenching effect. Compared with the prior art, it perfectly matches the operating temperature of the LED lighting device proposed in the present invention of 140 degrees Celsius, greatly improving the luminous life and safety of the white light LED device.
[0022] The power of the LED lighting device prepared by the present invention is 3W, and its brightness is 6047cd / m at a normal working voltage of 3.5V. 2 , brightness is 63140cd / m at 4.2V 2 , reaching the brightness standard required for outdoor lighting at night. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is Tb in Example 1 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 Molecular structure diagram of ([N(CH2CH2O)3])4;
[0024] Figure 2 is Eu in Example 4 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4 excitation emission spectrum, the left side is the excitation spectrum, the emission wavelength is 614 nanometers, the right side is the emission spectrum, the excitation wavelength is 394 nanometers;
[0025] Figure 3is Tb in Example 2 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4 excitation emission spectrum, the left side is the excitation spectrum, the emission wavelength is 545 nanometers, the right side is the emission spectrum, the excitation wavelength is 372 nanometers;
[0026] Figure 4 is the RE in Examples 2 and 4 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 Decay time curves of ([N(CH2CH2O)3])4 (RE=Eu or Tb) samples in solid and liquid states.
[0027] Figure 5 is the RE in Examples 2 and 4 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 Color coordinate diagram of ([N(CH2CH2O)3])4 (RE = Eu or Tb), the inset is a photo of the sample under UV light;
[0028] Figure 6 is Tb in Example 1 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 Mass spectrum of ([N(CH2CH2O)3])4.
[0029] Figure 7 is Tb in Example 1 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 Transmission electron microscopy image of ([N(CH2CH2O)3])4.
[0030] Figure 8 is Eu in Example 4 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 Transmission electron microscopy image of ([N(CH2CH2O)3])4.
[0031] Fig. 9 is the RE in Examples 1, 4, 6 and 9 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18Thermogravimetric curves of ([N(CH2CH2O)3])4 (RE = Y, Dy, Eu and Tb).
[0032] Fig.10 is Eu in Example 2 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 Temperature quenching diagram of ([N(CH2CH2O)3])4 between 300 and 500 K, with the inset being the temperature-dependent luminescence intensity curve.
[0033] Fig.11 is Tb in Example 1 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 Temperature-dependent luminescence intensity curve of ([N(CH2CH2O)3])4 between 300 and 500 °C.
[0034] Fig.12 is the RE in Examples 2 and 4 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 Electroluminescence spectrum of an LED lighting device in which ([N(CH2CH2O)3])4 (RE=Eu or Tb) is mixed with commercial BAM blue phosphor in UV-curing adhesive and packaged on a near-UV chip. The inset is a working state diagram of the device and a color coordinate diagram in the white light region. DETAILED DESCRIPTION
[0035] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0036] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0037] The present invention provides a high-stability rare earth nano-fluorine cluster for LED lighting, whose molecular formula is RE 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, where RE is a rare earth ion, μ4-F and μ3-F are two bridging modes of fluoride ions, [N(CH2CH2O)3] is triethanolamine, [(CH3)3CCOO] is trimethylacetic acid, [(CH3)3CCOO] - is the trimethylacetate ion, [N(CH2CH2O)3] 3- It is a completely deprotonated triethanolamine ion.
[0038] In the zero-dimensional rare earth fluorescent nanocluster material containing fluorine bridges, RE is one or more of Y, La, Ce, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb or Lu. 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4 and Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4 can be excited by near-ultraviolet light and blue light between 350 and 450 nanometers, and the emission peak range of both is in the visible light region between 550 and 750 nanometers. Two or three rare earth-doped isomorphous heterogeneous materials can also be obtained through preparation, such as: Tb8Gd8(μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4.
[0039] A method for preparing high-stability rare earth nanofluorine clusters for LED lighting:
[0040] S1, reflux the rare earth oxide and trimethylacetic acid solution at a temperature of 140 to 160 degrees Celsius for 3 to 8 hours, stop when the solution changes from turbid to clear, cool naturally, add a large amount of acetonitrile for washing and stirring when the temperature drops to 60 to 80 degrees Celsius, filter and dry after cooling to room temperature to obtain a rare earth precursor RE2(piv)6(Hpiv)6, dissolve and disperse the obtained rare earth precursor and alcohol amine ligand in an organic solvent to obtain a solution A;
[0041] The rare earth oxide is RE2O3 or rare earth carbonate Ln2(CO3)3, and the organic solvent is one or a mixture of acetonitrile, N,N-dimethylformamide or methanol.
[0042] S2, dispersing the fluorine source in a solvent to obtain solution B, mixing solution A and solution B, placing them in a polytetrafluoroethylene liner and transferring them to an autoclave for a solvothermal reaction, and obtaining transparent block-shaped high-stability rare earth nanofluorine clusters through programmed cooling.
[0043] Reaction equation: 8RE2(piv)6(Hpiv)6+18NH4F+4TEA+12Et3N+MeCN→RE 16 (μ4-F)6(μ3-F) 12 (piv) 18 [N(CH2CH2O)3]4.
[0044] The polytetrafluoroethylene lining (PTFE) is resistant to high pressure and high temperature, flame retardant, corrosion resistant, and the dense and smooth inner wall is conducive to crystal growth; the reaction solution does not exceed 2 or 3 of the volume of the autoclave container.
[0045] Precursor preparation: RE2O3+30Hpiv→RE2(piv)6(Hpiv)6+H2O, RE=Y, La, Nd, Sm, Eu, Gd, Dy, Ho, Er, Tm or Lu; Ln2(CO3)3+30Hpiv→Ln2(piv)6(Hpiv)6+H2O+CO2, Ln=Tb or Yb.
[0046] The organic solvent is one of methanol, ethanol, acetonitrile or N,N-dimethylformamide or a mixture of several thereof.
[0047] The solvent in step S2 is anhydrous ethanol; the solvent thermal reaction temperature is 100 to 160 degrees Celsius, the reaction time is 24 to 72 hours, and the programmed cooling rate is 3 to 5 degrees Celsius per hour.
[0048] The molar ratio of the rare earth precursor to the fluorine source is 1:(2-3).
[0049] The fluorine source is one of triethylamine trihydrofluoride, ammonium fluoride or tetramethylammonium fluoride tetrahydrate.
[0050] The rare earth precursor is trimethylacetic acid rare earth salt, and the alcoholamine ligand is triethanolamine.
[0051] The LED lighting device prepared according to the above-mentioned high-stability rare earth nano-fluorine cluster specifically includes a near-ultraviolet LED chip and an RGB three-color phosphor mixed with ultraviolet curing glue; wherein the green phosphor and the red phosphor in the RGB three-color phosphor adopt the above-mentioned high-stability rare earth nano-fluorine cluster Eu for LED lighting. 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4 and Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, the near-ultraviolet light chip is an InGaN semiconductor with an electroluminescent wavelength of 370 nanometers, and the blue phosphor is a commercial BAM phosphor.
[0052] The mass ratio of red: green: blue fluorescent materials in the RGB three-color fluorescent powder is 10:10:1-3.
[0053] The specific embodiments of the present invention are as follows:
[0054] Example 1
[0055] 50 mmol of terbium carbonate and 1.5 mol of trimethylacetic acid were added to a 500 ml round-bottom flask, and the reactants were heated to 150 degrees Celsius for 4 hours. The solution changed from white turbidity to clarity. After cooling to 70 degrees Celsius, 80 ml of acetonitrile was added to precipitate a large amount of rare earth precursor terbium trimethylacetate, and the yield was about 87%;
[0056] Weigh 0.75g (0.5mmol) of terbium trimethylacetate into a beaker, add 3ml of acetonitrile and 4ml of N,N-dimethylformamide to completely dissolve the rare earth precursor. Disperse 0.037g (1mmol) of amine fluoride in 2ml of ethanol, mix the two solutions and pour them into a 15ml polytetrafluoroethylene bottle, pressurize and react in a temperature-controlled oven at 150 degrees Celsius for 72 hours, and cool to room temperature for 36 hours to obtain pure colorless and transparent block crystals of Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18([N(CH2CH2O)3])4 was washed three times with acetonitrile, and the product yield was 81%. Its crystal structure was obtained by single crystal X-ray diffractometer.
[0057] See also Figure 1 , Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 Schematic diagram of the structure of the ([N(CH2CH2O)3])4 cluster (H atoms omitted in the figure), showing the arrangement of 16 terbium ions, with seven terbium ions sharing the same plane, and two adjacent planes sharing two terbium ions, with a total of 18 fluorine bridging ions and 4 completely deprotonated triethanolamine coordination. Figure 2 , showing that Eu 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The strongest emission peak of the ([N(CH2CH2O)3])4 sample under an excitation wavelength of 394 nm is located at 613 nm. Figure 3 Shows Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The strongest emission peak of ([N(CH2CH2O)3])4 at 372 nm is at 545 nm; see Figure 4 , under 394 nm and 372 nm UV light, RE 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The fluorescence lifetime of ([N(CH2CH2O)3])4(RE=Eu or Tb) sample; 1 is {Eu 16 F 18} solid, 2 is {Eu 16 F 18} tetrahydrofuran solution, 3 is {Tb 16 F 18} solid, 4 is {Tb 16 F 18 The fluorescence lifetimes of tetrahydrofuran solutions of} are 1.74ms, 1.14ms, 2.90ms and 2.41ms, respectively, all at the millimeter level. Figure 5 , CIE shows RE 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The ([N(CH2CH2O)3])4(RE=Eu or Tb) sample has good color purity. The sample in the illustration shows strong fluorescence under ultraviolet light. Figure 6 , Tb16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The mass spectrum of ([N(CH2CH2O)3])4 molecule is in negative ion mode, [M+F - ] has a peak value of 5308.69, which is consistent with the molecular weight in the single crystal structure, that is, it can stably exist in the organic solvent THF, and it proves that there are 18 fluoride ions in the molecular structure. Figure 7 It is shown that the Tb dispersed in anhydrous ethanol can be observed by transmission electron microscopy. 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The morphology and size of ([N(CH2CH2O)3])4 are between 100 and 300 nanometers, and they are regular diamond-shaped flakes and evenly distributed. Figure 8 The transmission electron microscope shows the sample Eu 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The morphology and size of ([N(CH2CH2O)3])4 dispersed in anhydrous ethanol are between 700 and 1000 nanometers, and are regular rhombus-shaped flakes with uniform distribution. Fig. 9 For sample RE 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The thermogravimetric curve of ([N(CH2CH2O)3])4 (RE is Y, Dy, Eu or Tb) shows excellent thermal stability in that the molecular structure does not collapse until 450 degrees Celsius in the absence of solvent molecule co-crystallization. Fig.10 Showing Eu 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The temperature quenching diagram of ([N(CH2CH2O)3])4 between 300 and 500K, and the inset is the temperature-dependent luminescence intensity curve. From the trend of the curve, it can be seen that when the temperature rises to 500K, the luminescence intensity of the material is still greater than 60% of that at room temperature, and the temperature quenching phenomenon is not obvious, which makes it suitable as a red phosphor for white light LED devices. Fig.11 Shows Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The temperature dependence of the luminescence intensity curve of ([N(CH2CH2O)3])4 between 300 and 500 K is similar to Fig.10The difference is that this material exhibits negative temperature quenching characteristics. The luminescence intensity increases with increasing temperature and gradually decreases starting from 420K, showing excellent luminescence properties. It is a key luminescent material for the preparation of white light LED devices. Fig.12 Shows RE 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The electroluminescence spectrum of the LED lighting device in which ([N(CH2CH2O)3])4 (RE=Eu or Tb) and commercial BAM blue phosphor are ground into fine powder respectively, mixed in two different proportions in UV curing adhesive and coated on a near-UV chip, shows that the spectrum is continuous and the luminous intensity is high in the wavelength range of 200 to 750 nanometers; the inset is the electroluminescence working state diagram of the corresponding device and the color coordinates of the two color temperature LED devices in the white light region.
[0058] Through testing and analysis of Eu 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4 and Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The fluorescence quantum yield of ([N(CH2CH2O)3])4 is 83.3% and 94.9% respectively under the best excitation state. The higher value shows a stronger quantum yield. The pure rare earth metal center in the molecular structure does not lead to concentration quenching, which improves and breaks through the shortcomings and difficulties of inorganic nano fluorescent materials in fluorescence properties. The spectrum of LED lighting devices was tested, and the spectrum from near ultraviolet to red light is continuous, showing characteristics such as high color rendering index and high brightness.
[0059] Example 2
[0060] Weigh 0.75g (0.5mmol) of terbium trimethylacetate into a beaker, add 3ml of acetonitrile and 4ml of N,N-dimethylformamide to completely dissolve the rare earth precursor. Disperse 0.037g (1mmol) of amine fluoride in 2ml of ethanol, mix the two solutions and pour them into a 15ml polytetrafluoroethylene bottle, react under pressure in a temperature-controlled oven at 120 degrees Celsius for 72 hours, and cool to room temperature for 36 hours to obtain pure colorless block crystals of Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, washed three times with acetonitrile, the product yield was 78%, and the crystal structure was determined by single crystal X-ray diffraction analysis, which was consistent with the previous Tb16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The crystal structure of ([N(CH2CH2O)3])4 is consistent.
[0061] Example 3 Weigh 1.5 g (1 mmol) of yttrium trimethylacetate in a beaker, add 3 ml of acetonitrile and 4 ml of N, N-dimethylformamide to completely dissolve the rare earth precursor. Take 0.074 g (2 mmol) of amine fluoride and disperse it in 2 ml of ethanol. Mix the two solutions and pour them into a 15 ml polytetrafluoroethylene bottle. Pressurize and react in a temperature-controlled oven at 150 degrees Celsius for 72 hours, and cool to room temperature for 40 hours to obtain pure colorless block crystals of Y 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, washed three times with acetonitrile, the product yield was 90%, and the crystal structure was determined by single crystal X-ray diffraction analysis, which was consistent with the previous Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The crystal structure of ([N(CH2CH2O)3])4 is consistent.
[0062] Example 4
[0063] Weigh 1.5g (1mmol) of trimethylacetate europium into a beaker, add 7ml of methanol to completely dissolve the rare earth precursor. Disperse 0.074g (2mmol) of fluorinated amine in 2ml of ethanol, mix the two solutions and pour them into a 15ml polytetrafluoroethylene bottle, react under pressure in a temperature-controlled oven at 150 degrees Celsius for 72 hours, and cool to room temperature for 36 hours to obtain regular rhombus flake crystals of Eu. 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, washed three times with acetonitrile, the product yield was 65%. The crystal structure was determined by single crystal X-ray diffraction analysis, which was consistent with the previous Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The crystal structure of ([N(CH2CH2O)3])4 is consistent.
[0064] Example 5
[0065] Weigh 1.5g (1mmol) of trimethylacetate europium into a beaker, add 3ml of acetonitrile and 4ml of N,N-dimethylformamide to completely dissolve the rare earth precursor. Disperse 0.074g (2mmol) of fluorinated amine in 2ml of ethanol, mix the two solutions and pour them into a 15ml polytetrafluoroethylene bottle, pressurize and react in a temperature-controlled oven at 150 degrees Celsius for 72 hours, and cool to room temperature for 36 hours to obtain pure colorless block crystals of Eu. 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, washed three times with acetonitrile, the product yield was 83%, and the crystal structure was determined by single crystal X-ray diffraction analysis, which was consistent with the previous Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The crystal structure of ([N(CH2CH2O)3])4 is consistent.
[0066] Example 6
[0067] Weigh 1.5g (1mmol) of lanthanum trimethyl acetate into a beaker, add 3ml of acetonitrile and 4ml of N,N-dimethylformamide to completely dissolve the rare earth precursor. Disperse 0.074g (2mmol) of amine fluoride in 2ml of ethanol, mix the two solutions and pour them into a 15ml polytetrafluoroethylene bottle, pressurize and react in a temperature-controlled oven at 150 degrees Celsius for 72 hours, and cool to room temperature for 36 hours to obtain pure colorless block crystals of La. 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, washed three times with acetonitrile, the product yield was 60%, and the crystal structure was determined by single crystal X-ray diffraction analysis, which was consistent with the previous Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The crystal structure of ([N(CH2CH2O)3])4 is consistent.
[0068] Example 7
[0069] Weigh 1.5g (1mmol) of cerium trimethylacetate into a beaker, add 3ml of acetonitrile and 4ml of N,N-dimethylformamide to completely dissolve the rare earth precursor. Disperse 0.074g (2mmol) of amine fluoride in 2ml of ethanol, mix the two solutions and pour them into a 15ml glass bottle, react under pressure in a temperature-controlled oven at 120 degrees Celsius for 72 hours, and cool to room temperature for 36 hours to obtain pure colorless block crystals of Ce. 16(μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, washed three times with acetonitrile, the product yield was 30%, and the crystal structure was determined by single crystal X-ray diffraction analysis, which was consistent with the previous Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The crystal structure of ([N(CH2CH2O)3])4 is consistent.
[0070] Example 8
[0071] Weigh 1.5g (1mmol) of neodymium trimethylacetate into a beaker, add 3ml of acetonitrile and 4ml of N,N-dimethylformamide to completely dissolve the rare earth precursor. Disperse 0.074g (2mmol) of amine fluoride in 2ml of ethanol, mix the two solutions and pour them into a 15ml polytetrafluoroethylene bottle, pressurize and react in a temperature-controlled oven at 150 degrees Celsius for 72 hours, and cool to room temperature for 36 hours to obtain pure purple transparent block crystals of Nd 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, washed three times with acetonitrile, the product yield was 23%, and the crystal structure was determined by single crystal X-ray diffraction analysis, which was consistent with the previous Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The crystal structure of ([N(CH2CH2O)3])4 is consistent.
[0072] Example 9
[0073] Weigh 1.5g (1mmol) of samarium trimethylacetate into a beaker, add 3ml of acetonitrile and 4ml of N,N-dimethylformamide to completely dissolve the rare earth precursor. Disperse 0.074g (2mmol) of amine fluoride in 2ml of ethanol, mix the two solutions and pour them into a 15ml polytetrafluoroethylene bottle, react under pressure in a temperature-controlled oven at 150 degrees Celsius for 72 hours, and cool to room temperature for 24 hours to obtain pure light yellow transparent block crystals of Sm 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, washed three times with acetonitrile, the product yield was 70%, and the crystal structure was determined by single crystal X-ray diffraction analysis, which was consistent with the previous Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO]18 The crystal structure of ([N(CH2CH2O)3])4 is consistent.
[0074] Example 10
[0075] Weigh 1.5g (1mmol) of dysprosium trimethylacetate into a beaker, add 3ml of acetonitrile and 4ml of N,N-dimethylformamide to completely dissolve the rare earth precursor. Disperse 0.074g (2mmol) of amine fluoride in 2ml of ethanol, mix the two solutions and pour them into a 15ml polytetrafluoroethylene bottle, react under pressure in a temperature-controlled oven at 150 degrees Celsius for 72 hours, and cool to room temperature for 36 hours to obtain pure colorless and transparent block crystals of Dy 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, washed three times with acetonitrile, the product yield was 73%, and the crystal structure was determined by single crystal X-ray diffraction analysis, which was consistent with the previous Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The crystal structure of ([N(CH2CH2O)3])4 is consistent.
[0076] Embodiment 11
[0077] Weigh 1.5g (1mmol) of trimethylacetic acid bait into a beaker, add 3ml of acetonitrile and 4ml of N,N-dimethylformamide to completely dissolve the rare earth precursor. Disperse 0.074g (2mmol) of fluorinated amine in 2ml of ethanol, mix the two solutions and pour them into a 15ml polytetrafluoroethylene bottle, react under pressure in a temperature-controlled oven at 150 degrees Celsius for 72 hours, and cool to room temperature for 36 hours to obtain pink transparent block crystals of Er 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, washed three times with acetonitrile, the product yield was 89%, and the crystal structure was determined by single crystal X-ray diffraction analysis, which was consistent with the previous Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The crystal structure of ([N(CH2CH2O)3])4 is consistent.
[0078] Example 12
[0079] Weigh 1.5g (1mmol) of thulium trimethylacetate into a beaker, add 3ml of acetonitrile and 4ml of N,N-dimethylformamide to completely dissolve the rare earth precursor. Disperse 0.074g (2mmol) of amine fluoride in 2ml of ethanol, mix the two solutions and pour them into a 15ml polytetrafluoroethylene bottle, react under pressure in a temperature-controlled oven at 150 degrees Celsius for 72 hours, and cool to room temperature for 36 hours to obtain pure colorless transparent block crystals of Tm 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, washed three times with acetonitrile, the product yield was 59%, and the crystal structure was determined by single crystal X-ray diffraction analysis, which was consistent with the previous Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The crystal structure of ([N(CH2CH2O)3])4 is consistent.
[0080] Embodiment 13
[0081] Weigh 1.5g (1mmol) of ytterbium trimethylacetate into a beaker, add 3ml of acetonitrile and 4ml of N,N-dimethylformamide to completely dissolve the rare earth precursor. Disperse 0.074g (2mmol) of amine fluoride in 2ml of ethanol, mix the two solutions and pour them into a 15ml polytetrafluoroethylene bottle, pressurize and react in a temperature-controlled oven at 150 degrees Celsius for 72 hours, and cool to room temperature for 36 hours to obtain pure colorless and transparent block crystals of Yb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, washed three times with acetonitrile, the product yield was 66%, and the crystal structure was determined by single crystal X-ray diffraction analysis, which was consistent with the previous Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The crystal structure of ([N(CH2CH2O)3])4 is consistent.
[0082] Embodiment 14
[0083] Weigh 0.75g (0.5mmol) of lutetium trimethylacetate into a beaker, add 7ml of anhydrous methanol to completely dissolve the rare earth precursor. Disperse 0.037g (1mmol) of amine fluoride in 2ml of ethanol, mix the two solutions and pour them into a 15ml polytetrafluoroethylene bottle, react under pressure in a temperature-controlled oven at 130 degrees Celsius for 72 hours, and cool to room temperature for 24 hours to obtain pure colorless and transparent block crystals of Lu. 16(μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, washed three times with acetonitrile, the product yield was 54%, and the crystal structure was determined by single crystal X-ray diffraction analysis, which was consistent with the previous Tb 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The crystal structure of ([N(CH2CH2O)3])4 is consistent.
[0084] The invention discloses a method for preparing a high-stability rare earth nano-fluorine cluster for LED lighting. A rare earth metal source and a fluorine source are reacted by a solvent thermal reaction method to obtain a high-stability rare earth nano-fluorine cluster with stable chemical properties. The synthesis method is simple and easy, with high yield, good dispersibility in organic solvents, and good thermal stability, which can reach above 450 degrees Celsius. In addition to the fluorine ions that play a bridging role in the molecular structure, there are also chelating metals by the outer organic ligands, so that the concentration quenching phenomenon of the rare earth luminescent material is eliminated. The bridging of the fluorine ions replaces the fluorescence quenching caused by the high-frequency vibration group "-OH", so that the fluorescence quantum yield is significantly improved to more than 80%.
[0085] The present invention discloses an LED lighting device, which comprises a high-stability rare earth nano-fluorine cluster (RE 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, RE=Tb or Eu) and commercial BAM blue phosphor are mixed in UV curing glue and coated on near-UV chip. White light with various color temperature modes can be achieved by adjusting the proportion of three-color fluorescent materials. Its high brightness, high appearance index, negative temperature quenching and other characteristics meet the lighting needs of outdoor LED lights at night; good thermal stability greatly extends the service life of LEDs and improves safety in practical applications.
Claims
1. A high-stability rare earth nanofluorine cluster for LED lighting, characterized in that: The molecular formula is RE 16 ( µ 4-F)6( µ 3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4, where RE is a rare earth ion, µ 4-F and µ 3-F is the bridging mode of fluoride ion, [N(CH2CH2O)3] 3- is a deprotonated triethanolamine ligand, [(CH3)3CCOO] - is a trimethylacetate ion, and RE is one or more of Y, La, Ce, Nd, Sm, Eu, Tb, Dy, Ho, Er, Tm, Yb or Lu.
2. The high-stability rare earth nano-fluorine cluster for LED lighting according to claim 1, characterized in that: Among them, Eu 16 ( µ 4-F)6( µ 3-F) 12 [(CH3)3CCOO] 18 ([N(CH2CH2O)3])4 and Tb 16 ( µ 4-F)6( µ 3-F) 12 [(CH3)3CCOO] 18 The emission peaks of ([N(CH2CH2O)3])4 are all in the visible light region, the excitation wavelength range is 350~450 nanometers, and the emission peak range is 550~750 nanometers.
3. A method for preparing the high-stability rare earth nano-fluorine clusters for LED lighting as claimed in claim 1, characterized in that: The following steps are involved: S1, reflux reaction of rare earth oxide and trimethylacetic acid solution at a temperature of 140-160 degrees Celsius to obtain a rare earth precursor, and dissolving and dispersing the rare earth precursor and triethanolamine ligand in an organic solvent to obtain a solution A; S2, dispersing a fluorine source in a solvent to obtain a solution B, subjecting solution A and solution B to a solvothermal reaction, and obtaining a colorless block-like high-stability rare earth nanofluorine cluster through programmed cooling; the fluorine source is triethylamine trihydrofluoride, ammonium fluoride, sodium fluoride or tetramethylammonium fluoride tetrahydrate.
4. The method for preparing a high-stability rare earth nano-fluorine cluster for LED lighting according to claim 3, characterized in that: The organic solvent is one of methanol, ethanol, acetonitrile or N,N-dimethylformamide or a mixture of several thereof.
5. The method for preparing a high-stability rare earth nano-fluorine cluster for LED lighting according to claim 3, characterized in that: The solvent thermal reaction temperature is 100~160 degrees Celsius, the reaction time is 24~72 hours, and the programmed cooling rate is 3~5 degrees Celsius per hour.
6. The method for preparing a high-stability rare earth nano-fluorine cluster for LED lighting according to claim 3, characterized in that: The rare earth precursor is trimethylacetic acid rare earth salt.
7. The method for preparing a high-stability rare earth nano-fluorine cluster for LED lighting according to claim 3, characterized in that: The molar ratio of rare earth precursor to fluorine source is 1:(2~3).
8. The method for preparing a high-stability rare earth nano-fluorine cluster for LED lighting according to claim 3, characterized in that: The solvent in step S2 is anhydrous ethanol.
9. Use of the high-stability rare earth nano-fluorine cluster for LED lighting according to claim 1 in LED lighting devices.